Flash non-woven fabric with low crease recovery angle

By using flower-like cerium oxide modified products and optimized drying process in flash nonwovens, the crease recovery angle and dryness are improved, and the lack of crease recovery angle performance of existing flash nonwovens is solved. The problem has expanded its application depth.

CN119061581APending Publication Date: 2024-12-03JIANGSU QINGYUN NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310653758.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The performance indicators of existing flash non-woven fabrics have not been effectively improved after being used for a period of time, which limits its application depth.

Method used

The flower-like cerium oxide modification is used as raw material, and the total crease recovery angle and drying degree of flash nonwoven fabrics are improved through specific spinning and drying processes, combined with the design of the drying device to enhance the strength of the fibers and Wear resistance.

Benefits of technology

The crease recovery angle performance of flash non-woven fabrics is significantly improved, reaching 60° to 80°, and its dryness is improved to 95% to 99%, thus expanding its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061581A_ABST
    Figure CN119061581A_ABST
Patent Text Reader

Abstract

The invention relates to a flash non-woven fabric with a low crease recovery angle, which is characterized in that the total crease recovery angle of the flash non-woven fabric is 60-80 degrees; the total crease recovery angle is measured according to a national standard GB / T 3819-1997 textile fabric crease recovery angle measurement method and a 9.1 horizontal method; the elongation at break of the flash non-woven fabric is 10%-20%; the dryness D of the flash non-woven fabric is 95%-99%. The flash non-woven fabric provided by the invention has a relatively low crease recovery angle and relatively low elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flash steaming production, and in particular relates to a flash steamed nonwoven fabric with a low crease recovery angle. Background Art

[0002] Chinese patent publication number CN112609334A relates to a flash nonwoven fabric and a method for preparing the same. This application aims to solve the problem in the prior art that solid adsorbents are difficult to flow, so different equipment needs to be switched to implement adsorption and desorption, and provides a flash nonwoven fabric and a method for preparing the same, including the steps of preparing spinning solution, spinning and tail gas treatment, wherein the tail gas treatment includes conveying the solvent vapor generated by solvent evaporation to the lower section of the adsorption tower through a fan, and the liquid adsorbent used to adsorb the solvent vapor is sprayed from the upper section of the adsorption tower and mixed with the solvent vapor in the adsorption tower. After the adsorption is completed, the liquid is discharged from the bottom of the adsorption tower and the gas is discharged from the top of the adsorption tower. This application uses countercurrent convection between the liquid adsorbent and the tail gas to be absorbed to achieve adsorption of the solvent vapor in the tail gas, which makes the entire process operation simpler and reduces production costs compared to the method of using solid adsorbents in the prior art.

[0003] Chinese patent publication number CN115976737A relates to a polyethylene flash nonwoven fabric, characterized in that its wet tensile strength is 1600-2400N / m, wet tensile strength retention rate is 0.55-0.70, opacity is 0.85-0.95, and gram weight is 35-45g / m2; the soaking process conditions of the sample are: first, the soaking water temperature is 40°C, and the soaking time is 8 hours; secondly, the temperature is raised to 60°C, and the soaking time is 8 hours. This application has good wet tensile strength and wet tensile strength retention rate, and is widely used.

[0004] Chinese patent publication number CN114687068A relates to an improved flash-steamed nonwoven fabric. The present invention aims to solve the problem that the brightness of flash-steamed nonwoven fabrics in the prior art decreases after being used for a period of time, and provides an improved flash-steamed nonwoven fabric. The loss rate of D65 fluorescence brightness of the improved flash-steamed nonwoven fabric is ▲F of 0.20-0.30; wherein ▲F=1F2 / F1; F1 is the D65 fluorescence brightness of the nonwoven fabric without aging treatment; F2 is the D65 fluorescence brightness of the nonwoven fabric after aging treatment; the process conditions of aging treatment are: the irradiance in the wavelength range of 300-400 nanometers is 60±2w / m2, the black mark temperature is 65±2℃, the air temperature of the test chamber is 38±3℃, the relative humidity is 50±10%, and the drying time is 1440 hours. The flash-steamed nonwoven fabric of this application can maintain a high brightness after being used for a period of time.

[0005] Chinese patent publication number CN115874350A relates to a mildew-proof polyethylene fabric and its production method and application, wherein the raw material comprises polyethylene, the ratio of cold shrinkage strength to heat shrinkage strength is 2:1 to 6:1; the cold shrinkage strength is 2.5 to 5.5 N / mm2; the mildew-proof grade of the mildew-proof polyethylene fabric is less than grade 3. This application significantly improves the mildew-proof and antibacterial function of the product by adding a nano titanium nitride modifier doped with copper and zinc; at the same time, it also improves the mechanical properties and expands its application range.

[0006] Chinese patent publication number CN114687069A relates to a multifunctional polymer nonwoven fabric and fabric thereof, characterized in that the attenuation rate of its elongation at break ▲E is 0.20-0.50; ▲E=1E2 / E1; E1 is the elongation at break of the multifunctional polymer nonwoven fabric not subjected to aging test; E2 is the elongation at break of the multifunctional polymer nonwoven fabric subjected to aging test; the value of E2 is less than 0.5. The process of this application is simple and widely used.

[0007] Chinese patent publication number CN114622341A relates to a polyethylene nonwoven fabric and its application, characterized in that the raw material of the polyethylene nonwoven fabric is mainly polyethylene, the first average bending stiffness DG of the polyethylene nonwoven fabric is 28-240 mN·cm, and the ratio of DG / XG is 1.03-3.0, and the larger average bending stiffness test value in the same sample is defined as the first average bending stiffness DG, and the smaller test value is defined as the second average bending stiffness XG. The polyethylene nonwoven fabric of this application has certain bending stiffness and good air permeability.

[0008] However, the existing patent technology does not involve the performance index of the crease recovery angle of flash-steamed nonwoven fabrics. However, there is an objective demand in the market for how to modify the crease recovery angle performance of flash-steamed nonwoven fabrics. Therefore, how to improve the crease recovery angle of flash-steamed nonwoven fabrics to expand the application depth of flash-steamed nonwoven fabrics has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0009] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a flash-steamed nonwoven fabric with a low crease recovery angle.

[0010] The objective of the present invention is achieved through the following technical solutions:

[0011] A flash-steamed nonwoven fabric with a low crease recovery angle, characterized in that the total crease recovery angle of the flash-steamed nonwoven fabric is 60° to 80°;

[0012] The total crease recovery angle is tested in accordance with the national standard GB / T 3819-1997 Determination of crease recovery of textile fabrics, recovery angle method, 9.1 horizontal method;

[0013] The elongation at break of flash nonwoven fabric is 10% to 20%;

[0014] The dryness D of flash nonwoven fabric is 95% to 99%;

[0015] D = (Q1 / Q0) * 100%;

[0016] Q1 is the mass of the flash nonwoven fabric after drying;

[0017] Q0 is the mass of the initial flash-steamed nonwoven fabric;

[0018] That is, before being dried by the drying device, the mass of the flash-steamed non-woven fabric sample is Q0, and after being dried by the drying device, the mass of the flash-steamed non-woven fabric sample is Q1.

[0019] The raw materials of flash nonwoven fabric are polyethylene and flower-shaped cerium oxide modified product.

[0020] The total crease recovery angle of the flash-steamed nonwoven fabric is 60° to 65°.

[0021] The total crease recovery angle of the flash nonwoven fabric is 65° to 70°.

[0022] The total crease recovery angle of the flash-steamed nonwoven fabric is 70° to 75°.

[0023] The total crease recovery angle of flash-steamed nonwoven fabric is 75° to 80°.

[0024] The breaking elongation of flash-steamed nonwoven fabric is 10% to 13%.

[0025] The elongation at break of flash-steamed nonwoven fabric is 13% to 16%.

[0026] The breaking elongation of flash-steamed nonwoven fabric is 16% to 20%.

[0027] The dryness D of flash-steamed nonwoven fabric is 95% to 97%.

[0028] The dryness D of flash-steamed nonwoven fabric is 97% to 99%.

[0029] A method for manufacturing a flash-steamed nonwoven fabric with a low crease recovery angle, comprising the following specific technical steps:

[0030] 1) Production of spinning solution:

[0031] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0032] The raw materials of the flash nonwoven fabric are polyethylene and flower-shaped cerium oxide modification; wherein the mass fraction of the flower-shaped cerium oxide modification in the raw materials of the flash nonwoven fabric is 2.5% to 3.5%.

[0033] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0034] The mass fraction of the raw material in the spinning solution is 6% to 16%.

[0035] The method for producing the flower-shaped cerium oxide modified product comprises the following technical steps:

[0036] (1) dispersing flower-shaped cerium oxide and barium sulfate in dilute sulfuric acid, stirring for 3 to 8 hours until no precipitation is generated, and then filtering and vacuum drying to obtain a flower-shaped cerium oxide modified product;

[0037] The mass ratio of barium sulfate to flower-like cerium oxide is 1:15 to 1:20;

[0038] The geometric appearance of each particle of flower-like cerium oxide is close to a sphere, with an average diameter of 100 nanometers to 100 micrometers. Many thin flakes with a thickness of 2 to 500 nm grow on each particle. The orientation of each thin flake is perpendicular to the surface of the sphere and radiates from the inside to the outside. Each thin flake is either a straight plane or a curved surface, and the thin flakes are connected to each other.

[0039] 2) Manufacturing of flash nonwoven fabrics

[0040] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0041] The drying device comprises a rotating roller and a polygonal air outlet component; the rotating rollers are sequentially staggered up and down and the non-woven fabrics are sequentially arranged on the outside of each rotating roller, and polygonal air outlet components are respectively arranged on both sides between two adjacent rotating rollers, and the polygonal air outlet component has an air outlet surface facing the side of the non-woven fabric and having a plurality of air outlets, and both sides of the non-woven fabric correspond to the air outlet surfaces of different polygonal air outlet components, and a heating pipe is arranged between the air outlet surface and the non-woven fabric;

[0042] The number of rotating rollers is more than 2;

[0043] The number of air outlet components is more than 2 and is matched with the number of rotating rollers;

[0044] The number of heating pipes is more than 2 and is matched with the number of air outlet components;

[0045] The heating tube is located between the air outlet component and the non-woven fabric, and the distance between the heating tube and the non-woven fabric is 3 to 15 cm;

[0046] The polygonal air outlet component is in the shape of a triangle, each polygonal air outlet component has at least one air outlet surface, and each air outlet surface is formed on different sides of the polygonal air outlet component;

[0047] The polygonal air outlet component is provided with wind by an external fan;

[0048] Two adjacent polygonal air outlet components are staggered in vertical arrangement and the corresponding air outlet surfaces of the two adjacent polygonal air outlet components are arranged parallel to each other;

[0049] The distances between the corresponding air outlet surfaces of two adjacent polygonal air outlet components are the same;

[0050] The non-woven fabric is arranged at the middle position of the air outlet surfaces corresponding to two adjacent polygonal air outlet components;

[0051] The rotating rollers are divided into upper rotating rollers and lower rotating rollers, and the upper rotating rollers and the lower rotating rollers are arranged one by one in an alternating manner. The upper rotating rollers are located on the same horizontal plane, and the lower rotating rollers are lower than the upper rotating rollers and the lower rotating rollers are located on the same horizontal plane.

[0052] Compared with the prior art, the present invention has the following positive effects:

[0053] 1. The present invention provides a method for modifying flower-shaped cerium oxide, and finds that adding a certain amount of the above-mentioned flower-shaped cerium oxide modified substance to the raw material can significantly improve the crease recovery angle of the final flash-steamed non-woven fabric. At the same time, its annular structure can play a buffering role when the flash-steamed non-woven fabric is subjected to force, thereby improving its strength performance.

[0054] 2. The present invention provides a drying device to improve the dryness of flash-steamed nonwoven fabrics. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 It is a structural schematic diagram of the drying device of the present invention;

[0056] In the figure: a drying box 1, a first upper rotating roller 2, a second lower rotating roller 21, a third upper rotating roller 22, a fourth lower rotating roller 23, a fifth upper rotating roller 24, a first polygonal air outlet component 3, a second polygonal air outlet component 31, a third polygonal air outlet component 32, a fourth polygonal air outlet component 33, a fifth polygonal air outlet component 34, a first heating tube 4, a second heating tube 41, a third heating tube 42, a fourth heat conducting tube 43, a fifth heating tube 44, a sixth heating tube 45, a seventh heating tube 46, an eighth heating tube 47, a non-woven fabric 5, and an exhaust port 6. DETAILED DESCRIPTION

[0057] The present invention will be further described in detail below in conjunction with specific implementation methods and accompanying drawings.

[0058] Example 1

[0059] This embodiment provides a flash-steamed nonwoven fabric with a low crease recovery angle and a processing method thereof. Figure 1 As shown, the specific technical steps involved are:

[0060] 1) Production of spinning solution:

[0061] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0062] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modification; wherein the mass fraction of the flower-shaped cerium oxide modification in the raw materials of the flash-steamed non-woven fabric is 2.5%.

[0063] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0064] The mass fraction of the raw material in the spinning solution is 7%.

[0065] A method for preparing a flower-shaped cerium oxide modified product, comprising the following technical steps:

[0066] (1) dispersing flower-shaped cerium oxide and barium sulfate in dilute sulfuric acid, stirring for 3 to 8 hours until no precipitation is generated, and then filtering and vacuum drying to obtain a flower-shaped cerium oxide modified product;

[0067] The mass ratio of barium sulfate to flower-structured cerium oxide is 1:15;

[0068] Each particle of the flower-shaped cerium oxide has a geometric appearance close to a sphere, with an average diameter of 100 nanometers to 100 micrometers. Many thin slices with a thickness of 2 to 500 nanometers grow on each particle. The orientation of each thin slice is perpendicular to the surface of the sphere and radiates from the inside to the outside. Each thin slice is either a straight plane or a curved surface, and the thin slices are connected to each other. The flower-shaped cerium oxide in the present invention is prepared by the preparation method recorded in the invention patent with application number "200510087129.1".

[0069] 2) Manufacturing of flash nonwoven fabrics

[0070] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0071] The drying device comprises a drying box 1 and a plurality of rotating rollers 2, 21, 22, 23, 24 and a plurality of polygonal air outlet components 3, 31, 32, 33, 34 arranged in the drying box 1; the rotating rollers 2, 21, 22, 23, 24 are sequentially staggered up and down and the non-woven fabric 5 is sequentially pressed on the outside of each rotating roller 2, 21, 22, 23, 24, the polygonal air outlet components 3, 31, 32, 33, 34 are arranged on both sides between two adjacent rotating rollers 2, 21, 22, 23, 24, the polygonal air outlet components 3, 31, 32, 33, 34 have an air outlet surface facing the side of the non-woven fabric 5 and having a plurality of air outlets, both sides of the non-woven fabric 5 correspond to the air outlet surfaces of different polygonal air outlet components 3, 31, 32, 33, 34, and heating tubes 4, 41, 42, 43, 44, 45, 46, 47 are arranged between the air outlet surface and the non-woven fabric 5;

[0072] Specifically, there are five rotating rollers parallel to each other, namely, the first upper rotating roller 2, the second lower rotating roller 21, the third upper rotating roller 22, the fourth lower rotating roller 23 and the fifth upper rotating roller 24. The non-woven fabric 5 that has not been subjected to heat pressing treatment extends from one side of the drying box 1 into the drying box 1, and is transported by the first upper rotating roller 2, the second lower rotating roller 21, the third upper rotating roller 22, the fourth lower rotating roller 23 and the fifth upper rotating roller 24 in sequence. A polygonal air outlet component for blowing air is arranged above or below each rotating roller, and a heating pipe is arranged between the polygonal air outlet component and the non-woven fabric 5, which is used to heat the air and blow it to the surface of the non-woven fabric 5. An air outlet 6 is arranged at the lower right end of the drying device 1.

[0073] The heating tube is located between the air outlet component and the non-woven fabric, and the distance between the heating tube and the non-woven fabric is 3 to 15 cm;

[0074] The polygonal air outlet component is in the shape of a triangle, each polygonal air outlet component has at least one air outlet surface, and each air outlet surface is formed on different sides of the polygonal air outlet component;

[0075] The polygonal air outlet component is provided with wind by an external fan;

[0076] Two adjacent polygonal air outlet components are staggered in vertical arrangement and the corresponding air outlet surfaces of the two adjacent polygonal air outlet components are arranged parallel to each other;

[0077] The distances between the corresponding air outlet surfaces of two adjacent polygonal air outlet components are the same;

[0078] The non-woven fabric is arranged at the middle position of the air outlet surfaces corresponding to two adjacent polygonal air outlet components;

[0079] The rotating rollers are divided into upper rotating rollers and lower rotating rollers, and the upper rotating rollers and the lower rotating rollers are arranged one by one in an alternating manner. The upper rotating rollers are located on the same horizontal plane, and the lower rotating rollers are lower than the upper rotating rollers and the lower rotating rollers are located on the same horizontal plane.

[0080] The performance test results of the flash-steamed nonwoven fabric prepared in this embodiment are shown in Table 1.

[0081] Example 2

[0082] This embodiment provides a flash-steamed nonwoven fabric with a low crease recovery angle and a processing method thereof. Figure 1 As shown, the specific technical steps involved are:

[0083] 1) Production of spinning solution:

[0084] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0085] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modified products; wherein the mass fraction of the flower-shaped cerium oxide modified products in the raw materials of the flash-steamed non-woven fabric is 3%.

[0086] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0087] The mass fraction of the raw material in the spinning solution is 10%.

[0088] A method for preparing a flower-shaped cerium oxide modified product, comprising the following technical steps:

[0089] (1) dispersing flower-shaped cerium oxide and barium sulfate in dilute sulfuric acid, stirring for 3 to 8 hours until no precipitation is generated, and then filtering and vacuum drying to obtain a flower-shaped cerium oxide modified product;

[0090] The mass ratio of barium sulfate to flower-structured cerium oxide is 1:19;

[0091] The geometric appearance of each particle of flower-like cerium oxide is close to a sphere, with an average diameter of 100 nanometers to 100 micrometers. Many thin flakes with a thickness of 2 to 500 nm grow on each particle. The orientation of each thin flake is perpendicular to the surface of the sphere and radiates from the inside to the outside. Each thin flake is either a straight plane or a curved surface, and the thin flakes are connected to each other.

[0092] 2) Manufacturing of flash nonwoven fabrics

[0093] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0094] The drying device comprises a drying box 1 and a plurality of rotating rollers 2, 21, 22, 23, 24 and a plurality of polygonal air outlet components 3, 31, 32, 33, 34 arranged in the drying box 1; the rotating rollers 2, 21, 22, 23, 24 are sequentially staggered up and down and the non-woven fabric 5 is sequentially pressed on the outside of each rotating roller 2, 21, 22, 23, 24, the polygonal air outlet components 3, 31, 32, 33, 34 are arranged on both sides between two adjacent rotating rollers 2, 21, 22, 23, 24, the polygonal air outlet components 3, 31, 32, 33, 34 have an air outlet surface facing the side of the non-woven fabric 5 and having a plurality of air outlets, both sides of the non-woven fabric 5 correspond to the air outlet surfaces of different polygonal air outlet components 3, 31, 32, 33, 34, and heating tubes 4, 41, 42, 43, 44, 45, 46, 47 are arranged between the air outlet surface and the non-woven fabric 5;

[0095] Specifically, there are five rotating rollers parallel to each other, namely, the first upper rotating roller 2, the second lower rotating roller 21, the third upper rotating roller 22, the fourth lower rotating roller 23 and the fifth upper rotating roller 24. The non-woven fabric 5 that has not been subjected to heat pressing treatment extends from one side of the drying box 1 into the drying box 1, and is transported by the first upper rotating roller 2, the second lower rotating roller 21, the third upper rotating roller 22, the fourth lower rotating roller 23 and the fifth upper rotating roller 24 in sequence. A polygonal air outlet component for blowing air is arranged above or below each rotating roller, and a heating pipe is arranged between the polygonal air outlet component and the non-woven fabric 5, which is used to heat the air and blow it to the surface of the non-woven fabric 5. An air outlet 6 is arranged at the lower right end of the drying device 1.

[0096] The heating tube is located between the air outlet component and the non-woven fabric, and the distance between the heating tube and the non-woven fabric is 3 to 15 cm;

[0097] The polygonal air outlet component is in the shape of a triangle, each polygonal air outlet component has at least one air outlet surface, and each air outlet surface is formed on different sides of the polygonal air outlet component;

[0098] The polygonal air outlet component is provided with wind by an external fan;

[0099] Two adjacent polygonal air outlet components are staggered in vertical arrangement and the corresponding air outlet surfaces of the two adjacent polygonal air outlet components are arranged parallel to each other;

[0100] The distances between the corresponding air outlet surfaces of two adjacent polygonal air outlet components are the same;

[0101] The non-woven fabric is arranged at the middle position of the air outlet surfaces corresponding to two adjacent polygonal air outlet components;

[0102] The rotating rollers are divided into upper rotating rollers and lower rotating rollers, and the upper rotating rollers and the lower rotating rollers are arranged one by one in an alternating manner. The upper rotating rollers are located on the same horizontal plane, and the lower rotating rollers are lower than the upper rotating rollers and the lower rotating rollers are located on the same horizontal plane.

[0103] The performance test results of the flash-steamed nonwoven fabric prepared in this embodiment are shown in Table 1.

[0104] Example 3

[0105] This embodiment provides a flash-steamed nonwoven fabric with a low crease recovery angle and a processing method thereof. Figure 1 As shown, the specific technical steps involved are:

[0106] 1) Production of spinning solution:

[0107] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0108] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modification; wherein the mass fraction of the flower-shaped cerium oxide modification in the raw materials of the flash-steamed non-woven fabric is 3.5%.

[0109] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0110] The mass fraction of the raw material in the spinning solution is 13%.

[0111] A method for preparing a flower-shaped cerium oxide modified product, comprising the following technical steps:

[0112] (1) dispersing flower-shaped cerium oxide and barium sulfate in dilute sulfuric acid, stirring for 3 to 8 hours until no precipitation is generated, and then filtering and vacuum drying to obtain a flower-shaped cerium oxide modified product;

[0113] The mass ratio of barium sulfate to flower-structured cerium oxide is 1:20;

[0114] The geometric appearance of each particle of flower-like cerium oxide is close to a sphere, with an average diameter of 100 nanometers to 100 micrometers. Many thin flakes with a thickness of 2 to 500 nm grow on each particle. The orientation of each thin flake is perpendicular to the surface of the sphere and radiates from the inside to the outside. Each thin flake is either a straight plane or a curved surface, and the thin flakes are connected to each other.

[0115] 2) Manufacturing of flash nonwoven fabrics

[0116] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0117] The drying device comprises a drying box 1 and a plurality of rotating rollers 2, 21, 22, 23, 24 and a plurality of polygonal air outlet components 3, 31, 32, 33, 34 arranged in the drying box 1; the rotating rollers 2, 21, 22, 23, 24 are sequentially staggered up and down and the non-woven fabric 5 is sequentially pressed on the outside of each rotating roller 2, 21, 22, 23, 24, the polygonal air outlet components 3, 31, 32, 33, 34 are arranged on both sides between two adjacent rotating rollers 2, 21, 22, 23, 24, the polygonal air outlet components 3, 31, 32, 33, 34 have an air outlet surface facing the side of the non-woven fabric 5 and having a plurality of air outlets, both sides of the non-woven fabric 5 correspond to the air outlet surfaces of different polygonal air outlet components 3, 31, 32, 33, 34, and heating tubes 4, 41, 42, 43, 44, 45, 46, 47 are arranged between the air outlet surface and the non-woven fabric 5;

[0118] Specifically, there are five rotating rollers parallel to each other, namely, the first upper rotating roller 2, the second lower rotating roller 21, the third upper rotating roller 22, the fourth lower rotating roller 23 and the fifth upper rotating roller 24. The non-woven fabric 5 that has not been subjected to heat pressing treatment extends from one side of the drying box 1 into the drying box 1, and is transported by the first upper rotating roller 2, the second lower rotating roller 21, the third upper rotating roller 22, the fourth lower rotating roller 23 and the fifth upper rotating roller 24 in sequence. A polygonal air outlet component for blowing air is arranged above or below each rotating roller, and a heating pipe is arranged between the polygonal air outlet component and the non-woven fabric 5, which is used to heat the air and blow it to the surface of the non-woven fabric 5. An air outlet 6 is arranged at the lower right end of the drying device 1.

[0119] The heating tube is located between the air outlet component and the non-woven fabric, and the distance between the heating tube and the non-woven fabric is 3 to 15 cm;

[0120] The polygonal air outlet component is in the shape of a triangle, each polygonal air outlet component has at least one air outlet surface, and each air outlet surface is formed on different sides of the polygonal air outlet component;

[0121] The polygonal air outlet component is provided with wind by an external fan;

[0122] Two adjacent polygonal air outlet components are staggered in vertical arrangement and the corresponding air outlet surfaces of the two adjacent polygonal air outlet components are arranged parallel to each other;

[0123] The distances between the corresponding air outlet surfaces of two adjacent polygonal air outlet components are the same;

[0124] The non-woven fabric is arranged at the middle position of the air outlet surfaces corresponding to two adjacent polygonal air outlet components;

[0125] The rotating rollers are divided into upper rotating rollers and lower rotating rollers, and the upper rotating rollers and the lower rotating rollers are arranged one by one in an alternating manner. The upper rotating rollers are located on the same horizontal plane, and the lower rotating rollers are lower than the upper rotating rollers and the lower rotating rollers are located on the same horizontal plane.

[0126] The performance test results of the flash-steamed nonwoven fabric prepared in this embodiment are shown in Table 1.

[0127] Comparative Example 1

[0128] This comparative example provides a flash-steamed nonwoven fabric and a processing method thereof, combined with Figure 1 As shown, the specific technical steps involved are:

[0129] 1) Production of spinning solution:

[0130] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0131] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modified products; wherein the mass fraction of the flower-shaped cerium oxide modified products in the raw materials of the flash-steamed non-woven fabric is 1%.

[0132] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0133] The mass fraction of the raw material in the spinning solution is 10%.

[0134] A method for preparing a flower-shaped cerium oxide modified product is the same as that in Example 2.

[0135] 2) Manufacturing of flash nonwoven fabrics

[0136] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0137] The structure of the drying device is the same as that of Example 2.

[0138] The performance test results of the flash-steamed nonwoven fabric prepared in this comparative example are shown in Table 1.

[0139] Comparative Example 2

[0140] This comparative example provides a flash-steamed nonwoven fabric and a processing method thereof, combined with Figure 1 As shown, the specific technical steps involved are:

[0141] 1) Production of spinning solution:

[0142] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0143] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modified products; wherein the mass fraction of the flower-shaped cerium oxide modified products in the raw materials of the flash-steamed non-woven fabric is 2%.

[0144] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0145] The mass fraction of the raw material in the spinning solution is 10%.

[0146] A method for preparing a flower-shaped cerium oxide modified product is the same as that in Example 2.

[0147] 2) Manufacturing of flash nonwoven fabrics

[0148] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0149] The structure of the drying device is the same as that of Example 2.

[0150] The performance test results of the flash-steamed nonwoven fabric prepared in this comparative example are shown in Table 1.

[0151] Comparative Example 3

[0152] This comparative example provides a flash-steamed nonwoven fabric and a processing method thereof, combined with Figure 1As shown, the specific technical steps involved are:

[0153] 1) Production of spinning solution:

[0154] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0155] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modification; wherein the mass fraction of the flower-shaped cerium oxide modification in the raw materials of the flash-steamed non-woven fabric is 4.5%.

[0156] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0157] The mass fraction of the raw material in the spinning solution is 10%.

[0158] A method for preparing a flower-shaped cerium oxide modified product is the same as that in Example 2.

[0159] 2) Manufacturing of flash nonwoven fabrics

[0160] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0161] The structure of the drying device is the same as that of Example 2.

[0162] The performance test results of the flash-steamed nonwoven fabric prepared in this comparative example are shown in Table 1.

[0163] Comparative Example 4

[0164] This comparative example provides a flash-steamed nonwoven fabric and a processing method thereof, combined with Figure 1 As shown, the specific technical steps involved are:

[0165] 1) Production of spinning solution:

[0166] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0167] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modified products; wherein the mass fraction of the flower-shaped cerium oxide modified products in the raw materials of the flash-steamed non-woven fabric is 6%.

[0168] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0169] The mass fraction of the raw material in the spinning solution is 10%.

[0170] A method for preparing a flower-shaped cerium oxide modified product is the same as that in Example 2.

[0171] 2) Manufacturing of flash nonwoven fabrics

[0172] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0173] The structure of the drying device is the same as that of Example 2.

[0174] The performance test results of the flash-steamed nonwoven fabric prepared in this comparative example are shown in Table 1.

[0175] Comparative Example 5

[0176] This comparative example provides a flash-steamed nonwoven fabric and a processing method thereof, combined with Figure 1 As shown, the specific technical steps involved are:

[0177] 1) Production of spinning solution:

[0178] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0179] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide; wherein the mass fraction of the flower-shaped cerium oxide modified substance in the raw materials of the flash-steamed non-woven fabric is 3%.

[0180] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0181] The mass fraction of the raw material in the spinning solution is 10%.

[0182] The geometric appearance of each particle of flower-like cerium oxide is close to a sphere, with an average diameter of 100 nanometers to 100 micrometers. Many thin flakes with a thickness of 2 to 500 nm grow on each particle. The orientation of each thin flake is perpendicular to the surface of the sphere and radiates from the inside to the outside. Each thin flake is either a straight plane or a curved surface, and the thin flakes are connected to each other.

[0183] 2) Manufacturing of flash nonwoven fabrics

[0184] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0185] The structure of the drying device is the same as that of Example 2.

[0186] The performance test results of the flash-steamed nonwoven fabric prepared in this comparative example are shown in Table 1.

[0187] Comparative Example 6

[0188] This comparative example provides a flash-steamed nonwoven fabric and a processing method thereof, combined with Figure 1 As shown, the specific technical steps involved are:

[0189] 1) Production of spinning solution:

[0190] Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution;

[0191] The raw materials of the flash-steamed non-woven fabric are polyethylene and flower-shaped cerium oxide modified products; wherein the mass fraction of the flower-shaped cerium oxide modified products in the raw materials of the flash-steamed non-woven fabric is 3%.

[0192] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons, alcohols, fluorocarbons and the like. Preferably, it is a mixture of dichloromethane, ethyl chloride, 1,2-dichloro-1,1-difluoroethane and 1,1,1,2-tetrafluoro-2-chloroethane, and the mass ratio of the four is 4:4:1:1.

[0193] The mass fraction of the raw material in the spinning solution is 10%.

[0194] A method for preparing a flower-shaped cerium oxide modified product is the same as that in Example 2.

[0195] 2) Manufacturing of flash nonwoven fabrics

[0196] The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

[0197] The structure of the drying device is basically the same as that of the embodiment 2, except that the drying device in this embodiment is not provided with a heating tube.

[0198] The performance test results of the flash-steamed nonwoven fabric prepared in this comparative example are shown in Table 1.

[0199] Table 1 Test results of this application

[0200]

[0201]

[0202] Result analysis: By comparing the above data, it can be seen that the flower-shaped cerium oxide modified substance provided by the present invention can significantly improve the crease recovery angle of the final flash-steamed non-woven fabric, thus achieving the intended purpose of the present invention.

[0203] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

[0204] Although the present invention uses more terms such as drying box 1, first upper rotating roller 2, second lower rotating roller 21, third upper rotating roller 22, fourth lower rotating roller 23, fifth upper rotating roller 24, first polygonal air outlet component 3, second polygonal air outlet component 31, third polygonal air outlet component 32, fourth polygonal air outlet component 33, fifth polygonal air outlet component 34, first heating tube 4, second heating tube 41, third heating tube 42, fourth heat conducting tube 43, fifth heating tube 44, sixth heating tube 45, seventh heating tube 46, eighth heating tube 47, non-woven fabric 5, exhaust port 6, etc., the possibility of using other terms is not excluded. The use of these terms is only for the purpose of more conveniently describing and explaining the essence of the present invention; interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A flash nonwoven fabric with low crease recovery angle, It is characterized in that The total crease recovery angle of flash nonwoven fabric is 60° to 80°; The total crease recovery angle is tested according to the horizontal method in Section 9.1 of GB / T 3819-1997 “Determination of Crease Recovery of Textile Fabrics - Recovery Angle Method”; The elongation at break of flash nonwoven fabric is 10% to 20%; The dryness D of flash nonwoven fabric is 95% to 99%; D = (Q1 / Q0) * 100%; Q1 is the mass of the flash nonwoven fabric after drying; Q0 is the mass of the initial flash-steamed nonwoven fabric; The raw materials of flash nonwoven fabric are polyethylene and flower-shaped cerium oxide modified product.

2. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The total crease recovery angle of the flash-steamed nonwoven fabric is 60° to 65°.

3. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The total crease recovery angle of the flash nonwoven fabric is 65° to 70°.

4. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The total crease recovery angle of the flash-steamed nonwoven fabric is 70° to 75°.

5. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The total crease recovery angle of flash-steamed nonwoven fabric is 75° to 80°.

6. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The breaking elongation of flash-steamed nonwoven fabric is 10% to 13%.

7. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The elongation at break of flash-steamed nonwoven fabric is 13% to 16%.

8. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The dryness D of flash-steamed nonwoven fabric is 95% to 97%.

9. A flash-steamed nonwoven fabric with a low crease recovery angle as claimed in claim 1, It is characterized in that The dryness D of flash-steamed nonwoven fabric is 97% to 99%.

10. The method for manufacturing a flash-steamed nonwoven fabric with a low crease recovery angle according to claim 1, comprising the following specific technical steps: 1) Production of spinning solution: Dissolving the raw material of the flash nonwoven fabric in a spinning solvent to form a spinning solution; 2) Manufacturing of flash nonwoven fabrics The spinning solution prepared in step 1) is flash-spun to obtain flash fibers at a spinning temperature of 190° C. to 230° C. The flash fibers are then laid and hot-pressed, and then dried by a drying device, and then wound to obtain a flash nonwoven fabric.

Citation Information

Patent Citations

  • Preparation method of flowerlike cerium oxide nano-material

    CN105585043A

  • Dynamic evaluation method of wrinkle recovery performance of fabrics

    CN106198937A

  • Testing method of yarn crease recovery angle

    CN113029934A

  • Preparation method of flash non-woven fabric with high optical tolerance

    CN114775271A

  • Method for evaluating folds on textile fabrics