Preparation method of artificial rock core for measuring mechanical retention volume of polymer in porous medium

By preparing polytetrafluoroethylene artificial cores with specific structures, the problem that the prior art cannot determine the mechanical retention amount of polymers separately is solved, and the accurate analysis of the polymer oil flooding process and the improvement of the oil flooding effect are achieved.

CN119064099APending Publication Date: 2024-12-03ZHEJIANG OCEAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410837872.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing technology cannot determine the mechanical retention amount of polymers in porous media alone, and cannot distinguish the severity of adsorption and mechanical retention, which affects the design of polymer oil flooding process and the numerical simulation of reservoirs.

Method used

An artificial core is prepared by mixing a cementitious agent composed of polyester resin and curing agent with polytetrafluoroethylene powder in a specific proportion, and a core with a specific pore structure is formed through pre-pressing, drying and demolding steps, for measurement. Mechanical retention of polymer, separation adsorption and mechanical retention.

Benefits of technology

The mechanical retention amount of polymer in pores is achieved separately, which improves the success rate of polymer flooding, binary composite flooding and ternary composite flooding, and helps analyze the main retention control factors during polymer flooding.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of polymer oil displacement, in particular to a preparation method of an artificial rock core for measuring the mechanical retention volume of a polymer in a porous medium. The invention discloses a polytetrafluoroethylene composite material which comprises the following raw materials in percentage by mass: 86-95.5% of a cementing agent and 4.5-14% of polytetrafluoroethylene powder, the mixing mass ratio of the cementing agent to the polytetrafluoroethylene powder is 1: 300, and the cementing agent comprises 86-95.5% of polyester resin and 4.5-14% of a curing agent (ethylenediamine). The particle size of the polytetrafluoroethylene powder is 100-1200 meshes. Polymer molecules are not adsorbed on the pore surface of the prepared polytetrafluoroethylene porous medium, the adsorption effect of a polymer on the pore surface in the polymer oil displacement process can be eliminated, pores of different structures and sizes and corresponding flow fields can be simulated, and the mechanical retention volume of the polymer in the pores can be independently measured. Adsorption retention and mechanical retention can be effectively separated, the main control factor of retention of polymer molecules in a porous medium in the polymer flooding process is further analyzed, and the success rate of polymer flooding, binary combination flooding and ternary combination flooding is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer flooding, and more specifically, to a method for preparing an artificial core for determining the mechanical retention of a polymer in a porous medium. Background Art

[0002] Polymer flooding can increase the recovery rate by 5-10%, because adding polymer to the injected water can increase the viscosity of the water phase and reduce the permeability of the water phase. Due to the interaction between polymer molecules and porous media, some polymer molecules remain in the pores and on the surface of the porous media. Appropriate retention can improve the hydrodynamic field of the injected fluid and achieve a diversion effect, but if the retention is too large, the polymer loss will be too much, which will reduce the viscosity-increasing ability of the injected water, delay the advancement speed of the polymer and the oil-rich zone, and make the oil displacement effect worse. According to the retention mechanism, it can be divided into polymer adsorption and mechanical retention (mechanical capture and hydrodynamic retention). Adsorption is the adsorption and retention of polymers on the surface of rock pores due to physical and chemical effects such as electrostatic attraction and hydrogen bonding. Mechanical capture refers to the phenomenon that larger molecules in polymer molecules fail to pass through narrow flow channels and remain in narrow pores, causing blockage. It is generally difficult to measure it alone. The retention of polymer is an important basis for the design of polymer flooding process and a basic input parameter for reservoir numerical simulation. Therefore, it is very important to accurately measure and analyze the polymer retention and the main control factors of retention.

[0003] In the current literature, polymer retention is measured by injecting polymer solution into artificial core or natural core, and then measuring the concentration difference at the inlet and outlet to determine the retention after adsorption equilibrium; or adding small molecular tracers to the polymer solution, continuously injecting polymer into the core, monitoring the pressure change, sampling the produced mixed system, and analyzing the mass concentration of polymer and tracer respectively until the pressure of the mixed system is stable. At this time, the output concentration of polymer is equal to the injection concentration, and water drive is performed until no polymer is produced; then continue to continuously inject the polymer mixed system into the core, and sample the produced mixed system at the same time, analyze the mass concentration of polymer and tracer until the pressure of the mixed system is stable. However, these measurement results are the combined results of adsorption and mechanical retention, and it is impossible to distinguish the severity of the two; some people can measure the adsorption amount of polymer solution through indoor static adsorption experiments, but it does not conform to the adsorption law in the pores of actual reservoirs. Mechanical retention can only occur when the solution flows through porous media, and it is impossible to exist in static. Therefore, it is impossible to determine the main controlling factor of polymer retention.

[0004] During polymer flooding, binary composite flooding and ternary composite flooding, there is an interaction between polymer molecules and porous media, so that some polymer molecules remain in the pores and on the surface of porous media. Excessive retention will lead to poor polymer effect. According to the retention mechanism, it can be divided into polymer adsorption and mechanical retention (mechanical capture and hydrodynamic retention). Adsorption is the adsorption and retention of polymers on the surface of rock pores due to physical and chemical effects such as electrostatic attraction and hydrogen bonding. Mechanical capture refers to the phenomenon that larger molecules in polymer molecules fail to pass through narrow flow channels and remain in narrow pores, causing blockage. It is generally difficult to measure it alone. The retention of polymers is an important basis for the design of polymer flooding processes and a basic input parameter for numerical simulation of oil reservoirs. Therefore, it is very important to accurately measure and analyze the retention of polymers and the main control factors of retention. However, the existing public technology can only measure the sum of adsorption and mechanical retention of polymer molecules in porous media, and cannot measure the two separately. Summary of the invention

[0005] The present invention provides a method for preparing an artificial core for measuring the mechanical retention of a polymer in a porous medium, thereby improving the success rate of polymer flooding, binary composite flooding and ternary composite flooding.

[0006] In a first aspect, the present disclosure provides an artificial core for measuring the mechanical retention of a polymer in a porous medium, which is composed of the following raw materials in percentage by mass: a binder and polytetrafluoroethylene powder, the mixing mass ratio of the binder to the polytetrafluoroethylene powder is 1:300, the binder is composed of a polyester resin and a curing agent, the mass percentage of the polyester resin is 86% to 95.5%, and the mass percentage of the curing agent is 4.5% to 14%. .

[0007] Preferably, the particle size of the polytetrafluoroethylene powder is 100 to 1200 meshes.

[0008] In a second aspect, the present disclosure provides a method for preparing a core for determining the mechanical retention of a polymer in a porous medium, comprising the following steps:

[0009] (4) weighing a binder and polytetrafluoroethylene powder of different mesh sizes according to a proportion, mixing and stirring the components evenly so that each particle is coated with the binder to prepare a mixture;

[0010] (5) placing the mixture obtained in step (1) into an artificial core production mold, pre-pressing, then maintaining a constant pressure of 20 MPa for 120 min, and releasing the pressure and demolding after standing;

[0011] (1) After demoulding, the artificial core is placed in a drying oven, dried and solidified at a constant temperature, and naturally cooled to room temperature to obtain an artificial polytetrafluoroethylene core.

[0012] Preferably, in step (2), the pre-pressing condition is 4-10 MPa, and the pre-pressing time is 20 min.

[0013] Preferably, in step (3), the constant temperature drying condition is a constant temperature of 70-80° C. and the drying time is 10-12 h.

[0014] In a third aspect, the present disclosure provides an application of an artificial core for determining the mechanical retention of a polymer in a porous medium.

[0015] In summary, this application has the following beneficial effects:

[0016] 1. The pore surface of the polytetrafluoroethylene porous medium prepared in the present application does not adsorb polymer molecules, which can eliminate the adsorption effect of the polymer on the pore surface during the polymer flooding process, and can simulate pores of different structures and sizes and the corresponding flow fields, and separately determine the mechanical retention of the polymer in the pores, which can effectively separate the adsorption retention from the mechanical retention, and then analyze the main controlling factors of the retention of polymer molecules in the porous medium during the polymer flooding process, thereby improving the success rate of polymer flooding, binary composite flooding and ternary composite flooding;

[0017] 2. This application helps to study the matching relationship between the pore structure of the formation and the polymer molecular coils in the polymer solution, and provides a reference for the optimization of the polymer.

[0018] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not intended to limit the scope of protection of the present disclosure. DETAILED DESCRIPTION

[0019] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0020] Example

[0021] Example 1

[0022] (1) preparing a binder: the binder is prepared by mixing an epoxy resin and a curing agent according to mass percentage, wherein the mass percentage of the epoxy resin is 86% and the mass percentage of the curing agent is 4.5%;

[0023] (2) Mixing ingredients and loading into mold: 150 mesh polytetrafluoroethylene powder and binder are mixed evenly in proportion, with the mass ratio of binder to polytetrafluoroethylene powder being 1:300, and loaded into the rectangular through hole of the mold. The mold is placed on a vibration device to vibrate to eliminate the bridging of the mixture so that it forms a close point contact, and then the surface of the mixture is scraped flat with a scraping tool, and finally a pressing block is placed on the surface of the mixture;

[0024] (3) Pressing: Use bolts to fix the pressing block and the main mold, place the filled mold on the hydraulic press, pre-press for 10 minutes at a pressing pressure of 20 MPa, and then maintain a constant pressure of 20 MPa for 15 minutes.

[0025] (4) Heating and curing: Place the mold after decompression into a high-temperature oven and bake it at 80°C for 12 hours.

[0026] (5) Demolding: The core in the heated and solidified mold is taken out to finally obtain an artificial columnar core with a diameter of 2.5 cm and a length of 10 cm.

[0027] (6) Place the artificial core with a smooth cut end face into the core holder and connect the displacement device. The gas permeability of the core is measured to be 2000mD. A partially hydrolyzed polyacrylamide solution (hydrolysis degree of 32.5%) with a molecular weight of 15 million and a concentration of 1000mg / L prepared with distilled water is injected into the core prepared above. According to the patented method for determining the dynamic retention of the polymer in the core and the inaccessible pore volume, the mechanical retention of the polymer in the pore is determined to be 5.11μg / g.

[0028] (7) Using 150-200 mesh quartz sand prepared according to the above conditions, the artificial diameter of the core is 2.5 cm and the length is 10 cm. The gas permeability of the core is measured to be 1920 mD. A partially hydrolyzed polyacrylamide solution (hydrolysis degree is 32.5%) with a molecular weight of 15 million and a concentration of 1000 mg / L prepared with distilled water is injected into the core prepared above. According to the patented method for determining the dynamic retention of the polymer in the core and the inaccessible pore volume, the adsorption retention of the polymer in the pore is determined to be 8.39 μg / g. By comparison, the adsorption and mechanical retention are 3.28 μg / g and 5.11 μg / g, respectively.

[0029] Example 2

[0030] (1) preparing a binder: the binder is prepared by mixing an epoxy resin and a curing agent according to mass percentage, wherein the mass percentage of the epoxy resin is 95.5% and the mass percentage of the curing agent is 14%;

[0031] (2) Mixing ingredients and loading into mold: Mix 600-mesh polytetrafluoroethylene powder and binder in a uniform proportion, with the mass ratio of binder to polytetrafluoroethylene powder being 1:300, and load them into the rectangular through hole of the mold. Place the mold on a vibration device to vibrate to eliminate the bridging of the mixture and form a close point contact. Then, use a scraping tool to scrape the surface of the mixture flat, and finally place the briquette on the surface of the mixture.

[0032] (3) Pressing: Use bolts to fix the pressing block and the main mold, place the filled mold on the hydraulic press, pre-press for 10 minutes at a pressing pressure of 20 MPa, and then maintain a constant pressure of 20 MPa for 15 minutes.

[0033] (4) Heating and curing: Place the mold after decompression into a high-temperature oven and bake it at 80°C for 12 hours.

[0034] (5) Demolding: The core in the heated and solidified mold is taken out to finally obtain a 200-mesh artificial columnar core.

[0035] (6) Place the core with the cut end surface into the core holder and connect the displacement device. The gas permeability of the core is measured to be 1105 mD. A partially hydrolyzed polyacrylamide solution (hydrolysis degree of 32.5%) with a molecular weight of 15 million and a concentration of 1000 mg / L prepared with distilled water is injected into the core prepared above. According to the patented method for determining the dynamic retention and inaccessible pore volume of the polymer in the core, the mechanical retention of the polymer in the pore is determined to be 6.35 μg / g.

[0036] 7) Using 500-600 mesh quartz sand prepared according to the above conditions, the diameter of the artificial core is 2.5 cm and the length is 10 cm. The gas permeability of the core is measured to be 905 mD. A partially hydrolyzed polyacrylamide solution (hydrolysis degree is 32.5%) with a molecular weight of 15 million and a concentration of 1000 mg / L prepared with distilled water is injected into the core prepared above. According to the patented method for determining the dynamic retention and inaccessible pore volume of the polymer in the core, the adsorption retention of the polymer in the pore is determined to be 9.69 μg / g. By comparison, the adsorption and mechanical retention are 3.34 μg / g and 6.35 μg / g, respectively.

[0037] The above is only an exemplary embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. An artificial core for determining the mechanical retention of a polymer in a porous medium, characterized in that: The invention is composed of the following raw materials in percentage by mass: a binder and polytetrafluoroethylene powder, the mixing mass ratio of the binder to the polytetrafluoroethylene powder is 1:300, the binder is composed of a polyester resin and a curing agent, the mass percentage of the polyester resin is 86% to 95.5%, and the mass percentage of the curing agent is 4.5% to 14%.

2. The artificial core according to claim 1, characterized in that: The particle size of polytetrafluoroethylene powder is 100-1200 mesh.

3. The method for preparing a core for determining the mechanical retention of a polymer in a porous medium according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) weighing a binder and polytetrafluoroethylene powder of different mesh sizes according to a proportion, mixing and stirring the components evenly so that each particle is coated with the binder to prepare a mixture; (2) placing the mixture obtained in step (1) into an artificial core production mold, pre-pressing, then maintaining a constant pressure of 20 MPa for 120 min, and releasing the pressure and demolding after standing; (3) After demoulding, the artificial core is placed in a drying oven, dried and solidified at a constant temperature, and naturally cooled to room temperature to obtain an artificial polytetrafluoroethylene core.

4. The method for preparing a core for determining the mechanical retention of a polymer in a porous medium according to claim 3, characterized in that: In step (2), the pre-pressing condition is 4-10 MPa, and the pre-pressing time is 20 min.

5. The method for preparing a core for determining the mechanical retention of a polymer in a porous medium according to claim 3, characterized in that: In step (3), the constant temperature drying condition is a constant temperature of 70-80° C. and a drying time of 10-12 h.

6. The use of the artificial core according to any one of claims 1 to 5, characterized in that: Artificial cores are used to determine the mechanical retention of polymers in porous media.