Drying method and drying system for methanol-washed metal oxide catalyst

Through the blade dryer and multi-stage condenser system, the labor intensity, uneven product quality and safety hazards of metal oxide catalyst drying in the prior art are solved, and the methanol moisture content is significantly reduced and continuous automatic drying is achieved. Reduces production costs and heat energy consumption.

CN119063435APending Publication Date: 2024-12-03WUHUAN ENG
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411164459.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing metal oxide catalyst drying technology has problems such as high labor intensity, uneven product quality, poor drying effect, and safety hazards of flammable and explosive solvents. In particular, the high energy consumption of flash drying and large investment in dust recovery devices are not suitable. Drying of solvents such as methanol.

Method used

The blade dryer is used to combine low-pressure saturated steam with indirect heating and drying. The methanol is recovered through bag dust collector and multi-stage condenser, and the carrier gas is recycled. The heater adjusts the outlet exhaust of the circulating fan to achieve continuous in the micro-negative pressure drying chamber. Automatic drying to reduce the moisture content of methanol.

Benefits of technology

It has achieved drying of metal oxide catalysts with excellent drying effect, low cost and high safety. The methanol moisture content has been reduced from 50 to 60% to no more than 0.2%, reducing heat energy consumption and personnel operation costs, avoiding dust spillage and safety hazards .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119063435A_ABST
    Figure CN119063435A_ABST
Patent Text Reader

Abstract

The invention discloses a method for drying a methanol-washed metal oxide catalyst, which comprises the following steps: feeding a wet metal oxide catalyst into a drying cavity of a paddle dryer, and introducing low-pressure saturated steam into the paddle dryer to indirectly heat and dry the wet metal oxide catalyst, dry tail gas generated by the paddle dryer is carried by circulating carrier gas to be fed into the bag type dust collector for dust removal, the tail gas subjected to dust removal enters the primary condenser, the uncondensed tail gas of the primary condenser is fed into the secondary condenser, and the uncondensed tail gas at an outlet of the secondary condenser serves as the circulating carrier gas, is pressurized by the circulating fan and then is fed into the carrier gas heater for heating; and the heated circulating carrier gas enters the drying cavity of the paddle dryer through the circulating carrier gas inlet pipeline for recycling. The device is simple in structure, few in accessory equipment and low in investment cost, the moisture content of methanol in the dried metal oxide catalyst is low, the drying effect is good, continuous automatic drying can be achieved, and the personnel operation cost is reduced; the using amount of saturated steam can be adjusted according to the temperature of materials at the discharge port of the paddle dryer, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal oxide catalyst drying, and in particular relates to a method and a drying system for a metal oxide catalyst after washing with methanol. Background Art

[0002] Methacrylonitrile is a colorless liquid and an important chemical raw material. It can be used as an intermediate product to produce a high-performance, lightweight and high-strength polymer material, methacrylimide (PMI).

[0003] When synthesizing methacrylonitrile, a metal oxide catalyst is needed to catalyze the reaction process to increase the yield of methacrylonitrile. However, the new products generated will cover the active components of the catalyst or block the pores of the catalyst, making it impossible for the reactants to contact the active components, causing the catalyst to temporarily lose its activity. At this time, the activity of the catalyst needs to be restored through methanol washing, filtration, drying and other operation units, and drying is the key link in restoring the activity of the catalyst.

[0004] Traditional drying methods for catalysts mainly include box drying, fluidized bed drying, flash drying and chain plate drying. Box drying has high labor intensity, uneven product quality, poor drying effect and difficulty in continuous operation; fluidized bed drying is prone to wet material agglomeration, and as the amount of material increases, the fluidization effect gradually decreases. Flash drying has high energy consumption, the material causes great wear on the equipment, and the investment in dust recovery equipment is large. Chain plate drying is an open cycle and is not suitable for drying flammable and explosive solvents such as methanol. In addition, open drying is also prone to serious safety hazards. Summary of the invention

[0005] The purpose of the present invention is to solve the above technical problems and provide a method and a drying system for a metal oxide catalyst after methanol washing with good drying effect and low cost.

[0006] To achieve the above object, the present invention provides a method for drying a metal oxide catalyst after washing with methanol as follows:

[0007] The wet metal oxide catalyst from the upstream centrifuge is fed into the drying chamber of the paddle dryer, and low-pressure saturated steam is passed into the paddle dryer to indirectly heat and dry the wet metal oxide catalyst to obtain a dried metal oxide catalyst product;

[0008] The dry exhaust gas produced by the paddle dryer is carried by the circulating carrier gas and sent to the bag filter for dust removal;

[0009] The tail gas after the bag filter dust removal enters the primary condenser, which uses circulating cooling water as a cold source to perform the initial condensation on the tail gas at the bag filter outlet, and the condensed liquid methanol is recovered;

[0010] The uncondensed tail gas from the primary condenser is then sent to the secondary condenser, which uses a refrigerant as a cold source to re-condense the outlet tail gas from the primary condenser, and the liquid methanol condensed by the secondary condenser is recovered;

[0011] The uncondensed exhaust gas at the outlet of the secondary condenser is used as circulating carrier gas and is pressurized by the circulating fan and then sent to the carrier gas heater; low-pressure saturated steam is introduced into the carrier gas heater as a heat source to heat the circulating carrier gas, and the heated circulating carrier gas enters the drying chamber of the paddle dryer through the circulating carrier gas inlet pipe for recycling.

[0012] Furthermore, the wet content of methanol in the wet metal oxide catalyst is 50-60 wt%.

[0013] Furthermore, the low-pressure saturated steam is introduced into the jacket and double hollow heat shaft of the paddle dryer to heat and dry the wet metal oxide catalyst through the wall; the residence time of the wet metal oxide catalyst in the drying chamber of the paddle dryer is 1.5 to 2.5 hours.

[0014] Furthermore, low-pressure saturated steam is introduced into the heating pipe of the bag filter to insulate the bag filter, thereby maintaining the exhaust temperature at the bag filter outlet at 80-90°C.

[0015] Furthermore, the uncondensed tail gas at the outlet of the secondary condenser is used as a circulating carrier gas and pressurized to 1500-2000 Pa by a circulating fan.

[0016] Furthermore, the carrier gas heater introduces low-pressure saturated steam as a heat source to heat the circulating carrier gas to 110-120°C.

[0017] Furthermore, a pressure measuring point is provided on the circulating carrier gas inlet pipe of the paddle dryer, and the exhaust volume at the circulating fan outlet is adjusted according to the pressure at the measuring point to maintain the negative pressure in the drying chamber of the paddle dryer at -180 to -200Pa.

[0018] Furthermore, the discharge port of the paddle dryer is provided with a temperature measuring point, and the flow rate of the low-pressure saturated steam is adjusted by measuring the temperature of the product at the discharge port, so as to control the temperature of the metal oxide catalyst product to be 110-120°C.

[0019] Furthermore, an online oxygen content measuring point is provided on the exhaust gas pipeline at the outlet of the bag filter. By measuring the oxygen content, when the oxygen content is greater than or equal to 5%, low-pressure nitrogen is supplemented at the outlet of the circulating fan.

[0020] Also provided is a drying system for the drying method as described above, comprising a feed buffer bin, a double screw feeder, a paddle dryer, a bag filter, a primary condenser, a secondary condenser, a circulating fan, a carrier gas heater and a methanol recovery tank;

[0021] The bottom outlet of the feed buffer bin is connected to the feed port of the paddle dryer via a double-screw feeder, the dry tail gas outlet of the paddle dryer is directly connected to the inlet of the bag dust collector, the top outlet of the bag dust collector is connected to the air inlet of the primary condenser, the air outlet of the primary condenser is connected to the air inlet of the secondary condenser, the air outlet of the secondary condenser is connected to the inlet of the circulation fan, the outlet of the circulation fan is connected to the air inlet of the carrier gas heater, and the air outlet of the carrier gas heater is connected to the circulating carrier gas inlet of the paddle dryer.

[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention has a simple structure, less auxiliary equipment, and low investment cost; the methanol moisture content of the metal oxide catalyst after drying is reduced from 50-60% to no more than 0.2%, the drying effect is good, continuous automatic drying can be realized, and the personnel operation cost is reduced; the amount of saturated steam can be adjusted according to the temperature of the material at the discharge port of the paddle dryer, thereby saving heat energy consumption and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is the flow chart of the drying system of the present invention. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0025] like Figure 1 The flow chart of the method for drying the metal oxide catalyst after washing with methanol is shown as follows:

[0026] The wet metal oxide catalyst (i.e., the metal oxide catalyst washed with methanol) from the upstream centrifuge enters the feed buffer bin 1 under the action of gravity, and is then forcibly fed into the drying chamber of the paddle dryer 3 through the double screw feeder 2; the methanol moisture content in the wet metal oxide catalyst is 50-60wt%.

[0027] Low-pressure saturated steam (0.5Mpag, 158°C) is continuously introduced into the jacket and double hollow hot shafts of the paddle dryer 3 to heat and dry the wet metal oxide catalyst through the wall; the double hollow hot shafts drive the hollow paddles to rotate and mesh with each other to prevent material deposition and agglomeration; the residence time of the wet metal oxide catalyst in the drying chamber of the paddle dryer 3 is 1.5 to 2.5 hours, and a metal oxide catalyst product with a methanol moisture content of ≤0.2wt% is obtained, and the average particle size of the product is 4 to 6μm.

[0028] The dry exhaust gas produced by the paddle dryer 3 is carried by the circulating carrier gas (methanol non-condensable steam + nitrogen) to the bag filter 4 for dust removal; the heating pipe of the bag filter 4 is passed through low-pressure saturated steam (0.5Mpag, 158°C) to keep the bag filter 4 warm and maintain the exhaust gas temperature at the outlet of the bag filter 4 at 80-90°C.

[0029] The tail gas after dust removal by the bag filter 4 enters the primary condenser 5. The primary condenser 5 uses circulating cooling water (0.45Mpag, 32°C) as a cold source to perform initial condensation on the tail gas at the outlet of the bag filter 4. The condensed liquid methanol is recovered into the methanol recovery tank 9.

[0030] The uncondensed tail gas from the primary condenser 5 is then sent to the secondary condenser 6. The secondary condenser 6 uses a refrigerant (0.45Mpag, -15°C) as a cold source to condense the outlet tail gas from the primary condenser 5 again. The liquid methanol condensed by the secondary condenser 6 is recovered to the methanol recovery tank 9.

[0031] The uncondensed methanol steam and nitrogen at the outlet of the secondary condenser 6 are pressurized to 1500-2000 Pa by the circulating fan 7 and then sent to the carrier gas heater 8 as circulating carrier gas for heating.

[0032] The carrier gas heater 8 introduces low-pressure saturated steam (0.5Mpag, 158°C) as a heat source to heat the circulating carrier gas to 110-120°C. The heated circulating carrier gas enters the drying chamber of the paddle dryer 3 through the circulating carrier gas inlet pipe for recycling.

[0033] A pressure measuring point 10 is provided on the circulating carrier gas inlet pipe of the blade dryer 3. The exhaust volume at the outlet of the circulating fan 7 is adjusted by the pressure at the measuring point to maintain a slight negative pressure of -180 to -200 Pa in the drying chamber of the blade dryer 3.

[0034] The discharge port of the paddle dryer 3 is provided with a temperature measuring point 11, and the flow rate of the low-pressure saturated steam is adjusted by measuring the temperature of the product at the discharge port to control the temperature of the metal oxide catalyst product to be 110-120°C.

[0035] An oxygen content online measuring point 12 is provided on the outlet exhaust pipe of the bag filter 4. By measuring the oxygen content, when the oxygen content is greater than or equal to 5%, low-pressure nitrogen is added at the outlet of the circulating fan to maintain the drying system in an inert environment.

[0036] Again Figure 1 The drying system for the metal oxide catalyst after methanol washing shown in the figure includes a feed buffer bin 1, a double screw feeder 2, a paddle dryer 3, a bag filter 4, a primary condenser 5, a secondary condenser 6, a circulating fan 7, a carrier gas heater 8, a methanol recovery tank 9, a pressure measuring point 10, a temperature measuring point 11 and an oxygen content measuring point 12.

[0037] The bottom outlet of the feed buffer bin 1 is connected to the feed port of the paddle dryer 3 via the double-screw feeder 2, the dry tail gas outlet of the paddle dryer 3 is directly connected to the inlet of the bag dust collector 4, the top outlet of the bag dust collector 4 is connected to the air inlet of the first-stage condenser 5, the air outlet of the first-stage condenser 5 is connected to the air inlet of the second-stage condenser 6, the air outlet of the second-stage condenser 6 is connected to the inlet of the circulating fan 7, the outlet of the circulating fan 7 is connected to the air inlet of the carrier gas heater 8, and the air outlet of the carrier gas heater 8 is connected to the circulating carrier gas inlet of the paddle dryer 3.

[0038] The condensate outlets of the primary condenser 5 and the secondary condenser 6 are both connected to the inlet of the methanol recovery tank 9, and the low-pressure nitrogen supplementary pipeline is connected to the outlet of the circulating fan. The pressure measuring point 10 is arranged on the circulating carrier gas inlet pipeline of the paddle dryer 3, the temperature measuring point 11 is arranged at the discharge port of the paddle dryer 3, and the oxygen content measuring point 12 is arranged on the outlet exhaust pipeline of the bag filter 4.

[0039] The invention adopts nitrogen closed circulation to dry the metal oxide catalyst containing methanol. The nitrogen consumption in the drying process is extremely small and the whole process is closed, which effectively reduces the nitrogen consumption and improves the safety of the metal oxide catalyst containing methanol in the drying process. The methanol moisture content of the metal oxide catalyst after drying is reduced from 50-60% to no more than 0.2%, and the drying effect is good.

[0040] The drying system of the present invention has a simple structure, few auxiliary equipment, and low investment cost. The methanol moisture content of the metal oxide catalyst after drying is reduced from 50-60% to no more than 0.2%, and the drying effect is good. Continuous automatic drying can be realized, and the operating cost of personnel can be reduced. The amount of saturated steam can be adjusted according to the temperature of the material at the discharge port of the paddle dryer, saving heat energy consumption and reducing production costs. A double-shaft paddle dryer is used for drying, and a slight negative pressure is maintained in the drying chamber to prevent dust from overflowing. The two hot shafts are meshed with each other to avoid the problems of metal oxide catalyst sticking to the wall, deposition, agglomeration, etc., and the catalyst wet material can be fully broken up and dried to ensure uniform product quality. A two-stage condenser is used to reduce the total heat transfer area, recover most of the methanol, and improve the drying capacity of the circulating carrier gas.

Claims

1. A method for drying a metal oxide catalyst after washing with methanol, characterized in that: The drying method is as follows: The wet metal oxide catalyst from the upstream centrifuge is fed into the drying chamber of the paddle dryer (3), and low-pressure saturated steam is passed into the paddle dryer (3) to indirectly heat and dry the wet metal oxide catalyst to obtain a dried metal oxide catalyst product; The dry exhaust gas generated by the paddle dryer (3) is carried by the circulating carrier gas to a bag filter (4) for dust removal; The tail gas after dust removal by the bag filter (4) enters the primary condenser (5), and the primary condenser (5) uses circulating cooling water as a cold source to perform primary condensation on the tail gas at the outlet of the bag filter (4), and the condensed liquid methanol is recovered; The uncondensed tail gas from the primary condenser 5 is then sent to the secondary condenser (6). The secondary condenser (6) uses a refrigerant as a cold source to condense the outlet tail gas from the primary condenser (5) again. The liquid methanol condensed by the secondary condenser (6) is recovered. The uncondensed tail gas at the outlet of the secondary condenser (6) is pressurized by a circulating fan (7) and then sent to a carrier gas heater (8) as a circulating carrier gas; low-pressure saturated steam is introduced into the carrier gas heater (8) as a heat source to heat the circulating carrier gas, and the heated circulating carrier gas enters the drying chamber of the paddle dryer (3) through a circulating carrier gas inlet pipe for cyclic use.

2. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: The wet content of methanol in the wet metal oxide catalyst is 50-60 wt %.

3. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: The low-pressure saturated steam is passed into the jacket and double hollow heat shafts of the paddle dryer (3) to heat and dry the wet metal oxide catalyst through the wall; the residence time of the wet metal oxide catalyst in the drying chamber of the paddle dryer (3) is 1.5 to 2.5 hours.

4. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: The heat tracing pipe of the bag filter (4) is passed through low-pressure saturated steam to keep the bag filter (4) warm, thereby maintaining the outlet tail gas temperature of the bag filter (4) at 80-90°C.

5. The method for drying the metal oxide catalyst after methanol washing according to claim 1, characterized in that: The uncondensed tail gas at the outlet of the secondary condenser (6) is used as a circulating carrier gas and pressurized to 1500-2000 Pa via a circulating fan (7).

6. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: The carrier gas heater (8) introduces low-pressure saturated steam as a heat source to heat the circulating carrier gas to 110-120°C.

7. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: A pressure measuring point (10) is provided on the circulating carrier gas inlet pipeline of the blade dryer (3), and the exhaust volume at the outlet of the circulating fan (7) is adjusted according to the pressure at the measuring point to maintain the negative pressure in the drying chamber of the blade dryer (3) at -180 to -200 Pa.

8. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: The discharge port of the paddle dryer (3) is provided with a temperature measuring point (11), and the flow rate of the low-pressure saturated steam is adjusted by measuring the temperature of the product at the discharge port, so that the temperature of the metal oxide catalyst product is controlled to be 110-120°C.

9. The method for drying a metal oxide catalyst after washing with methanol according to claim 1, characterized in that: An oxygen content online measuring point (12) is provided on the outlet tail gas pipeline of the bag filter (4). By measuring the oxygen content, when the oxygen content is greater than or equal to 5%, low-pressure nitrogen is supplemented at the outlet of the circulating fan (7).

10. A drying system for the drying method according to claim 1, characterized in that: It includes a feed buffer bin (1), a double screw feeder (2), a paddle dryer (3), a bag filter (4), a primary condenser (5), a secondary condenser (6), a circulating fan (7), a carrier gas heater (8) and a methanol recovery tank (9); The bottom outlet of the feed buffer bin (1) is connected to the feed port of the paddle dryer (3) via the double screw feeder (2); the dry tail gas outlet of the paddle dryer (3) is directly connected to the inlet of the bag filter (4); the top outlet of the bag filter (4) is connected to the air inlet of the primary condenser (5); the air outlet of the primary condenser (5) is connected to the air inlet of the secondary condenser (6); the air outlet of the secondary condenser (6) is connected to the inlet of the circulating fan (7); the outlet of the circulating fan (7) is connected to the air inlet of the carrier gas heater (8); and the air outlet of the carrier gas heater (8) is connected to the circulating carrier gas inlet of the paddle dryer (3).

Citation Information

Patent Citations

  • Nitrogen closed cycle drying and solvent recovery system

    CN101776372A

  • Efficient dedusting anti-condensation steam rotary drying process and lignite drying method

    CN103453753A

  • 2-benzothiazolethiol nitrogen circulation drying and solvent recovery method

    CN105004145A

  • Enclosed methanol recovery apparatus of vitamin C sodium salt continuous drying system

    CN201265998Y

  • Hollow blade drying and solvent recovery system

    CN202145080U