High-fireproof and high-covering advertising cloth and preparation method thereof
By combining halogen-free flame retardant and expandable graphite in the advertising cloth to form a dense carbonized layer, the problems of toxic smoke and poor dispersion in the prior art are solved, and advertising cloth with high fire resistance, high cover and good mechanical properties are achieved.
Patent Information
- Application Number
- CN202411004770.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-12-03
AI Technical Summary
Existing water-based flame retardant coatings produce toxic fumes and hydrogen halide gases during combustion, and the halogen-free flame retardant has poor dispersion and low mechanical properties, making it difficult to meet the needs of high fire resistance, high cover and good mechanical properties.
Halogen-free flame retardant combined with expandable graphite is used to prepare high fire-resistant and high-cover advertising cloth through a specific process. The composite flame retardant Trimer/APP and expandable graphite synergistically form a dense carbonized layer to enhance the strength of the coating. degree and flame retardant properties.
It achieves excellent flame retardancy, shielding and mechanical properties, avoids the production of toxic gases, improves the anti-gas erosion ability and tensile strength, and meets the environmentally friendly and efficient advertising requirements.
Smart Images

Figure CN119061705A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of coatings and relates to a highly fireproof and highly concealing advertising cloth and a preparation method thereof. Background Art
[0002] As a kind of polymer material, most of the fabrics are easy to burn, so good flame retardant properties are required in the application products; the fabric of the advertising cloth not only needs to be flame retardant, but also needs good shielding and uniform light transmittance to better adapt to the external environment and achieve the advertising effect.
[0003] At present, in the textile field, the most widely used and effective water-based flame retardant coating adhesive is the bromine antimony series, mainly antimony trioxide and decabromodiphenyl ether. The bromine antimony series flame retardant system has excellent gas phase flame retardant performance and high cost performance, so it is very popular. However, when a fire occurs, such materials made with halogen-containing flame retardants will produce a large amount of smoke and toxic and corrosive hydrogen halide gas when heated, causing secondary hazards. In addition, antimony is considered to be a heavy metal, toxic, and a homologue of arsenic. The crude product generally contains arsenic and other heavy metals. Arsenic trioxide is arsenic and cannot be used as a green filler or green flame retardant. Its use is increasingly restricted.
[0004] In contrast, halogen-free flame retardants have better environmental performance. They do not produce toxic halogen compounds during combustion. They are in line with the national development direction of clean production and energy conservation and emission reduction. Halogen-free flame retardants have the characteristics of expanding to produce porous foam layers. Their expansion combustion system has received great attention in the field of flame retardants in recent years. It uses acid sources, carbon sources and gas sources to produce synergistic effects with flame retardants. When heated, the entire coating expands and carbonizes to form a dense, stable, and low-thermal conductivity carbonized layer, which plays a role in heat insulation, heat absorption, and protection of the substrate. It is another classic synergistic combination in the field of flame retardancy.
[0005] At present, water-based latex bonds halogen-free intumescent flame retardant components together and uniformly coats them on the surface of the substrate to form a film structure, which can have a certain stability, but has the following disadvantages: it makes the free volume of the system smaller, the expansion ratio is not large when heated, and the uniformity of the bubbles inside the carbonization layer is slightly poor, which affects the flame retardant effect. In addition, the halogen-free flame retardant has poor dispersion in the material, which leads to low mechanical properties of the material, which needs to be further overcome.
[0006] Patent CN111394876A discloses a high-shielding fabric, but it has certain limitations when used on advertising cloths because it simply enhances shielding and light-shielding properties through a base material. It is basically unable to completely block the advertising display frame, affecting the overall look of the picture. If there is light on the back, there will be a little light leakage. The light exposure will also weaken the color of the advertisement due to the different degrees of absorption and reflection of the ink on the picture, affecting the vividness of the picture. By applying a shielding coating to its surface, it can better adapt to the external environment and achieve the advertising effect.
[0007] Therefore, there is a need for an environmentally friendly advertising cloth with high fire resistance, high hiding power and good mechanical properties. Summary of the invention
[0008] In order to solve the above problems, a high-fire-proof and high-coverage advertising cloth and a preparation method thereof are provided. The advertising cloth is prepared by combining a specific halogen-free flame retardant with expandable graphite under a specific process and has excellent flame retardancy, shielding properties and mechanical properties.
[0009] The specific technical solutions of this application are as follows:
[0010] The present application provides a high-fireproof and high-coverage advertising cloth, comprising a substrate, a primer slurry coated on the substrate, and a surface coating slurry coated on the primer slurry;
[0011] The substrate is obtained by immersing yarn in a pretreatment liquid containing 4.5-5.5% of polyethylene oxide with an average molecular weight of 100,000-3,000,000 and then setting it at 215-225°C; the polyethylene oxide within the molecular weight range can ensure the feel of the fabric and a certain saturation of the ink.
[0012] The primer coating comprises the following components in parts by weight:
[0013] The composite flame retardant Trimer / APP is 55-57 parts, the titanium dioxide is 30-35 parts, and the water-based polyurethane adhesive is 85-92 parts. The preparation method is as follows: according to the formula, 55-57 parts of the composite flame retardant Trimer / APP and 30-35 parts of titanium dioxide are weighed, water is added, and the primer coating is obtained after stirring and grinding.
[0014] The topcoat slurry comprises the following components in parts by weight:
[0015] The composite flame retardant Trimer / APP 55-59 parts, expandable graphite 5-6 parts, water-based polyurethane adhesive 85-92 parts, flame retardant accelerator 0.4-0.6 parts. The preparation method is as follows: according to the formula, weigh 55-59 parts of the composite flame retardant Trimer / APP, 5-6 parts of expandable graphite, add water, stir and grind, add 0.4-0.6 parts of flame retardant accelerator, and stir again to obtain the topcoat slurry.
[0016] Optionally, the primer coating further comprises the following components in parts by weight:
[0017] The preparation method is as follows: according to the formula, weigh 55-57 parts of the composite flame retardant Trimer / APP, 30-35 parts of titanium dioxide, 0.3-0.8 parts of the dispersant, 0.5-0.8 parts of the wetting agent, 0.5-0.7 parts of the leveling agent, and 0.6-1 parts of the defoaming agent, add 40 parts of water, disperse in a high-speed mixer for 15 minutes, grind, add 85-92 parts of water-based polyacrylic latex or polyurethane latex and 1-2 parts of curing agent, stir at a speed of 25-40rpm / min for 10-20 minutes; add a thickener to thicken to a viscosity of 6500-7500mPa.s to obtain a primer.
[0018] Optionally, the topcoat slurry further comprises the following components in parts by weight:
[0019] 7-8 parts of kaolin, 0.3-0.7 parts of dispersant, 0.2-0.5 parts of wetting agent, 0.5-0.7 parts of leveling agent, 0.6-1 parts of defoamer, 0.2-0.4 parts of thickener and 1-2 parts of curing agent. The preparation method is as follows: according to the formula, weigh 55-59 parts of composite flame retardant Trimer / APP, 5-6 parts of expandable graphite, 7-8 parts of inorganic filler kaolin, 0.3-0.7 parts of dispersant, 0.2-0.5 parts of wetting agent, add 60 parts of water, disperse for 20 minutes with a high-speed stirrer, add 85-92 parts of water-based polyacrylic latex or polyurethane latex and 1-2 parts of curing agent after grinding, stir at 25-40rpm / min for 10-20 minutes, thicken with thickener to a viscosity of 6500-7500mPa.s, and obtain a topcoat slurry.
[0020] Furthermore, the water-based polyurethane adhesive of the primer coating and the top coating slurry includes water-based polyacrylic latex and polyurethane latex.
[0021] The dispersants in the primer and topcoat slurry include phosphate dispersants, polyacid homopolymer dispersants, and polyacid copolymer dispersants; the wetting agent includes modified polydimethylsiloxane;
[0022] The leveling agent is organic siloxane or modified organic siloxane;
[0023] The defoamer is propylene oxide, or a mixture of ethylene oxide and propylene oxide;
[0024] The thickener is at least one of a polyurethane type, a synergistic thickener, and a polycarboxylic acid type;
[0025] The curing agent includes p-hydroxybenzenesulfonic acid.
[0026] Furthermore, the polyurethane thickener includes hydrophobically modified ethoxy polyurethane; the synergistic thickener includes diisocyanate; and the phosphate dispersant includes sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.
[0027] Preferably, the dispersant is prepared by mixing a polyacid homopolymer dispersant and a polyacid copolymer dispersant; the preferred dispersants are Tehaosan Kuaiyi and Tehaosan 731A.
[0028] Furthermore, the substrate is prepared by the following method:
[0029] Three yarns are used as the base material, the base material is put into the overflow cylinder to wash the cloth for about 4 hours, the cloth is opened and dropped after drying, and then the cloth is shaped at 215-225℃ on a shaping machine by impregnation with 5% polyethylene oxide pretreatment liquid with an average molecular weight of 100000-3000000.
[0030] Furthermore, the three yarns are all three-comb warp knitted fabrics with a fineness of 50-60D, a longitudinal and transverse density of 32×54, and a weight of 120-170gsm.
[0031] The present application also provides a method for preparing the above-mentioned advertising cloth, comprising the following steps:
[0032] Step 1: Use a scraper to apply the primer slurry on the impregnated substrate; dry at 130-170°C and 20m / min;
[0033] Step 2: Use a scraper to apply the topcoat slurry on the basecoat, dry it at 130-170°C and 20m / min to obtain an advertising cloth.
[0034] Optionally, the dry coating weight of the base coating slurry and the top coating slurry is 35-45 gsm; preferably, 40 gsm.
[0035] The present application also provides the use of the above-mentioned advertising cloth in the preparation of high-quality advertising textiles.
[0036] The polymerization rate of water-based latex is fast, and the product molecular weight is high. The polymerization can be carried out at a lower temperature. Water-based latex can bond halogen-free expandable flame retardant components together; but this also makes the free volume of the system smaller, the expansion ratio is not large when heated, and the uniformity of the pores inside the carbonized layer is slightly poor. This application adds filler-expandable graphite. On the one hand, the expandable graphite and the halogen-free expansion system play a synergistic role to promote foaming; on the other hand, it can enhance the toughness of the coating and the carbonized layer and improve the ability to resist gas erosion; expandable graphite just meets these two requirements.
[0037] Expandable graphite is a natural crystalline graphite that can expand into a worm shape instantly when exposed to high temperature after special treatment: it exists in a stable crystal form at room temperature and has good corrosion resistance and weather resistance.
[0038] The beneficial effects of this application include but are not limited to:
[0039] 1. This application adds fillers - expandable graphite and halogen-free flame retardant. The expandable graphite and the halogen-free expansion system play a synergistic role to promote foaming; on the other hand, it can enhance the strength of the coating and carbonized layer and improve the ability to resist gas erosion.
[0040] 2. The halogen-free flame retardant added in this application is a composite flame retardant Trimer / APP. The composite flame retardant Trimer / APP can cooperate with expandable graphite to promote rapid carbonization. The product test shows the beneficial effect of no smoldering and dripping. It is significantly better than the traditional expansion flame retardant system with expandable graphite in terms of anti-oxidation, damage length, flame propagation speed, and heat release. It can also enhance the tensile strength of the product.
[0041] 3. Furthermore, the mixed use of polyacid homopolymer dispersants and polyacid copolymer dispersants can better adsorb flame retardant particles, prevent particle agglomeration, further improve the compatibility of flame retardants with other components and substrates, and solve the problem of poor dispersion of halogen-free flame retardants in materials, thereby causing low mechanical properties of materials, and further improve the flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0043] Figure 1 This is a schematic diagram of the advertising cloth structure for this application.
[0044] List of parts and reference numerals:
[0045] 1. Substrate, 2. Primer, 3. Topcoat. DETAILED DESCRIPTION
[0046] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0047] Unless otherwise specified, the raw materials and catalysts in the examples of this application were purchased through commercial channels.
[0048] Example 1
[0049] A high-fireproof and high-coverage advertising cloth is prepared by the following method:
[0050] Step 1: Use three yarns as the base material, put the base material into the overflow tank to wash the cloth for about 4 hours, spin dry and then open the cloth to drop, and then immerse the cloth in a pretreatment liquid containing 5% polyethylene oxide with an average molecular weight of about 1,000,000 and set it on a setting machine at 220°C;
[0051] All three yarns are three-comb warp knitted fabrics with a fineness of 55D, a longitudinal and transverse density of 32×54, and a gram weight of approximately 150gsm.
[0052] Step 2: Use a scraper to apply the primer slurry on the impregnated substrate; dry at 150° C. and 20 m / min.
[0053] The bottom coating slurry preparation process is as follows:
[0054] Calculated by weight, weigh 55 parts of composite flame retardant Trimer / APP, 35 parts of titanium dioxide, 0.8 parts of dispersant (Super Good Dispersion Quick and Easy: Super Good Dispersion 731A mixed in a mass ratio of 1:1), 0.5 parts of wetting agent-modified polydimethylsiloxane, 0.7 parts of leveling agent-organic siloxane, 0.6 parts of defoaming agent-propylene oxide, add 40 parts of water, disperse in a high-speed stirrer for 15 minutes, add 85 parts of water-based polyacrylic latex and 2 parts of curing agent (p-hydroxybenzenesulfonic acid) after grinding, stir at a speed of 30rpm / min for 15 minutes; then use a polyurethane thickener (hydrophobically modified ethoxy polyurethane) to thicken to a viscosity of about 7000mPa.s to obtain a primer slurry.
[0055] Step 3: Use a scraper to apply the topcoat slurry on the basecoat layer, dry it at 150°C and 20m / min, and the basecoat layer has a dry coating weight of 40gsm.
[0056] The surface coating slurry preparation process is as follows:
[0057] Calculated by weight, 55 parts of composite flame retardant Trimer / APP, 6 parts of expandable graphite, 7 parts of inorganic filler kaolin, 0.7 parts of dispersant (Super Good Powder Quick and Easy: Super Good Powder 731A mixed in a mass ratio of 1:1), 0.2 parts of wetting agent (modified polydimethylsiloxane) were weighed, added to 60 parts of water, dispersed with a high-speed stirrer for 20 minutes, and after grinding, 92 parts of water-based polyacrylic latex and 1 part of curing agent (p-hydroxybenzenesulfonic acid) were added. The mixture was stirred at high speed for 15 minutes, and a thickener (hydrophobically modified ethoxy polyurethane) was used to thicken the mixture to a viscosity of 4#30rpm 7500mPa.s to obtain a top coating slurry.
[0058] The obtained advertising cloth structure is as follows Figure 1 shown.
[0059] In this embodiment, different pretreatments were performed on the yarns for screening, and the specific results are shown in Table 1.
[0060] The advertising cloth sample prepared in this embodiment was evaluated for ink droplet bleeding phenomenon; the evaluation method was: using a direct-injection machine to print a 400% ink black block on the advertising cloth sample, and observing the bleeding phenomenon at the edge of the black block.
[0061] Table 1 Effects of different yarn pretreatment methods on products
[0062]
[0063] According to the data in the above table, it can be seen that the relatively best pretreatment for the yarn is to immerse the yarn in a pretreatment liquid containing 100,000 to 3,000,000 polyethylene oxide and then fix it at 215-225°C.
[0064] The yarn substrate treated with the treatment liquid and the setting temperature will not show the phenomenon of ink droplet bleeding.
[0065] The pretreatment technology can solve the infiltration phenomenon in the prior art that ink droplets are easily diffused to the surroundings along the warp and weft directions of the fiber, and achieve the effect of bright color and high pattern precision of the fabric after inkjet printing.
[0066] Example 2
[0067] Step 1: Use three yarns as the base material, put the base material into the overflow tank to wash the cloth for about 4 hours, spin dry and then open the cloth to drop, and then immerse the cloth in a pretreatment liquid containing 5% polyethylene oxide with an average molecular weight of about 1,000,000 and set it on a setting machine at 220°C;
[0068] All three yarns are three-comb warp knitted fabrics with a fineness of 55D, a longitudinal and transverse density of 32×54, and a gram weight of approximately 150gsm.
[0069] Step 2: Use a scraper to apply the primer slurry on the impregnated substrate; dry at 150° C. and 20 m / min.
[0070] The bottom coating slurry preparation process is as follows:
[0071] Calculated by weight, weigh 55 parts of composite flame retardant Trimer / APP, 35 parts of titanium dioxide, 0.8 parts of dispersant (sodium tripolyphosphate and Tehaosan 731A mixed in a mass ratio of 1:1), 0.5 parts of wetting agent-modified polydimethylsiloxane, 0.7 parts of leveling agent-organic siloxane, 0.6 parts of defoaming agent-propylene oxide, add 40 parts of water, disperse in a high-speed stirrer for 15 minutes, add 85 parts of water-based polyacrylic latex and 2 parts of curing agent (p-hydroxybenzenesulfonic acid) after grinding, stir at a speed of 30rpm / min for 15 minutes; then use a polyurethane thickener (hydrophobically modified ethoxy polyurethane) to thicken to a viscosity of about 7000mPa.s to obtain a primer slurry.
[0072] Step 3: Use a scraper to apply the topcoat slurry on the basecoat layer, dry it at 150°C and 20m / min, and the basecoat layer has a dry coating weight of 40gsm.
[0073] The surface coating slurry preparation process is as follows:
[0074] Calculated by weight, weigh 55 parts of composite flame retardant Trimer / APP, 6 parts of expandable graphite, 7 parts of inorganic filler kaolin, 0.7 parts of dispersant (Super Good Powder Quick and Easy: Super Good Powder 731A mixed in a mass ratio of 1:1), 0.2 parts of wetting agent (modified polydimethylsiloxane), add to 60 parts of water, disperse with a high-speed stirrer for 20 minutes, add 92 parts of water-based polyacrylic latex and 1 part of curing agent (p-hydroxybenzenesulfonic acid) after grinding, stir at high speed for 15 minutes, use a thickener (hydrophobic modified ethoxy polyurethane) to thicken to a viscosity of 4#30rpm 7500mPa.s, and obtain a top coating slurry.
[0075] Example 3
[0076] A high-fireproof and high-coverage advertising cloth is prepared by the following method:
[0077] Step 1: Use three yarns as the base material, put the base material into the overflow tank to wash the cloth for about 4 hours, spin dry and then open the cloth to drop, and then immerse the cloth in a pretreatment liquid containing 5% polyethylene oxide with an average molecular weight of about 1,000,000 and set it on a setting machine at 220°C;
[0078] All three yarns are three-comb warp knitted fabrics with a fineness of 55D, a longitudinal and transverse density of 32×54, and a gram weight of approximately 150gsm.
[0079] Step 2: Use a scraper to apply the primer slurry on the impregnated substrate; dry at 150° C. and 20 m / min.
[0080] The bottom coating slurry preparation process is as follows:
[0081] Calculated by weight, weigh 56 parts of composite flame retardant Trimer / APP, 32 parts of titanium dioxide, 0.5 parts of dispersant (Tehaosan 731A), 0.7 parts of wetting agent-modified polydimethylsiloxane, 0.6 parts of leveling agent-organic siloxane, 0.8 parts of defoaming agent-propylene oxide, add 40 parts of water, disperse in a high-speed stirrer for 15 minutes, add 90 parts of polyurethane latex and 1 part of curing agent (p-hydroxybenzenesulfonic acid) after grinding, stir at a speed of 30rpm / min for 15 minutes; then use a thickener (hydrophobically modified ethoxy polyurethane) to thicken to a viscosity of 7500mPa.s to obtain a primer slurry.
[0082] Step 3: Use a scraper to apply the topcoat slurry on the basecoat layer, dry it at 150°C and 20m / min, and the basecoat layer has a dry coating weight of 40gsm.
[0083] The surface coating slurry preparation process is as follows:
[0084] Calculated by weight, 57 parts of composite flame retardant Trimer / APP, 6 parts of expandable graphite, 8 parts of inorganic filler kaolin, 0.5 parts of dispersant (Tehaosan 731A), and 0.4 parts of wetting agent (modified polydimethylsiloxane) were weighed, added to 60 parts of water, dispersed with a high-speed stirrer for 20 minutes, and after grinding, 88 parts of polyurethane latex and 2 parts of curing agent (p-hydroxybenzenesulfonic acid) were added. The mixture was stirred at a speed of 30 rpm / min for 15 minutes, and a thickener (hydrophobically modified ethoxy polyurethane) was used to thicken the mixture to a viscosity of about 6700 mPa.s to obtain a top coating slurry.
[0085] Example 4
[0086] A high-fireproof and high-coverage advertising cloth is prepared by the following method:
[0087] Step 1: Use three yarns as the base material, put the base material into the overflow tank to wash the cloth for about 4 hours, spin dry and then open the cloth to drop, and then immerse the cloth in a pretreatment liquid containing 5% polyethylene oxide with an average molecular weight of about 1,000,000 and set it on a setting machine at 220°C;
[0088] All three yarns are three-comb warp knitted fabrics with a fineness of 55D, a longitudinal and transverse density of 32×54, and a gram weight of approximately 150gsm.
[0089] Step 2: Use a scraper to apply the primer slurry on the impregnated substrate; dry at 150° C. and 20 m / min.
[0090] The bottom coating slurry preparation process is as follows:
[0091] Calculated by weight, weigh 56 parts of composite flame retardant Trimer / APP, 30-35 parts of titanium dioxide, 0.7 parts of dispersant (super good dispersion), 0.5 parts of wetting agent-modified polydimethylsiloxane, 0.6 parts of leveling agent-organic siloxane, 0.8 parts of defoaming agent-propylene oxide, add 40 parts of water, disperse in a high-speed stirrer for 15 minutes, add 86 parts of water-based polyacrylic latex and 1 part of curing agent (p-hydroxybenzenesulfonic acid) after grinding, and stir at a speed of 30rpm / min for 15 minutes; then use a polyurethane thickener (hydrophobically modified ethoxy polyurethane) to thicken to a viscosity of about 6900mPa.s to obtain a primer slurry.
[0092] Step 3: Use a scraper to apply the topcoat slurry on the basecoat layer, dry it at 150°C and 20m / min, and the basecoat layer has a dry coating weight of 40gsm.
[0093] The surface coating slurry preparation process is as follows:
[0094] Calculated by weight, 58 parts of composite flame retardant Trimer / APP, 6 parts of expandable graphite, 8 parts of inorganic filler kaolin, 0.4 parts of dispersant (super good dispersion), and 0.4 parts of wetting agent (modified polydimethylsiloxane) were weighed, added to 60 parts of water, dispersed with a high-speed stirrer for 20 minutes, and after grinding, 89 parts of water-based polyacrylic latex and 1-2 parts of curing agent (p-hydroxybenzenesulfonic acid) were added, stirred at a speed of 30 rpm / min for 15 minutes, and thickened with a thickener (hydrophobically modified ethoxy polyurethane) to a viscosity of 7500 mPa.s to obtain a top coating slurry.
[0095] Comparative Example 1
[0096] The difference from Example 1 is that the expandable graphite is replaced by ordinary carbon black.
[0097] Comparative Example 2
[0098] The difference from Example 1 is that the flame retardant used is different. The composite flame retardant is replaced with a bromine antimony flame retardant (obtained by compounding antimony trioxide and decabromodiphenylethane in a mass ratio of 1:1). The rest is the same as Example 1.
[0099] Comparative Example 3
[0100] The difference from Example 1 is that the halogen-free flame retardant used is different, that is, a mixed flame retardant obtained by compounding pentaerythritol, melamine and ammonium polyphosphate in a mass ratio of 1:1:1; and the expandable graphite is replaced by ordinary carbon black.
[0101] Comparative Example 4
[0102] The difference from Example 1 is that the halogen-free flame retardant used is different, and is a mixed flame retardant obtained by compounding pentaerythritol, melamine, and ammonium polyphosphate in a mass ratio of 1:1:1.
[0103] Comparative Example 5
[0104] The difference from Example 1 is that the preparation process is different: the high-shielding fabric disclosed in patent CN111394876A is directly dipped into the sample with 5% pretreatment liquid, and no other coating is applied.
[0105] Comparative Example 6
[0106] The difference from Example 1 is that expandable graphite is not added to the topcoat slurry. The rest is the same as Example 1.
[0107] Performance testing
[0108] The performance of the products prepared in the above examples and comparative examples was tested according to GB / T 8624 and DIN EN 13501-1. The results are shown in Tables 2 and 3 below.
[0109] FIGRA combustion growth rate index; flame lateral spread length LFS; total heat release THR600; flame tip height within 60s.
[0110] Table 2 Performance test of different products
[0111]
[0112] Table 2
[0113]
[0114] Compared with Comparative Example 3, the composite flame retardant Trimer / APP is significantly superior to the traditional intumescent flame retardant in terms of anti-oxidation, damage length, flame propagation speed, and heat release. Compared with Comparative Example 1, the embodiment of the present application adds expandable graphite to coordinate the composite flame retardant Trimer / APP, which is significantly better than Comparative Example 1 without adding it in terms of damage length, indicating that the addition of expandable graphite helps to quickly form carbon. Compared with Comparative Example 4, the embodiment is significantly better than the traditional intumescent flame retardant system with expandable graphite in terms of anti-oxidation, damage length, flame propagation speed, and heat release. Compared with Comparative Example 2, the present application is halogen-free and heavy metal-free, and its flame retardant performance index almost all exceeds that of bromine-antimony flame retardants. In particular, the intumescent system with the addition of expandable graphite and the synergistic composite flame retardant Trimer / APP has no smoldering and dripping phenomenon.
[0115] In addition, according to the comparison between Example 1 and Example 2, it can be seen that when the dispersant is a mixture of a polyacid homopolymer dispersant and a polyacid copolymer dispersant, the flame retardant effect is better. The reason may be that the mixture of the two can better adsorb the flame retardant particles and prevent the particles from agglomerating, thereby improving the compatibility of the flame retardant with other components and the substrate.
[0116] According to the examples and comparative example 6, after adding expandable graphite, the damage length of the product is significantly shortened, and the combustion growth rate index and the lateral flame spread length are significantly reduced, which indicates that expandable graphite has good flame retardancy after being added to the present application.
[0117] In addition, in the embodiment, the dispersant, wetting agent, leveling agent, and defoaming agent are mixed and added to form a uniform and stable coating, which has a positive effect on light shielding and flame retardancy.
[0118] The fire protection test comparison of the product in this application shows that it can achieve the B1 fire protection required by GB / T 8624 and the B fire protection in the European standard DIN EN13501-1.
[0119] Table 3 Performance tests of different products
[0120]
[0121] Compared with comparative examples 4-6, the opacity value of the present invention is the largest and the covering power is the strongest; the opacity and color density of the coated fabric far exceed the high-shielding fabric disclosed in patent CN111394876A without coating; the covering power and color density of the black coating are also better than those without black coating; from the comparison of the color density without lighting and backlighting, the larger the opacity value, the smaller the color density attenuation after lighting.
[0122] In addition, the addition of titanium dioxide in the base coating can cover the black topcoat while ensuring that the coating has a certain adhesion.
[0123] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A highly fireproof and high-covering advertising cloth, characterized in that: It includes a substrate, a primer slurry coated on the substrate, and a top coating slurry coated on the primer slurry; The substrate is obtained by padding the yarn with a polyethylene oxide pretreatment solution containing 4.5-5.5% of an average molecular weight of 100,000-3,000,000 and then setting it at 215-225°C; The primer coating comprises the following components in parts by weight: Composite flame retardant Trimer / APP 55-57 parts, titanium dioxide 30-35 parts; The topcoat slurry comprises the following components in parts by weight: Composite flame retardant Trimer / APP 55-59 parts, expandable graphite 5-6 parts, water-based polyurethane adhesive 85-92 parts, flame retardant accelerator 0.4-0.6 parts.
2. The advertising cloth according to claim 1, characterized in that: The primer coating also includes the following components in parts by weight: Dispersant 0.3-0.8 parts, wetting agent 0.5-0.8 parts, leveling agent 0.5-0.7 parts, defoaming agent 0.6-1 parts.
3. The advertising cloth according to claim 1, characterized in that: The topcoat slurry also includes the following components in parts by weight: 7-8 parts of kaolin, 0.3-0.7 parts of dispersant, 0.2-0.5 parts of wetting agent, 0.5-0.7 parts of leveling agent, 0.6-1 parts of defoaming agent, 0.2-0.4 parts of thickener and 1-2 parts of curing agent.
4. The advertising cloth according to claim 1, characterized in that: The water-based polyurethane adhesive includes water-based polyacrylic acid latex and polyurethane latex.
5. The advertising cloth according to claim 1, characterized in that: The primer coating is prepared by the following method: According to the formula, weigh 55-57 parts of the composite flame retardant Trimer / APP and 30-35 parts of titanium dioxide, add water, and obtain the primer coating after stirring and grinding.
6. The advertising cloth according to claim 2, characterized in that: The primer coating is prepared by the following method: According to the formula, weigh 55-57 parts of composite flame retardant Trimer / APP, 30-35 parts of titanium dioxide, 0.3-0.8 parts of dispersant, 0.5-0.8 parts of wetting agent, 0.5-0.7 parts of leveling agent, 0.6-1 parts of defoaming agent, add 40 parts of water, disperse in a high-speed mixer for 15 minutes, add 85-92 parts of water-based polyacrylic latex or polyurethane latex and 1-2 parts of curing agent after grinding, stir at 25-40rpm / min for 10-20 minutes; add thickener to thicken to a viscosity of 6500-7500mPa.s.
7. The advertising cloth according to claim 1, characterized in that: The topcoat slurry is prepared by the following method: weigh 55-59 parts of the composite flame retardant Trimer / APP and 5-6 parts of expandable graphite according to the formula, add water, stir and grind, add 0.4-0.6 parts of the flame retardant accelerator, and stir again to obtain the topcoat slurry.
8. The advertising cloth according to claim 2, characterized in that: The topcoat slurry is prepared by the following method: According to the formula, weigh 55-59 parts of composite flame retardant Trimer / APP, 5-6 parts of expandable graphite, 7-8 parts of inorganic filler kaolin, 0.3-0.7 parts of dispersant, 0.2-0.5 parts of wetting agent, add into 60 parts of water, disperse with high-speed stirrer for 20 minutes, add 85-92 parts of water-based polyacrylic latex or polyurethane latex and 1-2 parts of curing agent after grinding, stir at 25-40rpm / min for 10-20 minutes, and thicken with thickener to the viscosity of 6500-7500mPa.s.
9. The advertising cloth according to any one of claims 1 to 8, characterized in that: The substrate is prepared by the following method: Three yarns are used as the base material, the base material is put into the overflow cylinder to wash the cloth for about 4 hours, the cloth is opened and dropped after drying, and then the cloth is shaped at 215-225℃ on a shaping machine by impregnation with 5% polyethylene oxide pretreatment liquid with an average molecular weight of 100000-3000000.
10. A method for preparing the advertising cloth as claimed in any one of claims 1 to 9, characterized in that: The steps include: Step 1: Use a scraper to apply the primer slurry on the impregnated substrate; dry at 130-170°C and 20m / min; Step 2: Use a scraper to apply the topcoat slurry on the basecoat, dry it at 130-170°C and 20m / min to obtain an advertising cloth.