Recording method and composition set
By using a composition of high content of softener and resin particles in inkjet printing and dyeing, the problem of firmness of image wet friction and poor feel in inkjet printing and dyeing is solved, the process is simplified and the environmental load is reduced, and the image is efficient Attachment and color fixation.
Patent Information
- Application Number
- CN202410700436.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In inkjet printing and dyeing, the wet friction between pigment printing and dyeing images is firm and hard and has poor hand feel, and the process is complicated, and the drainage environment is high, making it difficult to simplify.
The soft liquid composition containing softener and water and the coating liquid composition containing anionic resin particles are used, and the softener content reaches more than 60%, and the resin particle content reaches more than volatile components. More than 80%, the wet friction firmness and feel of the image are improved by the adhesion process of soft liquid and coating liquid respectively.
The wet friction firmness and feel of the recording medium is significantly improved, the process is simplified, the environmental load is reduced, and a firm resin film is formed to prevent the color material from falling off.
Smart Images

Figure HDA0004870892310000011 
Figure HDA0004870892310000021 
Figure HDA0004870892310000031
Abstract
Description
Technical Field
[0001] The present invention relates to a recording method and a composition set. Background Art
[0002] The inkjet method is not only applicable to recording images on paper, but also to printing and dyeing of fabrics, and various inkjet printing and dyeing have been studied. Inkjet inks used for printing and dyeing contain color materials in order to obtain images of desired colors, and dyes and pigments are used as color materials. In addition, in inkjet printing and dyeing, various studies have been conducted on inks and recording methods.
[0003] For example, Patent Document 1 describes that in inkjet printing, organopolysiloxane is used for the purpose of improving image fastness by pigments, improving the feel of recorded materials, and the like.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: Japanese Patent Application Publication No. 2022-003175.
[0007] Pigment printing is inferior to dye printing in wet friction fastness of images and the feel of printed materials, and these are required to be improved. In addition, inkjet pigment printing is superior to analog printing and inkjet dye printing in that the process is simplified and the environmental load such as drainage is low, and it is also required to maintain the simplified process. Summary of the invention
[0008] One embodiment of the recording method according to the present invention comprises:
[0009] a softening liquid attaching step of attaching a softening liquid composition containing a softener and water to the recording medium; and
[0010] a coating liquid attaching step of attaching a coating liquid composition containing anionic resin particles and water to a recording medium,
[0011] The content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition.
[0012] The content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition.
[0013] The coating liquid attachment step is performed by an inkjet method,
[0014] The softening liquid attaching step is performed by an inkjet method or a spray method.
[0015] One embodiment of the composition set according to the present invention comprises:
[0016] A softening liquid composition comprising a softener and water; and
[0017] The coating liquid composition comprises anionic resin particles and water.
[0018] The content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition.
[0019] The content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition.
[0020] The coating liquid composition is used by ejecting it by an inkjet method.
[0021] The softening liquid composition is used by being ejected by an inkjet method or a spray method. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram showing a schematic overall structure of a recording device that can be applied to the recording method involved in this embodiment.
[0023] Figure 2 This is a schematic diagram showing an example of the arrangement of nozzle rows of an inkjet head.
[0024] Figure 3 It is a diagram showing ink ejected from the nozzle array in the example and the comparative example.
[0025] Figure 4 This is a table (Table 1) showing the composition of the first ink according to Examples and Comparative Examples.
[0026] Figure 5 This is a table (Table 2) showing the composition of the second ink according to Examples and Comparative Examples.
[0027] Figure 6 This is a table (Table 3) showing the composition of the third ink according to Examples and Comparative Examples.
[0028] Figure 7 This is a table (Table 4) showing the composition of the fourth ink according to Examples and Comparative Examples.
[0029] Figure 8 This is a table (Table 5) showing conditions and evaluation results related to the examples.
[0030] Fig. 9 This is a table (Table 6) showing the conditions and evaluation results involved in the examples.
[0031] Fig.10 This is a table (Table 7) showing the conditions and evaluation results involved in the examples.
[0032] Fig.11This is a table (Table 8) showing conditions and evaluation results related to the examples.
[0033] Fig.12 This is a table (Table 9) showing conditions and evaluation results related to comparative examples.
[0034] Explanation of symbols
[0035] 1. Control unit; 10. Medium supply unit; 11. Supply shaft unit; 12. Bearing unit; 20. Medium conveying unit; 21. Conveying roller; 22. Conveying roller; 23. Endless belt; 23a. Surface; 23b. Inner peripheral surface; 24. Belt rotating roller; 25. Belt driving roller; 26. Conveying roller; 27. Heating unit; 28. Conveying roller; 29. Adhesive; 30. Medium recovery unit; 31. Reel unit; 32. Bearing unit; 40. Printing unit; 42. Inkjet head; 42a, 42b, 42 c, 42d, nozzle array; 43, slide; 45, slide moving part; 45a, guide rail; 45b, guide rail; 46, pressure plate; 50, cleaning unit; 51, cleaning part; 52, pressing part; 53, moving part; 54, cleaning tank; 55, scraper; 56, cylinder; 57, ball bushing; 58, cleaning roller; 60, medium contact part; 61, pressing part; 69, abutment part; 90, frame part; 91, belt supporting part; 95, cloth; 99, ground; 100, recording device. DETAILED DESCRIPTION
[0036] Hereinafter, the embodiments of the present invention will be described. The embodiments described below are exemplary embodiments of the present invention. The present invention is not limited to the following embodiments, but also includes various modifications implemented within the scope of not changing the gist of the present invention. In addition, the configurations described below are not necessarily all necessary configurations of the present invention.
[0037] 1. Recording method
[0038] The recording method according to this embodiment includes a softening liquid attaching step of attaching a softening liquid composition containing a softener and water to a recording medium and a coating liquid attaching step of attaching a coating liquid composition containing anionic resin particles and water to a recording medium.
[0039] 1.1. Recording medium
[0040] The recording medium to which the recording method of this embodiment can be applied is not particularly limited. The recording medium may be a recording medium having a recording surface that absorbs ink or a recording medium that does not have a recording surface that absorbs ink. Therefore, the recording medium is not particularly limited, and examples thereof include liquid-absorbing recording media such as paper, film, and cloth; liquid-low-absorbing recording media such as printing paper; and liquid-non-absorbing recording media such as metal, glass, and polymers.
[0041] In the recording method of this embodiment, by using cloth even in the recording medium, the effect of improving the wet friction resistance and color development becomes more significant. The cloth is not particularly limited. The raw materials constituting the cloth are not particularly limited, and examples thereof include natural fibers such as cotton, linen, wool, and silk; synthetic fibers such as polypropylene, polyester, acetate, triacetate, polyamide, and polyurethane; biodegradable fibers such as polylactic acid, and blended fibers thereof. The cloth may be a cloth made of the above-mentioned fibers in any form such as woven fabrics, knitted fabrics, and non-woven fabrics, or a cloth mixed with weaving.
[0042] 1.2. Softening liquid attachment process
[0043] The softening liquid attaching step is to attach a softening liquid composition containing a softener and water to the recording medium.
[0044] 1.2.1. Softening liquid composition
[0045] The softening liquid composition contains a softener and water, and the content of the softener is 60% by mass or more based on the total amount of nonvolatile components in the softening liquid composition.
[0046] 1.2.1.(1) Softener
[0047] Examples of the softener include particles containing organopolysiloxane, fatty acid esters, dialkyldimethylammonium salts, imidazoline-based surfactants, and amphoteric surfactants.
[0048] Particles containing organopolysiloxane
[0049] The particles containing organopolysiloxane are not particularly limited as long as they contain organopolysiloxane, and may be, for example, particles of organopolysiloxane itself or particles in which organopolysiloxane is dispersed by an emulsifier, etc. The organopolysiloxane in the particles may be solid or liquid. For example, when oily organopolysiloxane is dispersed in water in the form of particles by an emulsifier, the dispersed particles correspond to particles containing organopolysiloxane.
[0050] Organopolysiloxane is a siloxane bond "-Si(R 1 R 2 )-O-" is a skeleton, in which methyl, phenyl, vinyl, amino, etc. are combined as organic groups R 1 , R 2 A general term for organosilicon compounds. Organopolysiloxanes can be oily, rubbery, or resinous, depending on their chemical composition and molecular weight, and are sometimes referred to as silicone oil, silicone rubber, or silicone resin (silicone resin), respectively.
[0051] The organopolysiloxane used in the softening liquid composition of the present embodiment is more preferably an oily compound. If the organopolysiloxane is an oily compound, it is easy to stably disperse it in the form of particles in an aqueous base by the emulsification treatment described below.
[0052] The molecular structure of the organopolysiloxane is not particularly limited, and examples thereof include linear, branched, cyclic, lattice, basket, etc. When the molecular structure of the organopolysiloxane is a non-cyclic structure, one or more groups selected from a hydrocarbon group which may have a substituent, an alkoxy group, a hydroxyl group, a hydrogen atom, and a halogen are usually bonded to the terminal Si atom of the molecule.
[0053] The organopolysiloxane is not particularly limited, and examples thereof include dimethyl silicone, alkyl-modified silicone, amino-modified silicone, epoxy-modified silicone, cyclic silicone, and methylphenyl silicone. These may be used alone or in combination of two or more.
[0054] In addition, the organopolysiloxane may also be a commercially available organosilicon oil. Examples thereof include dimethyl silicone oil, methylphenyl silicone oil, methyl hydrogen silicone oil, polyether modified silicone oil, aralkyl modified silicone oil, fluoroalkyl modified silicone oil, long-chain alkyl modified silicone oil, higher fatty acid ester modified silicone oil, higher fatty acid amide modified silicone oil, polyether / long-chain alkyl / aralkyl modified silicone oil, long-chain alkyl / aralkyl modified silicone oil, phenyl modified silicone oil, polyether / methoxy modified silicone oil, etc.
[0055] In addition, among the organopolysiloxanes exemplified above, nonionic silicones are more preferred. In addition, among the organopolysiloxanes exemplified above, unmodified silicones are more preferred. Such organopolysiloxanes are more chemically stable and are less likely to cause yellowing of the formed image.
[0056] Furthermore, the organopolysiloxane is more preferably at least one selected from dimethyl silicone, methylphenyl silicone, and methyl hydrogen silicone.
[0057] Commercially available products of silicone oil include: dimethyl silicone (manufactured by Shin-Etsu Chemical Co., Ltd.: KF-96 series), methyl hydrogen polysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.: KF-99 series, KF-9901, etc.), methyl phenyl silicone (manufactured by Shin-Etsu Chemical Co., Ltd.: KF-50 series, etc.), amino-modified silicone (manufactured by Shin-Etsu Silicone Co., Ltd., KF-868, etc.), silicone branched silicone treatment agent (manufactured by Shin-Etsu Chemical Co., Ltd.: KF-9908, KF-9909, etc.), etc.
[0058] The viscosity of silicone at 25°C is not particularly limited, but is preferably 1000 mPa·s or less, preferably 50 mPa·s or more, more preferably 500 mPa·s or more and 900 mPa·s or less, and further preferably 600 mPa·s or more and 700 mPa·s or less. The viscosity of the base oil in which silicone is emulsified and dispersed is not particularly limited, but the upper limit is preferably 1,000,000 mm 2 / s or less, more preferably 100000mm 2 / s or less, the lower limit is preferably 10mm 2 / s or more, more preferably 100mm 2 / s or more. In addition, the base oil viscosity indicates the viscosity of the base oil and is a numerical value obtained by measuring the internal resistance of the base oil. For the following base oils: the larger the base oil viscosity numerical value, the higher the viscosity, and the smaller the numerical value, the lower the viscosity.
[0059] The organopolysiloxane may be emulsified with various surfactants as emulsifiers to form particles and mixed. In this case, the emulsifier may be, for example, a nonionic surfactant, anionic surfactant, cationic surfactant, amphoteric surfactant, phospholipid, etc.
[0060] Examples of the nonionic surfactant include glycerol fatty acid esters, polyglycerol fatty acid esters, propylene glycol fatty acid esters, sorbitan fatty acid esters, and fatty acid esters of sorbitol, as well as alkylene glycol adducts thereof, polyalkylene glycol fatty acid esters, sucrose fatty acid esters, polysorbate 20, polysorbate 60, polysorbate 80, polyoxyalkylene alkyl ethers, and polyoxyethylene alkylphenyl ethers.
[0061] In addition, as the nonionic surfactant, it is also preferable to use nonionic surfactants such as polyoxyethylene glycerol fatty acid esters, polyglycerol fatty acid ester sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, polyethylene glycol fatty acid esters, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, polyoxyethylene phytosterols, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene lanolin, polyoxyethylene lanolin alcohol, polyoxyethylene beeswax derivatives, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, polyoxyethylene alkylphenyl formaldehyde condensates, and polyoxyethylene alkyl ether phosphates.
[0062] Examples of anionic surfactants include alkyl sulfate ester salts, polyoxyethylene alkyl sulfate ester salts, alkylbenzene sulfonates, α-olefin sulfonates, etc. Examples of cationic surfactants include alkyltrimethylammonium chloride, dialkyldimethylammonium chloride, benzalkonium chloride, etc. Examples of amphoteric surfactants include alkyldimethylaminoacetic acid betaine, alkylamidedimethylaminoacetic acid betaine, etc. In addition, naturally derived surfactants can be used, and examples thereof include lecithin, lanolin, cholesterol, saponin, etc.
[0063] The amount of the emulsifier blended when the organopolysiloxane is emulsified is preferably less than 20% by mass, more preferably 15% by mass or less, and particularly preferably 10% by mass or less, based on the total amount of the emulsified composition.
[0064] The average particle size of the particulate organopolysiloxane after emulsification is preferably 2 μm or less, more preferably 1 μm or less, and more preferably in the range of 0.05 to 0.5 μm.
[0065] Fatty acid esters
[0066] Examples of fatty acid esters include polyoxyethylene monocaprate, polyoxyethylene monocaprylate, polyoxyethylene monolaurate, polyoxyethylene monomyristate, polyoxyethylene monopalmitate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyoxyethylene monoisostearate, polyoxyethylene monobehenate, polyoxyethylene dicaprate, polyoxyethylene dicaprylate, polyoxyethylene dilaurate, polyoxyethylene dimyristate, polyoxyethylene dipalmitate, polyoxyethylene distearate, polyoxyethylene dioleate, polyoxyethylene diisostearate, and polyoxyethylene dibehenate.
[0067] Dialkyldimethylammonium salts
[0068] Examples of the dialkyldimethylammonium salts include (2,3-dioleyloxypropyl)trimethylammonium chloride (DOTAP), dioctadecenyloxy-3-methylammonium propane chloride (DOTMA), didecyldimethylammonium chloride, didecyldimethylammonium bromide, dicocoyldimethylammonium chloride, dicocoyldimethylammonium bromide, dilauryldimethylammonium chloride, diacetyldimethylammonium chloride, diacetyldimethylammonium bromide, distearyldimethylammonium chloride, distearyldimethylammonium bromide, dioleyldimethylammonium chloride, dibehenyldimethylammonium chloride, dibehenyldimethylammonium bromide, dialkyldimethylammonium chloride, dialkyldimethylammonium bromide, dicocoylethylhydroxyethylammonium methylsulfate, dipalmitoyloxyethylhydroxyethylammonium methylsulfate, and distearylethylhydroxyethylammonium methylsulfate.
[0069] Imidazoline surfactant
[0070] Examples of the imidazoline surfactant include 1-hydroxyethyl-2-lauryl imidazoline, 1-aminoethyl-2-lauryl imidazoline, 1-hydroxyethyl-2-myristyl imidazoline, 1-aminoethyl-2-myristyl imidazoline, 1-hydroxyethyl-2-palmityl imidazoline, 1-aminoethyl-2-palmityl imidazoline, 1-hydroxyethyl-2-oleyl imidazoline, 1-aminoethyl-2-oleyl imidazoline, 1-hydroxyethyl-2-stearyl imidazoline, 1-aminoethyl-2-stearyl imidazoline, 2-alkyl-N-carboxymethyl imidazoline betaine, 2-alkyl-N-carboxyethyl imidazolinium betaine, and 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine.
[0071] Amphoteric surfactant
[0072] Examples of the amphoteric surfactant include alkyl carboxybetaines, alkyl sulfobetaines, alkyl hydroxysulfobetaines, alkyl amidobetaines, lauryl dimethylamine oxide, and lauric acid amide propyl dimethylamine oxide.
[0073] The softener is preferably at least one selected from the above-exemplified particles containing organopolysiloxane, fatty acid esters, dialkyldimethylammonium salts, imidazoline surfactants and amphoteric surfactants. Thus, the wet friction fastness of the image of the recorded object formed by the recording method is further improved.
[0074] In addition, the softener is more preferably at least one selected from particles containing organopolysiloxane. Thus, the softening liquid composition can impart a water-repellent effect to the fibers of the recording medium, thereby further improving the wet friction fastness of the image of the recorded object.
[0075] Furthermore, when particles containing organopolysiloxane are selected as a softener, the organopolysiloxane is more preferably nonionic, thereby further reducing yellowing of recorded matter.
[0076] 1.2.1.(2) Water
[0077] The softening liquid composition contains water. Examples of the water include pure water such as ion exchange water, ultrafiltration water, reverse osmosis water, and distilled water, and water from which ionic impurities have been removed as much as possible, such as ultrapure water. In addition, if water is sterilized by ultraviolet irradiation or addition of hydrogen peroxide, the generation of bacteria and fungi can be reduced when the composition is stored for a long time.
[0078] The content of water is 30% by mass or more, preferably 40% by mass or more, more preferably 45% by mass or more, and further preferably 50% by mass or more relative to the total amount of the softening liquid composition. In addition, when it is referred to as water in the softening liquid, it includes, for example, water contained in the organic polysiloxane dispersion used as a raw material and added water. By making the content of water 30% by mass or more, the softening liquid composition can be made to have a relatively low viscosity. In addition, the upper limit of the content of water is preferably 90% by mass or less, more preferably 85% by mass or less, and further preferably 80% by mass or less relative to the total amount of the softening liquid composition. In addition, in this specification, when it is referred to as an "aqueous composition", it refers to a composition containing 30% by mass or more of water relative to the total mass (100% by mass) of the composition.
[0079] 1.2.1.(3) Other ingredients
[0080] The softening liquid composition may contain an emulsifier, a resin, a moisturizer, other solvents, and additives.
[0081] Emulsifier
[0082] As the emulsifier, the emulsifier used for forming the particles containing the above-mentioned organopolysiloxane may be contained, and the same emulsifier may be contained separately.
[0083] Resin
[0084] The softening liquid composition may contain a resin. As the resin, a water-soluble resin is preferred. As the water-soluble resin, there is no particular limitation, and examples thereof include carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl pyrrolidone, and polyethylene oxide. Among them, a nonionic resin is more preferred, and polyvinyl pyrrolidone is more preferred, for example. As polyvinyl pyrrolidone, it is not limited to a homopolymer, and a copolymer of vinyl pyrrolidone and other monomers may also be used. Commercially available products of polyvinyl pyrrolidone include, for example, polyvinyl pyrrolidone K-30, K-30W (the above are product names, manufactured by Nippon Shokubai Co., Ltd.), Pitzcol (registered trademark) K-17L, K-30, K-30L, K-30AL, K-60L, K-30, K-50, K-90, Creejus (registered trademark) K-30, Aiphtact (registered trademark) K-30PH (the above are product names, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), PVP K-30, PVP K-25, and PVP K-17 (the above are product names, manufactured by Ashland Inc.).
[0085] Moisturizer
[0086] The softening liquid composition may contain a moisturizer. The moisturizer is not particularly limited, and examples thereof include glycerin, 2-pyrroline, urea, triethanolamine, propylene glycol, 1-(2-hydroxyethyl)-2-pyrroline, trimethylolpropane, triethylene glycol, 1,5-pentanediol, triethylene glycol monomethyl ether, and amino coating. One or more of these may be used alone or in combination.
[0087] Other solvents
[0088] The softening liquid composition may also contain other solvents. As such a solvent, a water-soluble organic solvent is preferred. One of the functions of the organic solvent is to increase the wettability of the softening liquid composition to the fabric and to increase the moisture retention of the softening liquid composition. In addition, the organic solvent may also function as a penetrant.
[0089] Examples of organic solvents include esters, alkylene glycol ethers, cyclic esters, nitrogen-containing solvents, polyols, etc. Examples of nitrogen-containing solvents include cyclic amides, non-cyclic amides, etc. Examples of non-cyclic amides include alkoxyalkylamides, etc.
[0090] Examples of the esters include glycol monoacetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and ethylene glycol monobutyl ether acetate; and glycol diesters such as ethylene glycol diacetate, diethylene glycol diacetate, and propylene glycol diacetate.
[0091] The alkylene glycol ethers may be monoethers or diethers of alkylene glycol, and alkyl ethers are preferred. Specific examples include alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, and diethylene glycol monomethyl ether, and alkylene glycol dialkyl ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, and diethylene glycol diethyl ether.
[0092] Examples of the cyclic esters include cyclic esters (lactones) such as β-propiolactone, γ-butyrolactone, δ-valerolactone, ε-caprolactone, and β-butyrolactone, and compounds in which the hydrogen atoms of the methylene groups adjacent to the carbonyl groups thereof are substituted with alkyl groups having 1 to 4 carbon atoms.
[0093] Examples of the alkoxyalkylamides include 3-methoxy-N,N-dimethylpropionamide, 3-methoxy-N,N-diethylpropionamide, 3-methoxy-N,N-methylethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-diethylpropionamide, 3-ethoxy-N,N-methylethylpropionamide, 3-n-butoxy-N,N-dimethylpropionamide, 3-n-butoxy-N,N-diethylpropionamide, and 3-n-butoxy-N,N-methylethylpropionamide.
[0094] Examples of the cyclic amides include lactams, such as pyrrolidones such as 2-pyrrolidone, 1-methyl-2-pyrrolidone, 1-ethyl-2-pyrrolidone, 1-propyl-2-pyrrolidone and 1-butyl-2-pyrrolidone.
[0095] As the alkoxyalkylamides, compounds represented by the following general formula (1) are also preferably used.
[0096] R 1 -O-CH2CH2-(C=O)-NR 2 R 3 ……(1)
[0097] In the above formula (1), R 1 represents an alkyl group having 1 to 4 carbon atoms, R 2 and R 3 Each independently represents a methyl group or an ethyl group. The "alkyl group having a carbon number of 1 or more and 4 or less" can be a linear or branched alkyl group, for example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an isobutyl group, or a tert-butyl group. The compound represented by the above formula (1) can be used alone or in combination of two or more.
[0098] Examples of the polyhydric alcohol include 1,2-alkanediols (e.g., ethylene glycol, propylene glycol (also known as propane-1,2-diol), 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,2-heptanediol, 1,2-octanediol and other alkanediols), polyhydric alcohols other than 1,2-alkanediol (polyhydric alcohols) (e.g., diethylene glycol, dipropylene glycol, 1,3-propanediol, 1,3-butanediol (also known as 1,3-butylene glycol) , 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 2-ethyl-1,3-hexanediol, 3-methyl-1,5-pentanediol, 2-methylpentane-2,4-diol, trimethylolpropane, glycerol, etc.) and the like.
[0099] Examples of polyhydric alcohols include alkanediols and polyols. Alkanediols are diols of alkanes having 5 or more carbon atoms. The carbon number of the alkane is preferably 5 to 15, more preferably 6 to 10, and even more preferably 6 to 8. 1,2-alkanediol is preferred.
[0100] The polyol is an intermolecular condensate between hydroxyl groups of a polyol of an alkane having 4 or less carbon atoms or a polyol of an alkane having 4 or less carbon atoms. The carbon number of the alkane is preferably 2 to 3. The number of hydroxyl groups in the molecule of the polyol is 2 or more, preferably 5 or less, and more preferably 3 or less. When the polyol is the above-mentioned intermolecular condensate, the number of intermolecular condensation is 2 or more, preferably 4 or less, and more preferably 3 or less. The polyhydric alcohols can be used alone or in combination of two or more.
[0101] Alkanediols and polyols can function mainly as penetrating solvents and / or moisturizing solvents. However, alkanediols tend to have a strong property as penetrating solvents, and polyols tend to have a strong property as moisturizing solvents.
[0102] additive
[0103] The softening liquid composition may contain additives, and examples of the additives include pH adjusters, sugars, chelating agents, preservatives / antifungal agents, rust inhibitors, and others.
[0104] The pH adjuster is not particularly limited, and an appropriate combination of an acid, a base, a weak acid, and a weak base can be cited. Examples of acids and bases used in such a combination include: sulfuric acid, hydrochloric acid, nitric acid, etc. as inorganic acids; lithium hydroxide, sodium hydroxide, potassium hydroxide, potassium dihydrogen phosphate, disodium hydrogen phosphate, potassium carbonate, sodium carbonate, sodium bicarbonate, ammonia, etc. as inorganic bases; triethanolamine, diethanolamine, monoethanolamine, tripropanolamine, triisopropanolamine, diisopropanolamine, trishydroxymethylaminomethane (THAM), etc. as organic bases; adipic acid, citric acid, succinic acid, lactic acid, N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid (BES), 4-(2-hydroxyethyl)-1- Good's buffers such as piperazineethanesulfonic acid (HEPES), morpholinoethanesulfonic acid (MES), carbamoylmethyliminodiacetic acid (ADA), piperazine-1,4-bis(2-ethanesulfonic acid) (PIPES), N-(2-acetamido)-2-aminoethanesulfonic acid (ACES), N,N,N-trimethyl-2-aminoethyl) alkylammonium chloride, N-tris(hydroxymethyl)methyl-2-aminoethanesulfonic acid (TES), N-acetylamido glycine, N-tricarboxymethylglycine, glycinamide, N,N-dihydroxyethylglycine, phosphate buffer, citrate buffer, Tris buffer, etc. Furthermore, since the pH buffering effect can be obtained more stably, it is preferable to contain tertiary amines such as triethanolamine and triisopropanolamine and carboxyl-containing organic acids such as adipic acid, citric acid, succinic acid, and lactic acid as part or all of the pH adjuster.
[0105] Specific examples of sugars include glucose, mannose, fructose, ribose, xylose, arabinose, galactose, aldonic acid, glucitol (sorbitol), maltose, cellobiose, lactose, sucrose, trehalose, and maltotriose.
[0106] Examples of the chelating agent include ethylenediaminetetraacetic acid and salts thereof (eg, disodium dihydrogen ethylenediaminetetraacetate, nitrilotriacetate of ethylenediamine, hexametaphosphate, pyrophosphate, or metaphosphate).
[0107] Examples of the preservative and antifungal agent include sodium benzoate, sodium pentachlorophenol, sodium 2-pyridinethiol-1-oxide, sodium sorbate, sodium dehydroacetate, Proxel CRL, Proxel BDN, Proxel GXL, Proxel XL-2, Proxel IB and Proxel TN (all manufactured by Lonza Japan, trade names), 4-chloro-3-methylphenol (such as Preventol CMK manufactured by Bayer), and the like.
[0108] Examples of the rust inhibitor include benzotriazole, acidic sulfites, sodium thiosulfate, ammonium thioglycolate, diisopropylammonium nitrite, pentaerythritol tetranitrate, dicyclohexylammonium nitrite, and the like. Among them, benzotriazole is particularly preferred.
[0109] Examples of other additives include viscosity modifiers, antifungal agents, antioxidants, oxygen absorbers, and solubilizing agents.
[0110] In addition, in the softening liquid composition, the content of the coloring material is preferably 0.1% by mass or less relative to the total amount of the softening liquid composition. That is, the softening liquid composition is preferably used without coloring.
[0111] 1.2.1.(4) Manufacturing and physical properties
[0112] When the softening liquid composition is attached to a recording medium such as cloth by an inkjet method, its viscosity at 20°C is preferably 1.5 mPa·s to 15 mPa·s, more preferably 1.5 mPa·s to 7 mPa·s, and even more preferably 1.5 mPa·s to 5.5 mPa·s.
[0113] From the viewpoint of making the wettability and spreadability to the recording medium appropriate, the surface tension of the softening liquid composition at 25°C is 40 mN / m or less, preferably 38 mN / m or less, more preferably 35 mN / m or less, and further preferably 30 mN / m or less. In addition, the surface tension is preferably 20 mN / m or more, more preferably 25 mN / m or more.
[0114] The surface tension can be measured by using an automatic surface tensiometer CBVP-Z (manufactured by Kyowa Interface Science Co., Ltd.) and confirming the surface tension when a platinum plate is wetted with the composition in an environment of 25°C.
[0115] The softening liquid composition is obtained by mixing the above-mentioned components in an arbitrary order and filtering as needed to remove impurities. As a mixing method of the components, it is preferred to use a method in which the materials are sequentially added to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed. As a filtering method, centrifugal filtration, filter filtration, etc. can be performed as needed.
[0116] The shear hardness of the softening liquid composition is preferably smaller than the shear hardness of the coating liquid composition described below. This can improve the color development, bleeding, yellowing, and abrasion resistance (drying) of the recorded material.
[0117] 1.2.2. Attachment method
[0118] The softening liquid attaching step is performed by an inkjet method or a spray method. As a method for attaching the softening liquid to the recording medium, any one of an inkjet method and a method of applying the softening liquid to the recording medium using various sprayers or a method combining these methods can be used.
[0119] The softening liquid attaching step and the coating liquid attaching step described later may be performed either first or simultaneously on a predetermined area of the recording medium. For example, when the softening liquid attaching step is performed by an inkjet method, the softening liquid attaching step may be performed by the same scan as the coating liquid attaching step, or may be performed by a main scan different from the main scan of the softening liquid attaching step. In addition, when the softening liquid attaching step is performed by the same scan as the coating liquid attaching step, either the softening liquid composition or the coating liquid composition may be landed on the recording medium first.
[0120] As a method of simultaneously performing the softening liquid attaching step and the coating liquid attaching step described below, there is a method of attaching the coating liquid composition to the same scan area by the same scan as the scan for attaching the softening liquid composition to the recording medium.
[0121] The softening liquid attachment step is more preferably performed by an inkjet method. In this case, the viscosity at 20° C. is preferably set to 1.5 mPa·s to 15 mPa·s, more preferably 1.5 mPa·s to 7 mPa·s, and further preferably 1.5 mPa·s to 5.5 mPa·s. When the softening liquid is attached to the recording medium by an inkjet method, it is easy to efficiently form a predetermined softening liquid attachment area on the recording medium.
[0122] The amount of the softening liquid composition deposited in the softening liquid depositing step is preferably 5 g / m 2 Above 100g / m 2 Below, more preferably 15g / m 2 Above 80g / m 2 Below, more preferably 15g / m 2 Above 50g / m 2 In this way, the seepage of the softening liquid can be further suppressed. In addition, since the necessary minimum coating can be performed, the original water absorption and feel of the recording medium can be well maintained. Moreover, a colored image with good color development can be obtained.
[0123] The above-mentioned amount of the softening liquid composition is the amount of the softening liquid and the coating liquid composition in the recording area where the softening liquid and the coating liquid composition are overlapped and attached in the recording method of this embodiment. In addition, the maximum amount of the softening liquid composition in the area can also be set to the above range, which is more preferred.
[0124] 1.3. Coating liquid adhesion process
[0125] In the coating liquid attachment step, a coating liquid composition containing anionic resin particles and water is attached to a recording medium.
[0126] 1.3.1. Coating liquid composition
[0127] The coating liquid composition contains anionic resin particles and water, and the content of the anionic resin particles is 80% by mass or more relative to the total amount of nonvolatile components in the coating liquid composition.
[0128] 1.3.1.(1) Anionic resin particles
[0129] The coating liquid composition contains anionic resin particles. The resin particles can improve the adhesion of the image formed by the composition attached to the cloth. As anionic resin particles, for example, resin particles with anionicity made of urethane resins, acrylic resins (including styrene acrylic resins), fluorene resins, polyolefin resins, rosin-modified resins, terpene resins, polyester resins, polyamide resins, epoxy resins, vinyl chloride resins, vinyl chloride-vinyl acetate copolymers, ethylene vinyl acetate resins, silicone-acrylic resins, etc. can be cited. Among them, urethane resins, silicone-acrylic resins, acrylic resins, polyolefin resins, and polyester resins are preferred. Most of these resin particles are processed in the form of emulsions, but they can also be in the form of powders. In addition, the resin particles can be used alone or in combination of two or more.
[0130] Urethane resin is a general term for resins having urethane bonds. Examples of urethane resins include polyether urethane resins having ether bonds in the main chain, polyester urethane resins having ester bonds in the main chain, and polycarbonate urethane resins having carbonate bonds in the main chain. In addition, as the urethane resin, commercially available products can be used, for example, Superflex 460, 460s, 840, E-4000 (trade names, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.); Resamine D-1060, D-2020, D-4080, D-4200, D-6300, D-6455 (trade names, manufactured by Dainichi Seika Industries, Ltd.); Takelac WS-6021, W-512-A-6 (trade names, manufactured by Mitsui Chemicals Polyurethanes, Ltd.); Sancure 2710 (trade name, manufactured by LUBRIZOL); Permarin UA-150 (trade name, manufactured by Sanyo Chemical Industries, Ltd.); ETERNACOLL UW series such as UW-1527 (manufactured by Ube Industries, Ltd.) and other commercial products can also be used.
[0131] Acrylic resin is a general term for polymers obtained by polymerizing at least acrylic monomers such as (meth)acrylic acid and (meth)acrylate as one component, and examples thereof include resins obtained from acrylic monomers, copolymers of acrylic monomers and other monomers, etc. For example, acrylic-vinyl resins, which are copolymers of acrylic monomers and vinyl monomers, etc., can be mentioned. In addition, for example, as vinyl monomers, styrene, etc. can be mentioned.
[0132] As the acrylic monomer, acrylamide, acrylonitrile, etc. can also be used. The resin emulsion using acrylic resin as a raw material can use a commercial product, and can also be selected from, for example, FK-854 (trade name, manufactured by Chuo Rika Kogyo Co., Ltd.), Mowinyl 952B, 718A, 6760 (trade name, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), Nipol LX852, LX874 (trade name, manufactured by Nippon Zeon Co., Ltd.), etc.
[0133] In the present specification, the acrylic resin may be a styrene acrylic resin described below. In the present specification, the term "(meth)acrylic group" means at least one of an acrylic group and a methacrylic group.
[0134] Styrene acrylic resins are copolymers obtained from styrene monomers and (meth)acrylic monomers, and examples thereof include styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylate copolymers, styrene-α-methylstyrene-acrylic acid copolymers, and styrene-α-methylstyrene-acrylic acid-acrylate copolymers. As the styrene-acrylic resin, commercially available products can be used, for example, Joncryl 62J, 7100, 390, 711, 511, 7001, 632, 741, 450, 840, 74J, HRC-1645J, 734, 852, 7600, 775, 537J, 1535, PDX-7630A, 352J, 352D, PDX-7145, 538J, 7640, 7641, 631, 790, 780, 7610 (trade names, manufactured by BASF), Mowinyl 966A, 975N (trade names, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), Vinyblan 2586 (manufactured by Nissin Chemical Industry Co., Ltd.), etc. can be used.
[0135] As the silicone-acrylic copolymer resin, a commercially available product can be used. For example, FE-230N, FE-502, E-370, RU-911, R-170, R170S, LC-190, R-170BX of CHALINE series of Nissin Chemical Industry; SYMAX US-380, SYMAX US-450, SYMAX US-480 of Toagosei Co., Ltd.; IE-7170, SE1980CLEAR, BY22-826EX, propyleneoxy LON-MF-40 of Dow Corning Toray Co., Ltd.; LexanEXL of SABIC Innovative Plastics Japan Co., Ltd.; TARFLON NEO of Idemitsu Kosan Co., Ltd.; Vanstar S-806 of Siden Chemical Co., Ltd.; Mowinyl of Nippon Gosei Co., Ltd.; COATAX of Toray Industries, Ltd.; Daitosol 5000SJ of Daito Kasei Kogyo Co., Ltd.; "Yodosol GH41"; Shin-Etsu Chemical Co., Ltd.'s acrylate / ethylhexyl acrylate / dimethylsiloxane methacrylate copolymer (trade name: KP578); DIC Corporation's Voncoat and Ceranate; JSR's acrylic silicone emulsions "SIFCLEAR S101" and "SIFCLEAR S102", etc.
[0136] Polyolefin resin is the resin with olefins such as ethylene, propylene, butene in the structural skeleton, and well-known resin can be appropriately selected to use. As olefin resin, commercially available products can be used, such as ArrowBaseCB-1200, CD-1200 (trade name, Japan Unitika Co., Ltd. system) etc. can be used.
[0137] In addition, the resin particles can be provided in the form of an emulsion. Examples of commercially available products of such resin emulsions include Microgel E-1002 and E-5002 (trade names manufactured by Japan Paint Co., Ltd., styrene acrylic resin emulsions); Voncoat 4001 (trade name manufactured by DIC Co., Ltd., acrylic resin emulsion); Voncoat 5454 (trade name manufactured by DIC Co., Ltd., styrene-acrylic resin emulsion); Polysol AM-710, AM-920, AM-2300, AP-4735, AT-860, PSASE-4210E (acrylic resin emulsions); Polysol AP-7020 (styrene acrylic resin emulsion); Polysol SH-502 (vinyl acetate resin emulsion); Polysol AD-13, AD-2, AD-10, AD-96, AD-17, AD-70 (ethylene-vinyl acetate resin emulsions); Polysol PSASE-6010 (ethylene-vinyl acetate resin emulsion) (trade name of Showa Denko Co., Ltd.); Polysol SAE1014 (trade name, styrene-acrylic resin emulsion, manufactured by Nippon Zeon Co., Ltd.), Saivinol SK-200 (trade name, acrylic resin emulsion, manufactured by Saiden Chemical Co., Ltd.), AE-120A (trade name, acrylic resin emulsion manufactured by JSR Co., Ltd.), AE373D (trade name, carboxyl-modified styrene acrylic resin emulsion manufactured by E-TEC Co., Ltd.), Seikadyne 1900W (trade name, ethylene-vinyl acetate resin emulsion manufactured by Dainichi Seika Industries Co., Ltd.), Vinyblan 2682 (acrylic resin emulsion), Vinyblan 2886 (vinyl acetate-acrylic resin emulsion), Vinyblan 5202 (acetic acid acrylic resin emulsion) (trade name of Nissin Chemical Industry Co., Ltd.); Elitel KA-5071S, KT-8803, KT-9204, KT-8701, KT-8904, KT-0507 (trade names of Unitika Co., Ltd., polyester resin emulsion); HYTEC SN-2002 (trade name of Toho Chemical Co., Ltd., polyester resin emulsion); Takelac W-6020, W-635, W-6061, W-605, W-635, W-6021, W-5100 (trade names of Mitsui Chemicals Polyurethane Co., Ltd., urethane resin emulsion); Superflex 870, 800, 150, 420, 460, 470, 610, 700 (trade names of Dai-ichi Kogyo Seiyaku Co., Ltd., urethane resin emulsion); Permarin UA-150 (manufactured by Sanyo Chemical Industries, Ltd., urethane resin emulsion); Sancure 2710 (manufactured by Lubrizol Japan, urethane resin emulsion);NeoRez R-9660, R-9637, R-940 (made by Kusumoto Chemical Co., Ltd., urethane resin emulsion); AdekaBonTighter HUX-380, 290K (manufactured by ADEKA Co., Ltd., urethane resin emulsion); Mowinyl 966A, Mowinyl 7320 (manufactured by Nippon Synthetic Chemical Co., Ltd.); Joncryl 7100, 390, 711, 511, 7001, 632, 741, 450, 840, 74J, HRC-1645J, 734, 852, 7600, 775, 537J, 1535, PDX-7306A, 352J, 352D, PDX-7145, 538J, 7640, 7641, 631, 790, 780, 7610 (all manufactured by BASF); NK Binder R-5HN (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.); Hydran WLS-210 (non-crosslinking polyurethane: manufactured by DIC Corporation); Joncryl 7610 (manufactured by BASF Corporation) and the like can be selected for use.
[0138] The content of the resin particles in the coating liquid composition is 80% by mass or more relative to the total amount of nonvolatile components. The content of the resin particles in the coating liquid composition is more preferably 83% by mass or more relative to the total amount of nonvolatile components, and further preferably 90% by mass or more.
[0139] 1.3.1.(2) Water
[0140] The coating liquid composition contains water. As for water, since the composition and content thereof are the same as those of the softening liquid composition described above, the description thereof will be omitted.
[0141] 1.3.1.(3) Other ingredients
[0142] The coating liquid composition may contain, in addition to the anionic resin particles and water, a water-soluble resin, a humectant, other solvents, additives, a surfactant, etc. The water-soluble resin, humectant, other solvents, and additives are the same as those of the above-mentioned softener composition, and thus their description is omitted.
[0143] Surfactants
[0144] The coating liquid composition may contain a surfactant. The surfactant has a function of adjusting the surface tension of the composition, for example, adjusting wettability with a fabric, etc. Among the surfactants, for example, acetylene glycol-based surfactants, silicone-based surfactants, and fluorine-based surfactants can be preferably used.
[0145] The acetylene glycol surfactant is not particularly limited, and examples thereof include Surfynol 104, 104E, 104H, 104A, 104BC, 104DPM, 104PA, 104PG-50, 104S, 420, 440, 465, 485, SE, SE-F, 504, 61, DF37, CT111, CT121, CT131, CT136, TG, GA, and DF110D (all of the above are trade names, manufactured by Air Products and Chemicals Inc.); Olfine B, Y, P, A, STG, SPC, E1004, E1010, PD-001, PD-002W, PD-003, PD-004, EXP.4001, EXP.4036, EXP.4051, AF-103, AF-104, AK-02, SK-14, AE-3 (all of the above are trade names, manufactured by Nissin Chemical Industry Co., Ltd.); Acetylenol E00, E00P, E40, E100 (all of the above are trade names, manufactured by Kawakami Fine Chemical Co., Ltd.).
[0146] The silicone surfactant is not particularly limited, but preferably a polysiloxane compound is used. The polysiloxane compound is not particularly limited, and examples thereof include polyether-modified organic siloxanes. Commercially available products of the polyether-modified organic siloxanes include, for example, BYK-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, BYK-348 (the above are trade names, manufactured by BYK-Chemie Japan Co., Ltd.); KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-61 5A, KF-945, KF-640, KF-642, KF-643, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, KF-6017 (the above are trade names, manufactured by Shin-Etsu Chemical Co., Ltd.); Silface SAG002, 005, 503A, 008 (the above are trade names, manufactured by Nissin Chemical Co., Ltd.), etc.
[0147] As the fluorine-based surfactant, a fluorine-modified polymer is preferably used. Specific examples include BYK-3440 (manufactured by BYK-Chemie Japan Co., Ltd.), Surflon S-241, S-242, S-243 (these are trade names, manufactured by AGC Seimichemical Co., Ltd.), and Ftergent 215M (manufactured by Neos Co., Ltd.).
[0148] When the coating liquid composition contains a surfactant, it may contain multiple surfactants. The content of the surfactant contained in the coating liquid composition can be set to 0.1% by mass or more and 2% by mass or less relative to the total mass of the coating liquid composition, preferably 0.3% by mass or more and 1.5% by mass or less, and more preferably 0.4% by mass or more and 1.0% by mass or less.
[0149] In the coating liquid composition, the content of the colorant is preferably 0.1% by mass or less relative to the total amount of the coating liquid composition. That is, the coating liquid composition is preferably used without coloring.
[0150] 1.3.1.(4) Manufacturing and physical properties
[0151] In order to attach the coating liquid composition to a recording medium such as cloth by an inkjet method, its viscosity at 20°C is preferably 1.5 mPa·s to 15 mPa·s, more preferably 1.5 mPa·s to 7 mPa·s, and even more preferably 1.5 mPa·s to 5.5 mPa·s.
[0152] From the viewpoint of making the wettability and spreadability to the recording medium appropriate, the surface tension of the coating liquid composition at 25° C. is 40 mN / m or less, preferably 38 mN / m or less, more preferably 35 mN / m or less, and further preferably 30 mN / m or less. In addition, the surface tension is preferably 20 mN / m or more, more preferably 25 mN / m or more.
[0153] The coating liquid composition is obtained by mixing the above-mentioned components in an arbitrary order and filtering as needed to remove impurities. As a mixing method for each component, it is preferred to use a method in which materials are sequentially added to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed. As a filtering method, centrifugal filtration, filter filtration, etc. can be performed as needed.
[0154] Furthermore, the shear hardness of the coating liquid composition is more preferably greater than the shear hardness of the softening liquid composition. This can improve the abrasion resistance (drying) of the recorded object.
[0155] 1.3.2. Attachment method
[0156] The coating liquid attaching process is performed by an inkjet method. The coating liquid attaching process and the softening liquid attaching process may be performed either first or simultaneously on a predetermined area of the recording medium. For example, when the softening liquid attaching process is performed by an inkjet method, the softening liquid attaching process may be performed by the same scan as the coating liquid attaching process, or may be performed by a main scan different from the main scan of the softening liquid attaching process. In addition, when the softening liquid attaching process is performed by the same scan as the coating liquid attaching process, either the softening liquid composition or the coating liquid composition may be landed on the recording medium first.
[0157] The coating liquid composition adhesion amount in the coating liquid adhesion step is preferably 15 g / m 2 Above 80g / m 2 Below, more preferably 30g / m 2 Above 60g / m 2 Below, more preferably 30g / m 2 Above 50g / m 2 As a result, the bleeding of the coating liquid can be further suppressed. In addition, the coating can be applied to the minimum extent necessary, so the original water absorption and feel of the recording medium can be well maintained. Moreover, a colored image with good color development can be obtained.
[0158] Furthermore, in the adhesion area of the recording medium, the ratio of the adhesion amount of the softening liquid to the adhesion amount of the coating liquid composition is more preferably 0.25 or more and 1 or less. This can further reduce the bleeding of the softening liquid.
[0159] In addition, if a metal salt is used in the reaction liquid composition described later to increase the cationicity, an anionic resin is used in the ink composition described later to increase the anionicity, and a cationic silicone is used in the softening liquid composition to increase the cationicity, the mutual aggregation reaction is promoted, so that a structure that is more difficult to bleed can be formed.
[0160] Furthermore, the area on the recording medium coated with the coating liquid composition in the coating liquid attachment step is preferably larger than the area on the recording medium coated with the softening liquid composition in the above-mentioned softening liquid attachment step. In this way, the coating area of the coating liquid is wider than the coating area of the softening liquid, so the bleeding of the softening liquid can be further suppressed.
[0161] 1.4. Other processes
[0162] The recording method of this embodiment may further include: an ink attaching step of attaching an ink composition containing a pigment and water to a recording medium by an inkjet method; and a reaction liquid attaching step of attaching a reaction liquid composition containing a coagulant for aggregating the components of the ink composition and water to a recording medium by an inkjet method. In addition, the recording method of this embodiment may also include a drying step.
[0163] 1.4.1. Ink adhesion process
[0164] The recording method of the present embodiment may include an ink attaching step of attaching an ink composition containing a pigment and water to a recording medium by an inkjet method.
[0165] 1.4.1.(1) Ink composition
[0166] The ink composition contains at least a pigment and water. The ink composition is a so-called pigment color ink containing a pigment. The pigment contained in the ink composition may be, for example, a color pigment such as cyan, yellow, magenta, black, or a special pigment such as white or pearlescent.
[0167] The pigment may be a mixture. The pigment is excellent in storage stability such as light resistance, weather resistance, and gas resistance, and from this viewpoint, an organic pigment is preferred.
[0168] Specifically, the pigment can use azo pigments such as insoluble azo pigments, condensed azo pigments, azo lakes, chelated azo pigments, phthalocyanine pigments, perylene and perinone pigments, anthraquinone pigments, quinacridone pigments, dioxane pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments and other polycyclic pigments, dye chelates, dyeing lakes, nitro pigments, nitroso pigments, aniline black, daylight fluorescent pigments, carbon black, etc. The above-mentioned pigments can be used alone or in combination of two or more. Further, as the pigment, white pigments, bright pigments, etc. can also be used.
[0169] Specific examples of the pigment are not particularly limited, and examples thereof include the following pigments.
[0170] Examples of the black pigment include No. 2300, No. 900, MCF88, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, and No. 2200B (all manufactured by Mitsubishi Chemical Corporation); Raven 5750, Raven 5250, Raven 5000, Raven 3500, Raven 1255, and Raven 700 (all manufactured by Carbon Columbia Corporation); Regal 400R, Regal 330R, Regal 660R, Mogul L, Monarch 700, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, and Monarch 1400 (all manufactured by CABOT JAPAN Corporation); Pigment Black FW1, Pigment Black FW2, Pigment Black FW2V, Pigment Black FW18, Pigment Black FW200, Pigment Black S150, Pigment Black S160, Pigment Black S170, Printex 35, Printex U, Printex V, Printex 140U, Extra Black 6, Extra Black 5, Extra Black 4A, Extra Black 4 (all manufactured by Degussa).
[0171] Examples of the yellow pigment include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 151, 153, 154, 167, 172, and 180.
[0172] Examples of the magenta pigment include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48 (Ca), 48 (Mn), 57 (Ca), 57:1, 88, 112, 114, 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, and 245; and CI Pigment Violet 19, 23, 32, 33, 36, 38, 43, and 50.
[0173] Examples of the cyan pigment include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:34, 15:4, 16, 18, 22, 25, 60, 65, and 66; and CI Vat Blue 4 and 60.
[0174] Pigments other than magenta, cyan, and yellow are not particularly limited, and examples thereof include CI Pigment Green 7, 10, CI Pigment Brown 3, 5, 25, 26, and CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43, and 63.
[0175] The pearlescent pigment is not particularly limited, and examples thereof include pigments having pearl luster or interference luster, such as titanium dioxide-coated mica, fish scale foil, and bismuth oxychloride.
[0176] The metal pigment is not particularly limited, and examples thereof include particles composed of a single substance or an alloy of aluminum, silver, gold, platinum, nickel, chromium, tin, zinc, indium, titanium, copper, and the like.
[0177] As white pigment, for example, metal compounds such as metal oxide, barium sulfate, calcium carbonate can be mentioned. As metal oxide, for example, titanium dioxide, zinc oxide, silicon dioxide, aluminum oxide, magnesium oxide etc. can be mentioned. In addition, white pigment can also use particles with hollow structure, and as particles with hollow structure, known particles can be used.
[0178] The pigment is preferably capable of being stably dispersed in a dispersion medium, and for this purpose, a dispersant may be used to disperse the pigment. Examples of the dispersant include resin dispersants, which are selected from dispersants that can provide good dispersion stability of the pigment in the ink composition. In addition, the pigment may be used as a self-dispersible pigment by oxidizing or sulfonating the surface of the pigment particles, for example, with ozone, hypochlorous acid, fuming sulfuric acid, etc., to modify the surface of the pigment particles.
[0179] Examples of the resin dispersant (dispersant resin) include (meth)acrylic acid resins and salts thereof such as poly(meth)acrylic acid, (meth)acrylic acid-acrylonitrile copolymers, (meth)acrylic acid-(meth)acrylic ester copolymers, vinyl acetate-(meth)acrylic ester copolymers, vinyl acetate-(meth)acrylic acid copolymers, and vinylnaphthalene-(meth)acrylic acid copolymers; styrene resins and salts thereof such as styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic ester copolymers, styrene-α-methylstyrene-(meth)acrylic acid copolymers, styrene-α-methylstyrene-(meth)acrylic acid-(meth)acrylic ester copolymers, styrene-maleic acid copolymers, and styrene-maleic anhydride copolymers; urethane resins and salts thereof, which are polymer compounds (resins) containing urethane bonds formed by the reaction of an isocyanate group and a hydroxyl group, and may be linear and / or branched, regardless of the presence or absence of a cross-linked structure; polyvinyl alcohols; vinylnaphthalene-maleic acid copolymers and salts thereof; vinyl acetate-maleic acid ester copolymers and salts thereof; and water-soluble resins such as vinyl acetate-crotonic acid copolymers and salts thereof. Among them, copolymers of monomers having hydrophobic functional groups and monomers having hydrophilic functional groups, and polymers composed of monomers having both hydrophobic functional groups and hydrophilic functional groups are preferred. As the form of the copolymer, any form among random copolymers, block copolymers, alternating copolymers, and graft copolymers can be used.
[0180] Commercially available products of styrene-based resin dispersants include, for example, X-200, X-1, X-205, X-220, and X-228 (manufactured by Seikyo PMC Co., Ltd.); Nopcosperse (registered trademark) 6100 and 6110 (manufactured by SanNopco Co., Ltd.); Joncryl 67, 586, 611, 678, 680, 682, and 819 (manufactured by BASF); DISPERBYK-190 (manufactured by BYK-Chemie Japan Co., Ltd.); N-EA137, N-EA157, N-EA167, N-EA177, N-EA197D, N-EA207D, and E-EN10 (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.);
[0181] Examples of commercially available acrylic resin dispersants include BYK-187, BYK-190, BYK-191, BYK-194N, and BYK-199 (manufactured by BYK-Chemie Co., Ltd.); Aron A-210, A6114, AS-1100, AS-1800, A-30SL, A-7250, and CL-2 (manufactured by Toagosei Co., Ltd.).
[0182] Further, commercially available products of the urethane resin dispersant include BYK-182, BYK-183, BYK-184, BYK-185 (manufactured by BYK-Chemie Co., Ltd.), TEGO Disperse 710 (manufactured by Evonic Tego Chemi Co., Ltd.), and Borchi (registered trademark) Gen 1350 (manufactured by OMG Borschers Co., Ltd.).
[0183] Dispersant can be used alone or in combination. The total content of the dispersant is preferably 0.1 mass part or less than 30 mass parts relative to 50 mass parts of pigment, more preferably 0.5 mass part or less than 25 mass parts, further more preferably 1 mass part or less than 20 mass parts, and further preferably 1.5 mass parts or less than 15 mass parts. By making the content of the dispersant more than 0.1 mass part relative to 50 mass parts of pigment, the dispersion stability of the pigment can be further improved. In addition, if the content of the dispersant is less than 30 mass parts relative to 50 mass parts of pigment, the viscosity of the resulting dispersion can be suppressed to be smaller.
[0184] By using such a resin dispersant as a dispersant, the dispersion and aggregation of the pigment become better, and better dispersion stability and a better quality image can be obtained.
[0185] The dispersant resin preferably has an acid value of preferably 5 mgKOH / g or more, more preferably 10 to 200 mgKOH / g, further preferably 15 to 150 mgKOH / g, further preferably 20 to 100 mgKOH / g, further preferably 25 to 70 mgKOH / g.
[0186] The acid value can be measured by neutralization potentiometric titration in accordance with JIS K0070. As a titration apparatus, for example, "AT610" manufactured by Kyoto Denshi Kogyo Co., Ltd. can be used.
[0187] The content of the pigment is preferably 0.3% to 20% by mass, more preferably 0.5% to 15% by mass, relative to the total mass of the ink composition. Further, it is preferably 1% to 10% by mass, more preferably 2% to 7% by mass.
[0188] The ink composition may contain, in addition to the pigment and water, resin particles, a moisturizer, a solvent, a surfactant, an additive, etc. These substances are the same as those already described, and thus description thereof will be omitted.
[0189] 1.4.1.(2) Manufacturing and physical properties
[0190] In order to attach the ink composition to a recording medium such as cloth by an inkjet method, the viscosity of the ink composition at 20°C is preferably 1.5 mPa·s to 15 mPa·s, more preferably 1.5 mPa·s to 7 mPa·s, and even more preferably 1.5 mPa·s to 5.5 mPa·s.
[0191] From the viewpoint of achieving appropriate wetting and spreading properties on the recording medium, the surface tension of the ink composition at 25° C. is 40 mN / m or less, preferably 38 mN / m or less, more preferably 35 mN / m or less, and further preferably 30 mN / m or less. In addition, the surface tension is preferably 20 mN / m or more, and more preferably 25 mN / m or more.
[0192] The ink composition is obtained by mixing the above-mentioned components in an arbitrary order and filtering or the like as needed to remove impurities. As a method for mixing the components, it is preferable to use a method in which the materials are sequentially added to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed. As a filtering method, centrifugal filtration, filter filtration, etc. can be performed as needed.
[0193] 1.4.1.(3) Attachment method
[0194] The ink attaching step is performed by an inkjet method. The ink attaching step, the coating liquid attaching step, and the softening liquid attaching step may be performed one by one on a predetermined area of the recording medium, or may be performed simultaneously.
[0195] The amount of ink composition deposited in the ink depositing step is preferably 15 g / m 2 Above 120g / m 2 Below, more preferably 30g / m 2 Above 80g / m 2 Below, more preferably 30g / m 2 Above 60g / m 2 the following.
[0196] 1.4.2. Reaction solution adhesion step
[0197] The recording method of the present embodiment may include a reaction liquid attaching step of attaching a reaction liquid composition containing a coagulant for aggregating the components of the ink composition and water to a recording medium by an inkjet method.
[0198] 1.4.2.(1) Reaction solution composition
[0199] The reaction liquid contains at least a coagulant for aggregating the components of the ink composition and water. The coagulant has the function of aggregating the pigment and the resin particles by reacting with the components such as the pigment contained in the ink composition and the resin particles that may be contained in the ink composition. By such aggregating, for example, the color development of the pigment can be improved, the fixability of the resin particles can be improved, and / or the viscosity of the ink can be increased.
[0200] The coagulant is not particularly limited, and metal salts, inorganic acids, organic acids, cationic compounds, etc. can be cited. As the cationic compound, cationic resins (cationic polymers), cationic surfactants, etc. can be used. Among them, as the metal salt, a polyvalent metal salt is preferred, and as the cationic compound, a cationic resin is preferred. Therefore, as the coagulant, it is preferably selected from cationic resins, organic acids, and polyvalent metal salts in terms of particularly excellent image quality, abrasion resistance, gloss, etc.
[0201] As the metal salt, a polyvalent metal salt is preferred, but metal salts other than polyvalent metal salts may also be used. Among these coagulants, at least one selected from metal salts and organic acids is preferably used because of its excellent reactivity with the components contained in the ink. In addition, among cationic compounds, cationic resins are preferably used because they are easily soluble in softening liquid. In addition, multiple coagulants may be used simultaneously.
[0202] The polyvalent metal salt refers to a compound composed of a divalent or higher metal ion and an anion. Examples of divalent or higher metal ions include ions of calcium, magnesium, copper, nickel, zinc, barium, aluminum, titanium, strontium, chromium, cobalt, and iron. Among the metal ions constituting the polyvalent metal salt, at least one of calcium ions and magnesium ions is preferred from the perspective of excellent cohesion of the components of the ink.
[0203] Anions constituting the polyvalent metal salt are inorganic ions or organic ions. That is, the polyvalent metal salt in the present invention refers to a salt consisting of an inorganic ion or an organic ion and a polyvalent metal. Examples of such inorganic ions include chloride ions, bromide ions, iodide ions, nitrate ions, sulfate ions, hydroxide ions, and the like. Examples of organic ions include organic acid ions, such as carboxylic acid ions.
[0204] In addition, the polyvalent metal compound is preferably an ionic polyvalent metal salt, and the stability of the softening liquid is better when the polyvalent metal salt is a magnesium salt or a calcium salt. In addition, the counter ion of the polyvalent metal may be any one of an inorganic acid ion and an organic acid ion.
[0205] As the specific example of the above-mentioned polyvalent metal salt, calcium carbonate, calcium nitrate, calcium chloride, calcium sulfate, magnesium sulfate, calcium hydroxide, magnesium chloride, magnesium carbonate, barium sulfate, barium chloride, zinc carbonate, zinc sulfide, aluminum silicate, calcium silicate, magnesium silicate, copper nitrate, calcium formate, calcium acetate, magnesium acetate, aluminum acetate, etc. such as heavy calcium carbonate and light calcium carbonate can be enumerated. One of these polyvalent metal salts can be used alone, and two or more can be used simultaneously. Wherein, owing to can ensure sufficient solubility to water and the trace residue caused by the softening liquid is reduced (the trace becomes inconspicuous), therefore, at least any one of calcium formate, magnesium sulfate, calcium nitrate and calcium chloride is preferred, and calcium formate and calcium nitrate are more preferred. In addition, these metal salts can also have hydration water under the raw material form.
[0206] Examples of the metal salt other than the polyvalent metal salt include monovalent metal salts such as sodium salts and potassium salts, and examples thereof include sodium sulfate and potassium sulfate.
[0207] As organic acid, for example, poly (meth) acrylic acid, acetic acid, glycolic acid, malonic acid, malic acid, maleic acid, ascorbic acid, succinic acid, glutaric acid, fumaric acid, citric acid, tartaric acid, lactic acid, sulfonic acid, orthophosphoric acid, pyrrolidonecarboxylic acid, pyranonecarboxylic acid, pyrrolecarboxylic acid, furancarboxylic acid, pyridinecarboxylic acid, coumaric acid, thiophenecarboxylic acid, nicotinic acid or derivatives of these compounds, or their salts, etc. can be preferably mentioned. One organic acid can be used alone, or two or more organic acids can be used simultaneously. The substance that is a salt of an organic acid and a metal salt is included in the above-mentioned metal salt.
[0208] Examples of the inorganic acid include sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, etc. The inorganic acid may be used alone or in combination of two or more.
[0209] Examples of the cationic resin (cationic polymer) include cationic urethane resins, cationic olefin resins, cationic amine resins, cationic surfactants, etc. The cationic polymer is preferably water-soluble.
[0210] As the cationic urethane resin, commercially available products can be used, for example, HYDRAN CP-7010, CP-7020, CP-7030, CP-7040, CP-7050, CP-7060, CP-7610 (trade names, manufactured by Dainippon Ink & Chemicals Co., Ltd.), SUPERFLEX 600, 610, 620, 630, 640, 650 (trade names, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), polyurethane emulsions WBR-2120C, WBR-2122C (trade names, manufactured by Daisei Fine Chemicals Co., Ltd.), etc. can be used.
[0211] Cationic olefin resin is a resin having olefins such as ethylene and propylene in the structural skeleton, and well-known olefin resins can be appropriately selected for use. In addition, cationic olefin resins can also be an emulsion state dispersed in a solvent including water, an organic solvent, etc. As cationic olefin resins, commercially available products can be used, for example, ArrowBase CB-1200, CD-1200 (trade name, manufactured by Japan Unitika Co., Ltd.) etc. can be cited.
[0212] As cationic amine resin (cationic polymer), as long as it has an amino group in the structure, well-known amine resins can be appropriately selected for use. For example, polyamine resins, polyamide resins, polyallylamine resins, etc. can be cited. Polyamine resins are resins having amino groups in the main skeleton of the resin. Polyamide resins are resins having amide groups in the main skeleton of the resin. Polyallylamine resins are resins having a structure derived from allyl groups in the main skeleton of the resin.
[0213] In addition, examples of cationic polyamine resins include: UNISENSE KHE103L manufactured by SENKA Corporation (hexamethylenediamine / epichlorohydrin resin, 1% aqueous solution with a pH of about 5.0, a viscosity of 20 to 50 (mPa·s), and an aqueous solution with a solid content concentration of 50% by mass), UNISENSE KHE104L (dimethylamine / epichlorohydrin resin, 1% aqueous solution with a pH of about 7.0, a viscosity of 1 to 10 (mPa·s), and an aqueous solution with a solid content concentration of 20% by mass), etc. Specific examples of commercially available cationic polyamine resins include FL-14 (manufactured by SNF), ARAFIX 100, 251S, 255, 255LOX (manufactured by Arakawa Chemical Co., Ltd.), DK-6810, 6853, 6885; WS-4010, 4011, 4020, 4024, 4027, 4030 (manufactured by Seika PMC Co., Ltd.), PAPIOGEN P-105 (manufactured by SENKA Co., Ltd.), SUMIREZRESIN 650 (30), 675A, 6615, SLX-1 (manufactured by Taoka Chemical Industry Co., Ltd.), CATIOMASTER (registered trademark) PD-1, 7, 30, A, PDT-2, PE-10, PE-30, DT-EH, EPA-SK01, TMHMDA-E (manufactured by Yokkaichi Synthetic Co., Ltd.), JETFIX 36N, 38A, 5052 (manufactured by Satoda Chemical Co., Ltd.).
[0214] As the polyamine resin, polyallylamine resin can also be mentioned. Examples of the polyallylamine resin include, for example, polyallylamine hydrochloride, polyallylamine amide sulfate, allylamine hydrochloride-diallylamine hydrochloride copolymer, allylamine acetate-diallylamine acetate copolymer, allylamine acetate-diallylamine acetate copolymer, allylamine hydrochloride-dimethylallylamine hydrochloride copolymer, allylamine-dimethylallylamine copolymer, polydiallylamine hydrochloride, polymethyldiallylamine hydrochloride, polymethyldiallylamine amide sulfate, polymethyldiallylamine acetate, polydiallyldimethylammonium chloride, diallylamine acetate-sulfur dioxide copolymer, diallylmethylethylammonium ethyl sulfate-sulfur dioxide copolymer, methyldiallylamine hydrochloride-sulfur dioxide copolymer, diallyldimethylammonium chloride-sulfur dioxide copolymer, diallyldimethylammonium chloride-acrylamide copolymer, and the like.
[0215] Examples of the cationic surfactant include primary, secondary and tertiary amine salt compounds, alkylamine salts, dialkylamine salts, aliphatic amine salts, benzalkonium salts, quaternary ammonium salts, quaternary alkylammonium salts, alkylpyridinium salts, sulfonium salts, phosphonium salts, onium salts and imidazolinium salts.
[0216] These flocculating agents can also be used in a variety of ways. In addition, among these flocculating agents, if at least one of a polyvalent metal salt, an organic acid, and a cationic resin is selected, the flocculation effect is better, and therefore a higher quality (particularly good color development) image can be formed.
[0217] The total content of the coagulants in the reaction liquid composition is not limited, and is, for example, 0.1% by mass to 15% by mass, preferably 1% by mass to 10% by mass, and more preferably 2% by mass to 10% by mass, relative to the total mass of the reaction liquid composition.
[0218] The reaction liquid composition may contain, in addition to the coagulant and water, a humectant, a solvent, a surfactant, an additive, etc. These substances are the same as those already described, and thus description thereof will be omitted.
[0219] In addition, in the reaction liquid composition, the content of the coloring material is preferably 0.1% by mass or less relative to the total amount of the reaction liquid composition. That is, the reaction liquid composition is preferably used without coloring.
[0220] 1.4.2.(2) Manufacturing and physical properties
[0221] In order to attach the reaction liquid composition to a recording medium such as cloth by an inkjet method, its viscosity at 20°C is preferably 1.5 mPa·s to 15 mPa·s, more preferably 1.5 mPa·s to 7 mPa·s, and further preferably 1.5 mPa·s to 5.5 mPa·s.
[0222] From the viewpoint of making the wettability and spreadability to the recording medium appropriate, the surface tension of the reaction liquid composition at 25° C. is 40 mN / m or less, preferably 38 mN / m or less, more preferably 35 mN / m or less, and further preferably 30 mN / m or less. In addition, the surface tension is preferably 20 mN / m or more, and more preferably 25 mN / m or more.
[0223] The reaction liquid composition is obtained by mixing the above-mentioned components in an arbitrary order and filtering as needed to remove impurities. As a mixing method for each component, it is preferred to use a method in which materials are sequentially added to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed. As a filtering method, centrifugal filtration, filter filtration, etc. can be performed as needed.
[0224] 1.4.2.(3) Attachment method
[0225] The reaction liquid attaching step is performed by an inkjet method. The reaction liquid attaching step, ink attaching step, coating liquid attaching step, and softening liquid attaching step may be performed one by one on a predetermined area of the recording medium or may be performed simultaneously.
[0226] The deposition amount of the reaction liquid composition in the reaction liquid deposition step is preferably 15 g / m 2 Above 80g / m 2 Below, more preferably 30g / m 2 Above 60g / m 2 Below, more preferably 30g / m 2 Above 50g / m 2 the following.
[0227] 1.4.2.(4) Cohesion with respect to coating liquid composition and softening liquid composition
[0228] From the viewpoint of well exerting the effect of the softening liquid composition (the feel of the recorded object), the softening liquid composition preferably does not have the cohesion caused by the coagulant in the reaction liquid composition. However, in such a case, the softening liquid composition may sometimes bleed. In contrast, the coating liquid composition preferably has the cohesion caused by the coagulant in the reaction liquid composition. The coating liquid composition can well suppress the bleeding of the softening liquid composition by having the cohesion caused by the coagulant of the reaction liquid composition.
[0229] 1.4.3. Drying process
[0230] The recording method involved in this embodiment may include a drying process between or before and after each of the above-mentioned processes. As the drying process, it can be performed by a method of drying it using a drying mechanism. As the method of drying it using a drying mechanism, there can be cited: a method of supplying air at room temperature or warm air to the recording medium (air supply method), a method of irradiating the recording medium with radiation (infrared rays, etc.) that generates heat (radiation method), a component that contacts the recording medium and transfers heat to the recording medium (conduction method), and a combination of two or more of these methods. In the case of having a drying process, it is preferably performed by a drying mechanism that heats the recording medium. In particular, the case where a drying mechanism that heats the recording medium is used as the drying mechanism is referred to as a heating process.
[0231] The surface temperature of the recording medium when each composition is attached is preferably 45°C or less, more preferably 10°C or more and 45°C or less. In addition, it is preferably 15°C or more and 40°C or less, more preferably 20°C or more and 30°C or less. This temperature is the surface temperature of the portion of the recording surface of the recording medium to which the liquid is attached during the attachment process, and is the highest temperature of the attachment process in the recording area. When the surface temperature is within the above range, it is more preferred in terms of image quality, abrasion resistance, and reduced clogging.
[0232] There is no particular limitation on the method of heating the recording medium, and examples thereof include hot pressing, normal pressure steam method, high pressure steam method, thermal fixing method, and the like. The heat source for heating is not particularly limited, and for example, an infrared lamp or the like can be used. The heating temperature is preferably a temperature at which the resin particles in the ink are melted and the medium such as water evaporates. For example, it is preferably above 100°C and below 200°C, more preferably below 170°C, and further preferably below 160°C. Here, the heating temperature in the heating process refers to the surface temperature of the image or the like formed on the cloth serving as the recording medium. The time for heating is not particularly limited, and for example, it is above 30 seconds and below 20 minutes.
[0233] In addition, it is also preferable not to have a drying step, because this may allow an image with good color development to be obtained in a shorter time.
[0234] 1.5. Process sequence
[0235] In the recording method of this embodiment, the coating liquid attachment process can be performed before the softening liquid attachment process, or can be performed simultaneously with the softening liquid attachment process. In this way, it is difficult to hinder the adhesion of the coating formed by the coating liquid composition to the recording medium (fiber), the wet friction fastness can be improved, and the color unevenness of the recorded object can be further reduced. This effect is due to the fact that the softener contained in the softening liquid composition is hydrophobic, so it is easier to produce adhesion between the coating and the recording medium (fiber) than when the softening liquid is first attached to the recording medium.
[0236] In the recording method of this embodiment, the ink attaching step and the reaction liquid attaching step may be performed before the coating liquid attaching step, or may be performed simultaneously with the softening liquid attaching step and the coating liquid attaching step. In this way, the wet friction fastness is more significantly exhibited.
[0237] Furthermore, in the recording method of this embodiment, the reaction liquid attaching step may be performed before the ink attaching step or simultaneously with the ink attaching step. In this way, an image with better color development properties can be formed.
[0238] 1.6. Effects, etc.
[0239] According to the recording method of this embodiment, by attaching the softening liquid composition to the recording medium, the softener (depending on the hydrophobicity) is attached to the fibers of the recording medium, making the molecules of the fibers easy to move, and the hardness of the fibers is relaxed (because the fibers become easy to slide and the fibers become difficult to shrink by hindering the bonding of the OH groups of the fibers in the case of natural fibers), and the feel of the recorded object can be improved. On the basis of this effect, the hydrophobic color material such as the pigment and disperse dye from the ink composition exposed to the surface of the recording medium is covered with the resin of the coating liquid, and the amount of resin in the coating liquid is also large, so that a resin film containing a strong color material can be formed. As a result, the color material is difficult to fall off, and the wet friction fastness of the recorded object can also be improved. In addition, due to the coagulant of the reaction liquid composition, the pigment in the ink composition can be coagulated, and the color development of the recorded object can also be improved.
[0240] In addition, according to the recording method of this embodiment, by attaching the softening liquid composition to the recording medium, the softener (depending on the degree of hydrophobicity) is attached to the fibers of the recording medium, making it easy for the molecules of the fibers to move, and the hardness of the fibers is relaxed (because the fibers become easy to slide against each other and in the case of natural fibers, the OH groups of the fibers are hindered from bonding with each other, making it difficult for the fibers to shrink), which can make the feel of the recorded object better.
[0241] On the other hand, because the softener is a hydrophobic material, it has a strong affinity with the hydrophobic color material. Therefore, the hydrophobic color material becomes difficult to be taken into the fixing resin on the recording medium from other compositions. Thus, the hydrophobic color material easily falls off from the recording medium, and there is a tendency for the wet friction fastness to deteriorate.
[0242] However, according to the recording method of this embodiment, by using the coating liquid at the same time, the hydrophobic color material exposed on the surface of the recording medium is covered with the resin of the coating liquid, and the amount of resin in the coating liquid is also large, so that a strong resin film can be formed. As a result, the hydrophobic color material becomes difficult to fall off, the wet friction fastness of the recorded object can be improved, and the hand feel can also be improved.
[0243] Such an effect is obtained by applying the softening liquid and the coating liquid in different attachment processes. That is, when a softener and resin particles are contained in one composition and attached to a recording medium, the softener and the resin particles are uniformly mixed in the composition and in the attached droplets, and the softener enters the resin coating film, making it difficult to form a resin network and unable to achieve good wet friction fastness. Therefore, in this recording method, by combining the softener and the resin particles in different compositions and attaching them to the recording medium separately, it is possible to suppress the softener from entering the resin coating film, thereby achieving both the feel of the recorded object and the wet friction fastness.
[0244] 2. Combination group
[0245] The composition group of this embodiment has the above-mentioned softening liquid composition and the above-mentioned coating liquid composition, the content of the softener is more than 60 mass% relative to the total amount of non-volatile components in the softening liquid composition, the content of the resin particles is more than 80 mass% relative to the total amount of non-volatile components in the coating liquid composition, the coating liquid composition is used by spraying by inkjet method, and the softening liquid composition is used by spraying by inkjet method or spray method.
[0246] According to the composition group of this embodiment, by attaching the softening liquid composition to the recording medium, the softener (depending on the degree of hydrophobicity) is attached to the fibers of the recording medium, making it easy for the molecules of the fibers to move, and the hardness of the fibers is relaxed (because the fibers become easy to slide against each other and in the case of natural fibers, the OH groups of the fibers are hindered from bonding with each other, making it difficult for the fibers to shrink), which can make the feel of the recorded material good.
[0247] In addition, according to the composition set, by using a coating liquid at the same time, the hydrophobic color material exposed on the surface of the recording medium is covered with the resin of the coating liquid, and the amount of resin in the coating liquid is also large, so that a strong resin film can be formed. As a result, the hydrophobic color material becomes difficult to fall off, the wet friction fastness of the recorded object can be improved, and the hand feel can also be improved.
[0248] 3. Example of a recording device
[0249] Reference Figure 1 An example of an inkjet printing device (recording device) including an inkjet head that can be applied to the recording method according to the present embodiment will be described.
[0250] In addition, Figure 1 In order to make each layer and each component recognizable, the size of each layer and each component is different from the actual size. Figure 1 In the figure, for convenience of explanation, the X-axis, Y-axis, and Z-axis are illustrated as three axes orthogonal to each other, the tip side of the arrow indicating the axial direction is referred to as the "+ side", and the base side is referred to as the "- side". The direction parallel to the X-axis is referred to as the "X-axis direction", the direction parallel to the Y-axis is referred to as the "Y-axis direction", and the direction parallel to the Z-axis is referred to as the "Z-axis direction".
[0251] 3.1. Overall structure
[0252] Figure 1 1 is a schematic diagram showing a schematic overall structure of the recording device 100. Figure 1 The overall structure of the recording device 100 will be described.
[0253] like Figure 1 As shown, the recording device 100 includes a medium conveying unit 20, a medium contacting unit 60, a belt supporting unit 91, a printing unit 40, a heating unit 27, a cleaning unit 50, etc. In the recording device 100, at least one of the medium contacting unit 60 and the belt supporting unit 91 corresponds to a heating unit for heating the endless belt 23. In addition, the recording device 100 includes a control unit 1 for controlling these units. Each unit of the recording device 100 is mounted on the frame unit 90.
[0254] Furthermore, when a heating unit for heating the endless belt is provided, it only needs to be located upstream of the printing unit 40 in the conveying direction, and may be provided at a position different from the medium close contact unit 60 and the belt support unit 91. For example, the heating unit may be located upstream of the medium close contact unit 60 in the conveying direction. With such a structure, the heating unit can also dry the endless belt 23 that is wetted during washing. In addition, the heating unit may heat the endless belt in a non-contact manner.
[0255] The medium conveying unit 20 conveys the fabric 95 in a conveying direction and includes a medium supply unit 10 , conveying rollers 21 , 22 , an endless belt 23 , a belt rotating roller 24 , a belt driving roller 25 as a driving roller, conveying rollers 26 , 28 , and a medium collecting unit 30 .
[0256] 3.2. Medium conveying unit
[0257] First, the conveyance path of the cloth 95 from the medium supply unit 10 to the medium recovery unit 30 will be described. Figure 1 In the figure, the direction along the direction of gravity is defined as the Z-axis direction, the direction in which the cloth 95 is conveyed in the printing unit 40 is defined as the +X-axis direction, and the width direction of the cloth 95 intersecting both the Z-axis direction and the X-axis direction is defined as the Y-axis direction. In addition, the positional relationship along the conveying direction of the cloth 95 or the moving direction of the endless belt 23 is also referred to as the "upstream side" or the "downstream side".
[0258] The medium supply unit 10 supplies the cloth 95 on which the image is formed to the printing unit 40 side. The medium supply unit 10 includes a supply shaft unit 11 and a bearing unit 12. The supply shaft unit 11 is formed in a cylindrical or columnar shape and is arranged in a manner that can rotate in the circumferential direction. A strip of cloth 95 is rolled up on the supply shaft unit 11. The supply shaft unit 11 is mounted on the bearing unit 12 in a manner that allows for loading and unloading. Thus, the cloth 95 in a state of being pre-wound on the supply shaft unit 11 can be mounted on the bearing unit 12 together with the supply shaft unit 11.
[0259] The bearing portion 12 supports both ends of the supply shaft portion 11 in an axial direction so as to be rotatable. The medium supply portion 10 has a rotation drive portion (not shown) for driving the supply shaft portion 11 to rotate. The rotation drive portion rotates the supply shaft portion 11 in a direction in which the cloth 95 is fed. The operation of the rotation drive portion is controlled by the control portion 1. The conveying rollers 21 and 22 relay the cloth 95 from the medium supply portion 10 to the endless belt 23.
[0260] The endless belt 23 is held between at least two rollers that rotate the endless belt 23, and the endless belt 23 rotates to support the cloth 95 while conveying it in the conveying direction (+X axis direction). Specifically, the endless belt 23 is a seamless belt formed by seamlessly connecting the two ends of a belt-shaped belt, and is hung between two rollers, a belt rotating roller 24 and a belt driving roller 25.
[0261] The endless belt 23 is held in a state where a predetermined tension is applied so that the portion between the belt rotating roller 24 and the belt driving roller 25 is horizontal. An adhesive 29 for bonding the cloth 95 is applied to the surface (supporting surface) 23a of the endless belt 23. That is, the endless belt 23 has an adhesive layer composed of the adhesive 29. The cloth 95 is attached to the endless belt 23 via the adhesive 29. The endless belt 23 supports (holds) the cloth 95 supplied from the conveying roller 22 and in close contact with the adhesive 29 in the medium close contact portion 60 described later.
[0262] The adhesive 29 preferably has increased adhesiveness due to heating. By using the adhesive 29 whose adhesiveness is increased due to heating, the fabric 95 and the adhesive layer can be well adhered. As such an adhesive 29, for example, a hot melt adhesive having a thermoplastic elastomer SIS (styrene-isoprene-styrene) as a main component can be cited.
[0263] The belt rotating roller 24 and the belt driving roller 25 support the inner peripheral surface 23b of the endless belt 23. Between the belt rotating roller 24 and the belt driving roller 25, there are provided a contact portion 69, a belt supporting portion 91, and a pressing plate 46 for supporting the endless belt 23. The contact portion 69 is provided in a region opposite to a pressing portion 61 to be described later across the endless belt 23, the pressing plate 46 is provided in a region opposite to the printing portion 40 across the endless belt 23, and the belt supporting portion 91 is provided between the contact portion 69 and the pressing plate 46. By supporting the endless belt 23 by the contact portion 69, the belt supporting portion 91, and the pressing plate 46, it is possible to suppress the vibration of the endless belt 23 as the endless belt 23 is moved.
[0264] The belt drive roller 25 is a driving unit that transports the cloth 95 in the transport direction by rotating the endless belt 23, and has a motor (not shown) that drives the belt drive roller 25 to rotate. The belt drive roller 25 is disposed on the downstream side of the printing unit 40 in the transport direction of the cloth 95, and the belt rotating roller 24 is disposed on the upstream side of the printing unit 40. When the belt drive roller 25 is driven to rotate, the endless belt 23 rotates with the rotation of the belt drive roller 25, and the belt rotating roller 24 rotates due to the rotation of the endless belt 23. Due to the rotation of the endless belt 23, the cloth 95 supported by the endless belt 23 is transported in the transport direction (+X axis direction), and an image is formed on the cloth 95 in the printing unit 40 described later.
[0265] exist Figure 1 In the example shown, the cloth 95 is supported on the side (+Z axis side) of the surface 23a of the endless belt 23 opposite to the printing section 40, and the cloth 95 is transported from the belt rotating roller 24 side to the belt driving roller 25 side together with the endless belt 23. In addition, on the side (-Z axis side) of the surface 23a of the endless belt 23 opposite to the cleaning unit 50, only the endless belt 23 moves from the belt driving roller 25 side to the belt rotating roller 24 side.
[0266] The transport roller 26 peels the cloth 95 on which the image is formed from the adhesive 29 of the endless belt 23 . The transport rollers 26 and 28 relay the cloth 95 from the endless belt 23 to the medium recovery unit 30 .
[0267] The medium recovery unit 30 recovers the cloth 95 transported by the medium transport unit 20. The medium recovery unit 30 includes a reel unit 31 and a bearing unit 32. The reel unit 31 is formed in a cylindrical or columnar shape and is arranged to be rotatable in the circumferential direction. The strip-shaped cloth 95 is rolled up on the reel unit 31. The reel unit 31 is mounted on the bearing unit 32 in a detachable manner. Thus, the cloth 95 wound on the reel unit 31 can be removed together with the reel unit 31.
[0268] The bearing 32 rotatably supports both ends of the axial direction of the reel 31. The medium recovery unit 30 includes a rotation drive unit (not shown) for driving the reel 31 to rotate. The rotation drive unit rotates the reel 31 in a direction to wind the fabric 95. The operation of the rotation drive unit is controlled by the control unit 1.
[0269] Next, the heating section, the printing section 40 , the heating unit 27 , and the cleaning unit 50 provided along the medium conveying section 20 will be described.
[0270] 3.3. Heating unit
[0271] It is preferable that a heater for heating the endless belt 23 is provided on at least one of the contact portion 69 and the belt support portion 91. The heater constitutes the heating portion. When the contact portion 69 is provided with a heater, a pressing force and heat can be applied to the endless belt 23 by the pressing portion 61, so that the close contact of the fabric 95 to the endless belt 23 can be improved, which is preferable. Therefore, when a heater is provided on one of the contact portion 69 and the belt support portion 91, it is more preferable to provide it on the contact portion 69.
[0272] The heating unit heats the adhesive layer to soften it, thereby exerting its adhesiveness and improving the adhesion between the cloth 95 and the adhesive layer. This prevents the cloth 95 from moving on the endless belt 23, and enables good conveying accuracy.
[0273] A heater is provided on at least one of the abutment portion 69 and the belt support portion 91. When the endless belt 23 is heated, the temperature of the surface 23a of the endless belt 23 is preferably below 80 degrees, more preferably below 70 degrees Celsius, and further preferably below 60 degrees Celsius. When the temperature of the surface 23a of the endless belt 23 is within the above range, the reactivity of the resin particles contained in the ink composition can sometimes be suppressed, making it easier to clean the belt. In addition, the lower limit of the temperature of the surface 23a of the endless belt 23 is preferably above 30 degrees Celsius, more preferably above 35 degrees Celsius, and further preferably above 40 degrees Celsius, as long as the adhesiveness of the adhesive layer is exerted. In addition, the temperature of the surface 23a of the endless belt 23 can be measured by, for example, a radiation thermometer, a contact thermometer, etc., and is more preferably measured by a radiation thermometer.
[0274] When at least one of the contact portion 69 and the belt support portion 91 is provided with a heater, a temperature detection portion (not shown) for detecting the surface temperature of the endless belt 23 may be provided. As the temperature detection portion, for example, a thermocouple or the like may be used. Thus, the control unit 1 controls the heater based on the temperature detected by the temperature detection portion, thereby enabling the endless belt 23 to reach a predetermined temperature. In addition, a non-contact thermometer using infrared rays may be used as the temperature detection portion.
[0275] 3.4. Printing Department
[0276] The printing unit 40 is arranged above (on the +Z axis side) relative to the arrangement position of the endless belt 23, and prints on the cloth 95 placed on the surface 23a of the endless belt 23. The printing unit 40 includes an inkjet head 42, a carriage 43 carrying the inkjet head 42, and a carriage moving unit 45 that moves the carriage 43 in the width direction (Y axis direction) of the cloth 95 intersecting the conveying direction.
[0277] The inkjet head 42 is a unit that ejects the liquid composition supplied from the liquid box (not shown) from a plurality of nozzles to the cloth 95 under the control of the control unit 1 to attach it. The inkjet head 42 has a plurality of nozzles that eject the liquid composition to the cloth 95 to which the liquid composition is attached so that it is attached to the cloth 95. These multiple nozzles are arranged in a row to form a nozzle row, and the nozzle row is individually configured corresponding to the liquid composition. The liquid composition is supplied to the inkjet head 42 from each liquid box, and is ejected from the nozzle as droplets through an actuator (not shown) in the inkjet head 42. The droplets of the ejected liquid composition land on the cloth 95, forming images, texts, patterns, colors, etc. in the printing and dyeing area of the cloth 95.
[0278] The liquid composition mentioned here may be the above-mentioned softening liquid composition, coating liquid composition, ink composition, and reaction liquid composition. In addition, the type and amount of these liquid compositions can be appropriately set.
[0279] In the inkjet head 42, a piezoelectric element is used as a driving unit, i.e., an actuator, but the present invention is not limited to this method. For example, an electromechanical conversion element that displaces a vibration plate as an actuator by electrostatic adsorption, or an electrothermal conversion element that ejects a liquid composition as droplets by using bubbles generated by heating may also be used.
[0280] Figure 2 Schematic diagram showing an example of the arrangement of nozzle columns of an inkjet head. Figure 2 In the example of , the inkjet head is provided with: a nozzle column 42a having a nozzle group for ejecting the third ink (coating liquid composition), a nozzle column 42b having a nozzle group for ejecting the fourth ink (softening liquid composition), a nozzle column 42c having a nozzle group for ejecting the second ink (ink composition), and a nozzle column 42d having a nozzle group for ejecting the first ink (reaction liquid composition). Figure 2 The area surrounded by the frame in represents one chip, and two rows of nozzle groups constitute one chip. Moreover, eight chips a located on the upstream side in the X direction and eight chips b located on the downstream side are arranged along the Y direction, thereby forming a row of chips a and a row of chips b. In this example, these 16 chips are arranged in a zigzag shape (staggered shape) along the Y direction and are set on the carriage.
[0281] For example, the nozzles of two nozzle rows in one chip are arranged staggered in the X direction and arranged in a zigzag pattern (staggered pattern) along the X direction. On the other hand, the row of chip a and the row of chip b arranged along the Y direction are arranged in a straight line along the Y direction.
[0282] The rows of chips on the upstream and downstream sides of the X direction can make each composition attached to the same area of the fabric at an appropriate time in one main scan. In addition, the rows of two chips are staggered in the sub-scanning direction (X-axis direction), and the area to which each composition is attached can be changed according to the movement distance of the fabric obtained by the sub-scanning, or each composition can be attached to the same area multiple times.
[0283] In addition, the head nozzle group that performs ejection means the nozzle group used for recording in the recording method. When performing the main scan (Y-axis direction), if there is an image to be recorded in the area of the cloth opposite to the nozzle group, it is a group of nozzles that can eject the liquid composition from the nozzles, and is a nozzle group that is continuous in the conveying direction (+X-axis direction). Therefore, although the nozzle group itself exists, the nozzle group that is not used for recording in the recording method is not included in the nozzle group that performs ejection.
[0284] The carriage moving unit 45 is provided above the endless belt 23 (on the +Z axis side). The carriage moving unit 45 has a pair of guide rails 45a and 45b extending along the Y axis direction. The inkjet head 42 is supported by the guide rails 45a and 45b so as to be reciprocable along the Y axis direction together with the carriage 43.
[0285] The carriage moving part 45 is provided with a moving mechanism and a power source which are not shown in the figure. As the moving mechanism, for example, a mechanism composed of a ball screw and a ball nut, a linear guide mechanism, etc. can be used. In addition, the carriage moving part 45 has a motor (not shown) as a power source for moving the carriage 43 along the guide rails 45a and 45b. As the motor, various motors such as a stepping motor, a servo motor, and a linear motor can be used. When the motor is driven by the control of the control unit 1, the inkjet head 42 moves along the Y-axis direction together with the carriage 43.
[0286] 3.5. Heating unit
[0287] The heating unit 27 may also be disposed between the conveying roller 26 and the conveying roller 28. The heating unit 27 heats the ink composition, softening liquid composition, and coating liquid composition ejected onto the cloth 95. As a result, there is a tendency that the reaction of the resin particles contained in the ink composition can be fully carried out. By allowing the resin particles to react fully, an image with good friction fastness can sometimes be formed. In addition, the heating unit 27 may also be used for the purpose of drying the cloth 95. The heating unit 27 includes, for example, an IR heater, and by driving the IR heater, the ink composition and coating liquid composition ejected onto the cloth 95 can be reacted in a short time. As a result, the strip-shaped cloth 95 on which an image or the like is formed can be wound around the reel portion 31.
[0288] 3.6. Cleaning unit
[0289] The cleaning unit 50 is disposed between the belt rotating roller 24 and the belt driving roller 25 in the X-axis direction. The cleaning unit 50 includes a cleaning portion 51, a pressing portion 52, and a moving portion 53. The moving portion 53 moves the cleaning unit 50 integrally along the floor surface 99 and fixes the cleaning unit 50 at a predetermined position.
[0290] The pressing part 52 is a lifting device composed of, for example, a cylinder 56 and a ball bushing 57, and makes the cleaning part 51 disposed on the upper part thereof contact the surface 23a of the endless belt 23. The cleaning part 51 is hung between the belt rotating roller 24 and the belt driving roller 25 with a predetermined tension applied thereto, and cleans the surface (supporting surface) 23a of the endless belt 23 moving from the belt driving roller 25 toward the belt rotating roller 24 from below (in the -Z-axis direction).
[0291] The cleaning section 51 includes a cleaning tank 54, a cleaning roller 58, and a scraper 55. The cleaning tank 54 is a tank for storing a cleaning liquid for cleaning ink and foreign matter attached to the surface 23a of the endless belt 23, and the cleaning roller 58 and the scraper 55 are provided inside the cleaning tank 54. As the cleaning liquid, for example, water or a water-soluble solvent (such as an alcohol aqueous solution) can be used, and a surfactant or a defoaming agent can be added as needed.
[0292] When the cleaning roller 58 rotates, the cleaning liquid is supplied to the surface 23a of the endless belt 23, and the cleaning roller 58 and the endless belt 23 slide. Thus, the ink composition attached to the endless belt 23, the fibers of the cloth 95, etc. are removed by the cleaning roller 58.
[0293] The scraper 55 can be formed of a flexible material such as silicone rubber. The scraper 55 is provided downstream of the cleaning roller 58 in the conveying direction of the endless belt 23. The cleaning liquid remaining on the surface 23a of the endless belt 23 is removed by sliding between the endless belt 23 and the scraper 55.
[0294] According to such a recording device 100 , the recording method of this embodiment can be easily executed.
[0295] 4. Examples and Comparative Examples
[0296] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are based on mass unless otherwise specified. In addition, unless otherwise specified, the evaluation is performed under an environment of a temperature of 25° C. and a relative humidity of 40.0%.
[0297] 4.1. Preparation of ink
[0298] The first ink (reaction liquid composition), the second ink (ink composition), the third ink (coating liquid composition), and the fourth ink (softening liquid composition) were prepared as follows.
[0299] 4.1.1. Preparation of reaction solution composition
[0300] The components were placed in a container according to the composition of Table 1, mixed and stirred for 2 hours with a magnetic stirrer, and then filtered with a membrane filter with a pore size of 5 μm to obtain the first ink (reaction liquid) "Ink 1-1 to Ink 1-7" used in the examples and comparative examples. In addition, the numerical values in the table represent the amount of effective ingredients.
[0301] 4.1.2. Preparation of ink composition
[0302] The components were placed in a container according to the composition of Table 2, mixed and stirred for 2 hours with a magnetic stirrer, and then filtered with a membrane filter with a pore size of 5 μm to obtain the second ink (ink composition) "Ink 2-1 to Ink 2-3" used in the examples and comparative examples. In addition, the numerical values in the table represent the amount of effective ingredients. In addition, the anionic self-dispersible pigment and the anionic resin-dispersible pigment used the pigment dispersion prepared as follows.
[0303] Self-dispersible pigments
[0304] 500 g of carbon black raw material powder (primary particle size = 18 nm, BET specific surface area = 180 m 2 / g, DBP absorption = 186mL / 100g) was added to 3750g of ion exchange water, stirred with a dissolver, and heated to 45°C. Then, using a sand mill using zirconium oxide beads with a diameter of 0.8mm, 30000g of an aqueous solution of sodium hypochlorite (effective chlorine concentration = 12%) was added thereto while crushing at 45°C for 3.5 hours. Then, the sand mill was continued to crush for 30 minutes to obtain a reaction solution containing self-dispersible carbon black. The reaction solution was filtered with a 400-mesh metal wire mesh to separate the zirconium oxide beads and unreacted carbon black from the reaction solution. A 5% aqueous solution of potassium hydroxide was added to the separated reaction solution and adjusted to pH = 7.5. Desalination and purification were performed by ultrafiltration membrane until the conductivity of the liquid was 1.5mS / cm. Desalination and purification were further performed using an electrodialysis device until the conductivity of the liquid was 1.0mS / cm. The liquid was concentrated to a concentration of 17% by mass of self-dispersible carbon black. The concentrate was centrifuged to remove coarse particles and filtered through a 0.6 μm filter. Ion exchange water was added to the obtained filtrate to dilute it to a concentration of 15% by mass of the self-dispersible carbon black, and the mixture was dispersed to obtain a self-dispersible pigment dispersion.
[0305] Resin Dispersed Pigments
[0306] 10 parts by mass of ammonium salt of styrene-acrylic acid copolymer (weight average molecular weight 10000) as a dispersant and 55 parts by mass of ion exchange water were added to 15 parts by mass of carbon black as a polymer component and mixed thoroughly. The mixture was then dispersed in a sand mill (manufactured by Yaskawa Seisakusho Co., Ltd.) together with glass beads (diameter 1.7 mm, 1.5 times the amount of the mixture) for 2 hours. After dispersion, the glass beads were removed to obtain a resin-dispersed pigment dispersion.
[0307] 4.1.3. Preparation of coating liquid composition
[0308] The components were placed in a container according to the composition of Table 3, mixed and stirred for 2 hours with a magnetic stirrer, and then filtered with a membrane filter with a pore size of 5 μm to obtain the third ink (coating liquid composition) "Ink 3-1 to Ink 3-4" used in the examples and comparative examples. In addition, the numerical values in the table represent the amount of effective ingredients.
[0309] 4.1.4. Preparation of softening liquid composition
[0310] The fourth inks (softening liquid compositions) "Ink 4-1 to Ink 4-9" shown in Table 4 were obtained as follows. The numerical values in the table represent the amounts of effective ingredients.
[0311] Ink 4-2, Ink 4-7 and Ink 4-8
[0312] 90g of dimethyl silicone oil (Shin-Etsu silicone, KF-96H-10,000cs), 171.5g of ion exchange water, 6.4g of polyoxyethylene tridecyl ether (Japan emulsifier, Newcol 1310), 6.4g of polyoxyethylene tridecyl ether (Japan emulsifier, Newcol 1305) and 25.7g of 1,2-hexanediol were placed in a beaker, and a homogenizer (made by PRIMIX, homogenizer MARKII2.5 type) was used to stir the contents of the beaker at a rotation speed of 2000rpm and 50°C for 30 minutes, and then allowed to stand for 30 minutes. Then, the contents of the beaker were filtered with a 10μm membrane filter to obtain 300g of an emulsion in which oil particles containing nonionic silicone oil were dispersed. Next, ion exchange water and glycerin were added and stirred to prepare ink 4-2 described in Table 4.
[0313] Ink 4-7 and Ink 4-8 were prepared as follows: after obtaining an emulsion by changing the amount of dimethyl silicone oil (Shin-Etsu Silicone, KF-96H-10,000cs) used, ion exchange water, glycerin and polyvinyl pyrrolidone were added to the concentrations shown in Table 4 and stirred.
[0314] Ink 4-1
[0315] 90 g of amino-modified silicone oil ("KF-868" manufactured by Shin-Etsu Chemical Co., Ltd., functional group equivalent: 8,800 g / mol), 173.2 g of ion-exchanged water, 5.1 g of polyoxyethylene tridecyl ether (Japan emulsifier, Newcol 1310), 25.7 g of 1,2-hexanediol and 6 g of lactic acid were placed in a beaker, and a homogenizer (manufactured by PRIMIX Co., Ltd., homogenizer MARKII2.5 type) was used to stir the contents of the beaker at a rotation speed of 2000 rpm and 50°C for 30 minutes, and then allowed to stand for 30 minutes. Next, the contents of the beaker were filtered with a 10 μm membrane filter to obtain 300 g of an emulsion in which oil particles containing amino-modified silicone oil were dispersed. Next, ion-exchanged water and glycerin were added and stirred to prepare ink 4-1.
[0316] Ink 4-3~Ink 4-6
[0317] 51.4 g of each softener listed in Table 4, 210.5 g of ion exchange water, 6.4 g of polyoxyethylene tridecyl ether (Japan emulsifier, Newcol 1310), 6.4 g of polyoxyethylene tridecyl ether (Japan emulsifier, Newcol 1305), 25.7 g of 1,2-hexanediol and 6 g of lactic acid were placed in a beaker, and the contents of the beaker were stirred at a rotation speed of 2000 rpm and 50°C for 30 minutes using a homogenizer (manufactured by PRIMIX, homogenizer II.5 type) and allowed to stand for 30 minutes. Then, the contents of the beaker were filtered with a 10 μm membrane filter to obtain 300 g of a liquid containing each softener. Next, ion exchange water and glycerin were added and stirred to prepare inks 4-3 to 4-6.
[0318] Ink 4-9
[0319] 64.3 g of polyoxyethylene dilaurate, 191.2 g of ion exchange water, 6.4 g of polyoxyethylene tridecyl ether (Japan emulsifier, Necol 1310), 6.4 g of polyoxyethylene tridecyl ether (Japan emulsifier, Necol 1305), 25.7 g of 1,2-hexanediol and 6 g of lactic acid were placed in a beaker, and a homogenizer (manufactured by PRIMIX, homogenizer MARKII2.5 type) was used to stir the contents of the beaker at a rotation speed of 2000 rpm and 50°C for 30 minutes, and then allowed to stand for 30 minutes. Then, the contents of the beaker were filtered with a 10 μm membrane filter to obtain 300 g of a liquid containing a softener and polyoxyethylene dilaurate. Then, ion exchange water, glycerol and polyvinyl pyrrolidone were added to the concentrations described in Table 4 and stirred to prepare inks 4-9.
[0320] "OLFINE E1010" described in Tables 1 to 3 is an acetylene glycol-based surfactant manufactured by Nissin Chemical Industry Co., Ltd.
[0321] Evaluation methods
[0322] 4.2.1. Recording test
[0323] Using a modified EvoTre16 (manufactured by Seiko Epson Corporation), printing was performed on a recording medium of 100% cotton white wide cloth (#4000, manufactured by Nisshinbo Co., Ltd.) under the conditions described in Tables 5 to 9. The same scanning area was subjected to multiple (2, 4, 8, 12, or 16) main scans to form a 20 cm × 5 cm full-print pattern image on the cloth as the recording medium. Then, the cloth was conveyed 5 cm in the sub-scanning direction, and the same scanning area was printed again in the same manner. By printing twice, a 20 cm × 10 cm full-print pattern image was formed on the cloth as the recording medium.
[0324] After the image is formed, it is placed for 3 minutes and then heated in an oven at 160°C for 3 minutes to dry it, thereby producing the printed and dyed products involved in each embodiment and each comparative example. In addition, the "full-plate pattern image" refers to an image with dots uniformly formed on the entire surface of the recording area (main scanning direction × sub-scanning direction: 20 cm × 10 cm) in a manner such that the coating amount of each ink becomes the numerical value recorded in the embodiment.
[0325] The inkjet head used was a head unit in which the nozzle spacing in the sub-scanning direction was 600 dpi and two head chips were arranged in the sub-scanning direction so that the length of the nozzle array exceeded 2 inches.
[0326] use Figure 2 In each example, the inkjet head shown in the figure has a nozzle group for ejecting each ink as shown in the figure. Figure 2 Each ink is filled so as to be arranged in the main scanning direction. Figure 3 TABLE 1 is a table showing ink ejected from the nozzle array of the inkjet head used in the examples and comparative examples. Figure 3 The first to fourth in the figure represent the first ink (reaction liquid) to the fourth ink (softening liquid), respectively, and indicate that the inks are ejected from the nozzle arrays shown in the figure.
[0327] In addition, in each embodiment, the nozzle group for ejecting each ink is as follows: Figure 3 Each ink is filled in a manner arranged in the main scanning direction as shown in the head structure in FIG. Figure 3 A plurality of nozzle rows are arranged in parallel in the left-right direction. Figure 3 The vertical direction is described in the figure, but in the actual nozzle arrangement Figure 2That is, each row has a chip a and a chip b arranged on the left and right. Chip a and chip b each have two rows of nozzles. Figure 3 The composition ejected from each column is described in the column. A blank column indicates that the composition was not ejected. Figure 2 Columns 1 to 16 of chip a in correspond to Figure 3 Columns 1 to 16 of chip a in Figure 2 Columns 1 to 16 of chip b in correspond to Figure 3 Columns 1 to 16 of chip b in .
[0328] In addition, only the fourth ink of Example 2 was applied by spraying. In the other examples using the first ink, the second ink, the third ink, and the fourth ink, they were all applied by the inkjet method.
[0329] In Example 29, the first ink (reaction liquid) and the third ink (coating liquid) were attached to 2.0 mm outside the attachment area of the fourth ink (softening liquid). In other examples and comparative examples, the third ink (coating liquid) and the fourth ink (softening liquid) were attached to the same area as the first ink (reaction liquid).
[0330] 4.2.2. Evaluation of hair color (black)
[0331] For the printed product obtained by the above-mentioned printing method, the optical density (OD value, Status E) of the black color of the printed image was measured on the surface of the printed image using a colorimeter (FD-7, manufactured by Konica Minolta Co., Ltd.), and the evaluation was performed according to the following criteria. In the case of a C evaluation or above, it can withstand actual use.
[0332] Judgment Criteria
[0333] SS: OD value is above 1.60
[0334] S: OD value is 1.51 or more and less than 1.60
[0335] A: OD value is 1.46 or more and less than 1.51
[0336] B: OD value is 1.43 or more and less than 1.46
[0337] C: OD value is 1.35 or more and less than 1.43
[0338] 4.2.3. Evaluation of seepage
[0339] In each example, a printed material is prepared which is dried by heating at 160°C for 3 minutes in an oven after being placed for 60 minutes after the image is formed in the above-mentioned printing method. In addition, a printed material is prepared as a reference after being dried after being printed with the first ink (reaction liquid) and the second ink (ink composition) in Example 1. The boundary between the printed image area and the unprinted non-printing area is observed, and the difference in length (mm) in the sub-scanning direction of the printed image that has been placed for 60 minutes in each example relative to the printed image as a reference is determined based on the following criteria. In the case of a C rating or above, it can withstand actual use.
[0340] Judgment Criteria
[0341] S: The difference in length is less than 1 mm
[0342] A: The difference in length is more than 1mm and less than 3mm
[0343] B: The difference in length is more than 3 mm and less than 7 mm
[0344] C: The difference in length is more than 7 mm and less than 12 mm
[0345] 4.2.4. Evaluation of yellowing
[0346] In the above printing method, only the fourth ink (softening liquid) of each example was prepared at 30 g / m 2 The printed cloth recorded on the recording cloth and dried by the above method was used as a sample, and the L*, a*, and b* of the surface of the printed image were measured using a colorimeter (FD-7, manufactured by Konica Minolta). In addition, a cloth that was not printed by a printer in the above method but dried in an oven at 160°C for 3 minutes was prepared, and L*, a*, and b* were measured in the same way as a reference. For this reference, the color difference ΔE00 (ΔE2000) of the sample was calculated, and judgment was made according to the following criteria.
[0347] Judgment Criteria
[0348] A: Color difference ΔE00 is less than 2
[0349] B: Color difference ΔE00 is more than 2 and less than 7
[0350] 4.2.5. Evaluation of abrasion resistance (drying)
[0351] For the printed product produced by the above printing method, a clock meter (FI-306, manufactured by Tester Industry Co., Ltd.) was used to rub the image of the printed product 10 times with a muslin cloth (cotton white cloth) at a load of 9 N. Then, the optical density (OD, Status E) of the black color of the printed image was measured in the area of the muslin cloth contaminated by the ink after rubbing using a colorimeter (FD-7, manufactured by Konica Minolta Co., Ltd.), and the evaluation was made according to the following criteria. In the case of a C rating or above, it can withstand actual use.
[0352] Judgment Criteria
[0353] S: Black OD is 0.15 or less
[0354] A: Black OD is more than 0.15 and less than 0.19
[0355] B: Black OD is more than 0.19 and less than 0.23
[0356] C: Black OD is more than 0.23 and less than 0.33
[0357] 4.2.6. Evaluation of abrasion resistance (wetting)
[0358] For each example of printed matter produced by the above-mentioned printing method, a clock meter (FI-306, manufactured by Tester Industry Co., Ltd.) was used to rub the image of the printed matter 10 times with a muslin cloth (cotton white cloth) moistened with water in an amount equal to the weight of the cloth at a load of 9 N. Then, the optical density (OD, Status E) of the black color of the printed image was measured in the area of the muslin cloth contaminated with ink after rubbing using a colorimeter (FD-7, manufactured by Konica Minolta Co., Ltd.), and the evaluation was made according to the following criteria. In the case of an evaluation of B or more, it can be said that a good effect was obtained.
[0359] Judgment Criteria
[0360] S: Black OD is 0.26 or less
[0361] A: Black OD is more than 0.26 and less than 0.31
[0362] B: Black OD is more than 0.31 and less than 0.45
[0363] C: Black OD exceeds 0.45
[0364] 4.2.7. Evaluation of hand feel (shear hardness G)
[0365] For each printed product, the shear stiffness G (gf / cm / degree) was tested using a tensile shear tester ("KES-FB1-A" manufactured by Kado Technology Co., Ltd.). Next, as a reference, a printed product printed with only the first ink and the second ink in addition to the third ink and the fourth ink in each example and then dried was prepared, and the shear stiffness G was tested in the same way. The change in shear stiffness G was calculated by the following formula, and the feel was evaluated according to the following evaluation criteria. In the case of A evaluation, it can be said that a good effect was obtained.
[0366] ((Shear stiffness G of each example) - (Shear stiffness G of reference))
[0367] Judgment Criteria
[0368] A: The change in shear stiffness G is less than +1.5
[0369] C: The change in shear stiffness G exceeds +1.5
[0370] On the other hand, the texture when treated alone was determined as follows and is shown in Tables 3 and 4.
[0371] The third ink (coating liquid) or the fourth ink (softening liquid) described in each example was impregnated into a recording medium of 100% cotton white wide cloth (#4000, manufactured by Nisshinbo Co., Ltd.), and each composition was applied to the cloth using a squeeze roller so that the squeeze ratio was 80%. Then, it was dried at 160°C for 3 minutes to obtain cloths with each composition attached thereto.
[0372] In addition, the liquid squeeze rate (S) is calculated by the following formula.
[0373] S(%)=[(AB) / B]×100
[0374] In the above formula, S represents the squeeze rate (%), A represents the mass of the cloth to which each composition is attached, and B represents the mass of the cloth before each composition is attached.
[0375] Next, the shear stiffness G (gf / cm / degree) of the cloth to which each composition was attached alone (treated cloth) was tested using a tensile shear tester ("KES-FB1-A" manufactured by Kado Technology Co., Ltd.). In addition, in Tables 5 to 9, the "magnitude relationship of the fourth ink relative to the third ink" describes the magnitude relationship of the feel (shear hardness) of the fourth ink (softening liquid) used in each example when treated alone relative to the feel (shear hardness) of the third ink (coating liquid) when treated alone.
[0376] 4.2.8. Evaluation of water absorption
[0377] For each printed product produced using the above printing method, the time from when one drop of pure water was dripped onto the back of the printed surface to when the water droplet penetrated into the printed fabric and could no longer be seen on the printed surface was measured at room temperature, and evaluation was performed according to the following evaluation criteria.
[0378] Judgment Criteria
[0379] A: The time until the water droplets can no longer be seen on the printed surface is less than 5 seconds
[0380] B: The time until the water droplets can no longer be seen on the printed surface exceeds 5 seconds
[0381] 4.2.9. Evaluation of the cohesiveness of the mixture with the first ink (reaction solution)
[0382] 15 mL of the first ink (reaction liquid) was added to a 30 mL glass bottle, and 0.1 ml of the second ink (ink composition), the third ink (coating liquid), or the fourth ink (softening liquid) was dripped from the top thereof with a dropper at 25°C. After dripping, the mixture was allowed to stand at 25°C for 1 minute, and then oscillated and stirred 5 times. When the sediment or floating matter can be visually confirmed, the mixed cohesion is considered to be "yes". On the other hand, when the mixture is visually dissolved or diluted, the mixed cohesion is considered to be "no". The results are recorded in Tables 5 to 9.
[0383] Evaluation results
[0384] It has been found that in each embodiment, a recorded object with good image resistance (wetting) and good feel is obtained, wherein each embodiment has: a softening liquid attachment step of attaching a softening liquid composition containing a softener and water to a recording medium; and a coating liquid attachment step of attaching a coating liquid composition containing anionic resin particles and water to a recording medium, wherein the content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition, and the content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition, and the coating liquid attachment step is performed by an inkjet method, and the softening liquid attachment step is performed by an inkjet method or a spray method.
[0385] The present invention includes substantially the same configuration as that described in the embodiment, for example, a configuration having the same function, method and result, or a configuration having the same purpose and effect. In addition, the present invention includes a configuration in which a non-essential part of the configuration described in the embodiment is replaced. In addition, the present invention includes a configuration having the same effect as that of the configuration described in the embodiment, or a configuration capable of achieving the same purpose. In addition, the present invention includes a configuration in which a known technology is added to the configuration described in the embodiment.
[0386] The following contents are derived from the above-mentioned embodiments and modifications.
[0387] The record method has:
[0388] a softening liquid attaching step of attaching a softening liquid composition containing a softener and water to the recording medium; and
[0389] a coating liquid attaching step of attaching a coating liquid composition containing anionic resin particles and water to a recording medium,
[0390] The content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition.
[0391] The content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition.
[0392] The coating liquid attachment step is performed by an inkjet method,
[0393] The softening liquid attaching step is performed by an inkjet method or a spray method.
[0394] According to this recording method, by attaching a softening liquid composition to a recording medium, a softener (depending on the degree of hydrophobicity) is attached to the fibers of the recording medium, making it easy for the molecules of the fibers to move, and the hardness of the fibers is relaxed (because the fibers become easy to slide against each other and in the case of natural fibers, the OH groups of the fibers are hindered from bonding with each other, making it difficult for the fibers to shrink), so that the feel of the recorded object can be improved.
[0395] On the other hand, since the softener is a hydrophobic material, it has a strong affinity with the hydrophobic color materials such as pigments and disperse dyes. Therefore, the hydrophobic color material is difficult to be taken into the fixing resin on the recording medium from other compositions. Thus, the hydrophobic color material easily falls off from the recording medium, and there is a tendency for the wet friction fastness to deteriorate.
[0396] However, according to this recording method, by using a coating liquid at the same time, the hydrophobic color material exposed on the surface of the recording medium is covered with the resin of the coating liquid, and the amount of resin in the coating liquid is large, so that a strong resin film can be formed. As a result, the hydrophobic color material is difficult to fall off, the wet friction fastness of the recorded object can be improved, and the hand feel can also be improved.
[0397] Such an effect is obtained by applying the softening liquid and the coating liquid in different attachment processes. That is, when a softener and resin particles are contained in one composition and attached to a recording medium, the softener and the resin particles are uniformly mixed in the composition and in the attached droplets, and the softener enters the resin coating film, making it difficult to form a resin network and unable to achieve good wet friction fastness. Therefore, in this recording method, by combining the softener and the resin particles in different compositions and attaching them to the recording medium separately, it is possible to suppress the softener from entering the resin coating film, thereby achieving both the feel of the recorded object and the wet friction fastness.
[0398] In the above recording method,
[0399] The recording medium may be cloth.
[0400] According to this recording method, the above-mentioned effect is more significantly exhibited.
[0401] In the above recording method,
[0402] The softener may be at least one selected from particles containing organopolysiloxane, fatty acid esters, dialkyldimethylammonium salts, imidazoline-type surfactants, and amphoteric surfactants.
[0403] According to this recording method, a recorded object having even better wet friction fastness can be obtained.
[0404] In the above recording method,
[0405] The softener may include particles containing organopolysiloxane.
[0406] According to this recording method, a water-repellent effect can be imparted to the fibers of the recording medium, and thus the wet friction fastness of the recorded object can be further improved.
[0407] In the above recording method,
[0408] The organopolysiloxane may be nonionic.
[0409] According to this recording method, yellowing of recorded matter can be further reduced.
[0410] In the above recording method,
[0411] The coating liquid attaching step may be performed before the softening liquid attaching step, or may be performed simultaneously with the softening liquid attaching step.
[0412] According to the recording method, it is difficult to hinder the adhesion between the coating formed by the coating liquid composition and the recording medium (fiber), the wet friction fastness can be improved, and the uneven color development of the recorded object can be further reduced. This effect is due to the fact that the softener contained in the softening liquid composition is hydrophobic, so the adhesion between the coating and the recording medium (fiber) is easier to occur than when the softening liquid is first attached to the recording medium.
[0413] In the above recording method, the following may also be included:
[0414] an ink attaching step of attaching an ink composition containing a pigment and water to a recording medium by an inkjet method; and
[0415] In the reaction liquid attachment step, a reaction liquid composition containing a coagulant for aggregating the components of the ink composition and water is attached to a recording medium by an inkjet method.
[0416] According to this recording method, by attaching the softening liquid composition to the recording medium, the softener (depending on the hydrophobicity) is attached to the fibers of the recording medium, so that the molecules of the fibers become easy to move, and the hardness of the fibers is relaxed (because the fibers become easy to slide and the fibers become difficult to shrink by hindering the bonding of the OH groups of the fibers in the case of natural fibers), the feel of the recorded object can be improved. On the basis of this effect, the pigment from the ink composition exposed to the surface of the recording medium is covered with the resin of the coating liquid, and the amount of resin in the coating liquid is also large, so that a resin film with a strong pigment can be formed. As a result, the pigment is difficult to fall off, and the wet friction fastness of the recorded object can also be improved. In addition, due to the coagulant of the reaction liquid composition, the pigment in the ink composition can be coagulated, and the color development of the recorded object can also be improved.
[0417] In the above recording method,
[0418] The ink attaching step and the reaction liquid attaching step may be performed before the coating liquid attaching step or simultaneously with the coating liquid attaching step.
[0419] According to this recording method, the above-mentioned effect of wet friction fastness is more significantly exhibited.
[0420] In the above recording method,
[0421] The reaction liquid attaching step may be performed before the ink attaching step or simultaneously with the ink attaching step.
[0422] According to this recording method, the above-mentioned effect of color development is more significantly exhibited.
[0423] In the above recording method, it can also be,
[0424] The coating liquid composition has cohesiveness due to the coagulant, and the softening liquid composition does not have cohesiveness due to the coagulant.
[0425] According to this recording method, the bleeding of the softening liquid composition on the recording medium can be further suppressed. In the above recording method,
[0426] The shear hardness of the softening liquid composition may be smaller than the shear hardness of the coating liquid composition.
[0427] According to this recording method, the color development, bleeding, yellowing, and abrasion resistance (drying) of the recorded matter can be improved.
[0428] In the above recording method,
[0429] The amount of softening liquid attached can be 15g / m 2 Above 80g / m 2 the following.
[0430] According to this recording method, the bleeding of the softening liquid can be further suppressed. In addition, since the coating can be performed to the minimum extent necessary, the original water absorption and feel of the recording medium can be well maintained.
[0431] In the above recording method,
[0432] The coating composition can have an attachment amount of 30 g / m 2 Above 60g / m 2 the following.
[0433] In the above recording method,
[0434] The ratio of the amount of the softening liquid attached to the amount of the coating liquid composition attached may be 0.25 or more and 1 or less.
[0435] According to this recording method, since the softening liquid is prone to bleeding, the amount of the softening liquid deposited is smaller than that of the coating liquid, thereby making it more difficult for bleeding to occur.
[0436] In the above recording method,
[0437] The area on the recording medium to which the coating liquid composition is applied in the coating liquid attaching step may be larger than the area on the recording medium to which the softening liquid composition is applied in the softening liquid attaching step.
[0438] According to this recording method, the coating area of the coating liquid located below is made wider than the coating area of the softening liquid, so that the bleeding of the softening liquid can be further suppressed.
[0439] In the above recording method,
[0440] The content of the colorant in the softening liquid composition may be 0.1% by mass or less relative to the total amount of the softening liquid composition.
[0441] The composition group has:
[0442] A softening liquid composition comprising a softener and water; and
[0443] The coating liquid composition comprises anionic resin particles and water.
[0444] The content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition.
[0445] The content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition.
[0446] The coating liquid composition is used by ejecting it by an inkjet method.
[0447] The softening liquid composition is used by being ejected by an inkjet method or a spray method.
[0448] According to this composition group, by attaching the softening liquid composition to the recording medium, the softener (depending on the degree of hydrophobicity) is attached to the fibers of the recording medium, making it easy for the molecules of the fibers to move, and the hardness of the fibers is relaxed (because the fibers become easy to slide against each other and in the case of natural fibers, the OH groups of the fibers are hindered from bonding with each other, making it difficult for the fibers to shrink), which can make the feel of the recorded material good.
[0449] In addition, according to the composition set, by using the coating liquid at the same time, the hydrophobic color material exposed on the surface of the recording medium is covered with the resin of the coating liquid, and the amount of resin in the coating liquid is also large, so that a strong resin film can be formed. As a result, the hydrophobic color material is difficult to fall off, the wet friction fastness of the recorded object can be improved, and the hand feel can also be improved.
Claims
1. A recording method, characterized in that: have: A softening liquid attaching step of attaching a softening liquid composition containing a softener and water to the recording medium; as well as a coating liquid attaching step of attaching a coating liquid composition containing anionic resin particles and water to a recording medium, The content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition. The content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition. The coating liquid attachment step is performed by an inkjet method, The softening liquid attaching step is performed by an inkjet method or a spray method.
2. The recording method according to claim 1, characterized in that The recording medium is cloth.
3. The recording method according to claim 1 or 2, characterized in that: The softener is at least one selected from particles containing organic polysiloxane, fatty acid esters, dialkyldimethylammonium salts, imidazoline surfactants and amphoteric surfactants.
4. The recording method according to claim 1 or 2, characterized in that: The softener includes particles containing organopolysiloxane.
5. The recording method according to claim 4, characterized in that: The organopolysiloxane is nonionic.
6. The recording method according to claim 1 or 2, characterized in that: The coating liquid attaching step is performed before the softening liquid attaching step, or is performed simultaneously with the softening liquid attaching step.
7. The recording method according to claim 1 or 2, characterized in that: Also features: An ink attaching step of attaching an ink composition containing a pigment and water to a recording medium by an inkjet method; as well as In the reaction liquid attachment step, a reaction liquid composition containing a coagulant for aggregating the components of the ink composition and water is attached to a recording medium by an inkjet method.
8. The recording method according to claim 7, characterized in that: The ink attaching step and the reaction liquid attaching step are performed before the coating liquid attaching step or simultaneously with the coating liquid attaching step.
9. The recording method according to claim 7, characterized in that: The reaction liquid attaching step is performed before the ink attaching step or simultaneously with the ink attaching step.
10. The recording method according to claim 7, characterized in that: The coating liquid composition has cohesiveness due to the coagulant, and the softening liquid composition does not have cohesiveness due to the coagulant.
11. The recording method according to claim 1 or 2, characterized in that: The shear hardness of the softening liquid composition is smaller than the shear hardness of the coating liquid composition.
12. The recording method according to claim 1 or 2, characterized in that: The attachment amount of the softening liquid is 15g / m 2 Above and 80g / m 2 the following.
13. The recording method according to claim 1 or 2, characterized in that: The coating composition has an adhesion of 30 g / m 2 Above and 60g / m 2 the following.
14. The recording method according to claim 1 or 2, characterized in that: The ratio of the adhesion amount of the softening liquid to the adhesion amount of the coating liquid composition is 0.25 or more and 1 or less.
15. The recording method according to claim 1 or 2, characterized in that: The area on the recording medium to which the coating liquid composition is applied in the coating liquid attaching step is larger than the area on the recording medium to which the softening liquid composition is applied in the softening liquid attaching step.
16. The recording method according to claim 1 or 2, characterized in that: The content of the colorant in the softening liquid composition is 0.1% by mass or less relative to the total amount of the softening liquid composition.
17. A composition set, characterized in that: have: A softening liquid composition comprising a softener and water; and The coating liquid composition comprises anionic resin particles and water. The content of the softener is 60% by mass or more relative to the total amount of non-volatile components in the softening liquid composition. The content of the resin particles is 80% by mass or more relative to the total amount of non-volatile components in the coating liquid composition. The coating liquid composition is used by ejecting it by an inkjet method. The softening liquid composition is used by being ejected by an inkjet method or a spray method.