Sensing layer containing self-assembled modified magnesium aluminum silicate and sensor and preparation method thereof

By using a self-assembled modified magnesium silicate sensor in glucose electrochemical sensor, the problems of initial sensor sensitivity consistency and stability are solved, achieving higher sensor accuracy and timeliness of use.

CN119064430AActive Publication Date: 2024-12-03JIANGXI SITOMAI MEDICAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411179744.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing glucose electrochemical sensors have challenges in the consistency and stability of initial sensitivity, which is difficult to meet the real-time monitoring of blood sugar, and it is difficult to ensure consistency of the sensor layer during mass production.

Method used

Using a sensing layer containing self-assembled modified magnesium aluminum silicate, the modified layer is formed by grafting the hydrophilic organic polymer on the working electrode of the flexible electrode, and the redox polymer, tool enzyme and Components such as magnesium and aluminum silicate are mixed to form a sensing layer solution, which is prepared by plasma treatment and buffer solution to ensure the uniformity and stability of the sensing layer.

Benefits of technology

Improve the consistency and stability of the sensor, reduce the loss of enzyme activity, ensure the consistency of the dropping area, enhance the accuracy and timeliness of the sensor, broaden the monitoring range, and reduce the interference of non-specific adsorbed proteins. Improves the timeliness of sensor use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064430A_ABST
    Figure CN119064430A_ABST
Patent Text Reader

Abstract

The invention discloses a sensing layer containing self-assembled modified magnesium aluminum silicate, a sensor containing the sensing layer and a preparation method of the sensor. A hydrophilic organic high-molecular polymer is grafted on a working electrode of a flexible electrode to obtain a modified layer, and the modified layer is coated with a sensing layer solution which can be self-assembled and modified with the modified layer. The sensing layer solution comprises a redox polymer, a tool enzyme, a cross-linking agent A and magnesium aluminum silicate, and the mass ratio of the redox polymer to the tool enzyme to the cross-linking agent A to the magnesium aluminum silicate is (15-40): (20-45): (5-30): (1-10). According to the invention, the hydrophilic organic high-molecular polymer is grafted on the surface of the working electrode, the hydrophilic organic high-molecular polymer can be self-assembled and compounded with the magnesium aluminum silicate, and the compounded and modified magnesium aluminum silicate has excellent gel performance and rheological property and good film forming effect, and can improve the consistency, stability and accuracy of the sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical sensors, and in particular to a sensing layer containing self-assembled modified magnesium aluminum silicate, a sensor thereof and a preparation method thereof. Background Art

[0002] At present, diabetes has become the third leading cause of death in my country after cardiovascular disease and cancer. There are nearly 130 million diabetes patients in China, ranking first in the world, and the prevalence of diabetes has increased exponentially. Diabetes is a chronic, systemic, metabolic disease caused by the long-term combined effects of genetic and environmental factors, characterized by elevated plasma glucose levels. It is mainly a disease caused by the disorder of sugar, fat, and protein metabolism caused by insufficient insulin secretion or dysfunction in the body, which affects normal physiological activities.

[0003] At present, the main method of testing blood sugar is to collect fingertip blood with in vitro glucose monitoring test strips. Patients need to prick their fingers several times a day to know the blood sugar value at a certain moment. This practice cannot reflect the real-time concentration changes and trend changes of blood sugar, and will also cause physical harm to patients. The continuous glucose monitoring system can display the user's blood sugar changes in real time during the use time. It is faster and easier to use, and provides detailed blood sugar data support for patients and medical treatment. The electrochemical reaction principle of the continuous glucose monitoring system is to measure the glucose concentration in the tissue fluid through the biological enzyme fixed on the sensor, such as glucose oxidase, which is implanted into the subcutaneous tissue. The electrical signal measured by glucose oxidase is converted into glucose concentration through the transmitter or receiver of CGMS and algorithm processing, and displayed on the display or software to form a glucose monitoring graph.

[0004] Glucose electrochemical sensors need to have high accuracy to meet the needs of real-time blood sugar monitoring, which poses a huge challenge to the consistency and stability of the sensor's initial sensitivity. Therefore, ensuring the consistency of the sensing layer is very important in the mass production of glucose electrochemical sensors. Summary of the invention

[0005] The purpose of the present invention is to provide a sensing layer and a sensor thereof with less agglomeration, high stability, high consistency and better control of drop coating area, as well as a preparation method thereof, in view of the above problems.

[0006] In order to achieve its purpose, the present invention adopts the following technical solution:

[0007] The first aspect of the present invention provides a sensing layer containing self-assembled modified magnesium aluminum silicate, which is used to prepare an electrochemical sensor, wherein the electrochemical sensor comprises a flexible electrode, and the sensing layer is formed by drop-coating a sensing layer solution that can be self-assembled and modified with the modified layer on a modified layer obtained by grafting a hydrophilic organic high molecular polymer on a working electrode of the flexible electrode;

[0008] The sensing layer solution comprises a redox polymer, a tool enzyme, a crosslinking agent A, and magnesium aluminum silicate, and the mass ratio of the redox polymer: the tool enzyme: the crosslinking agent A: the magnesium aluminum silicate is 15-40: 20-45: 5-30: 1-10.

[0009] Preferably, the hydrophilic organic high molecular polymer is selected from one or more of polyallylamine, polyethylene glycol, polyethyleneimine, polyamide-amine dendrimer, and poly(L-lysine);

[0010] The redox polymer is a redox polymer containing a transition metal, and the transition metal includes ruthenium, rhodium, and osmium;

[0011] The tool enzyme is selected from glucose dehydrogenase, glucose oxidase, uricase, lactate oxidase, and cholesterol oxidase;

[0012] The crosslinking agent A is selected from one or more of 1,4-butanediol diglycidyl ether, poly(dimethylsiloxane)-diglycidyl ether, glutaraldehyde, polyethylene glycol diglycidyl ether, tetraepoxypropyl-4,4-diaminodiphenylmethane or glycerol triglycidyl ether; preferably, the crosslinking agent A is polyethylene glycol diglycidyl ether with MW=200Da-5000Da, preferably MW=400Da.

[0013] Preferably, the mass ratio of the redox polymer: tool enzyme: cross-linking agent A: magnesium aluminum silicate is 35-40:20-35:20-30:4-10, preferably 35-40:25-35:25-30:5-10, more preferably 39:31:25:5;

[0014] The concentration of the redox polymer in the sensing layer solution is 2-5 mg / ml, preferably 2-4.5 mg / ml, and more preferably 3.0-4.5 mg / ml.

[0015] A second aspect of the present invention provides a method for preparing a sensing layer, wherein the sensing layer is a sensing layer containing self-assembled modified magnesium aluminum silicate as described in any one of the above items, and the preparation method comprises the following steps:

[0016] S1. Plasma-induced grafting of a hydrophilic organic polymer on a working electrode of a flexible electrode to obtain a modified layer;

[0017] S2, drop-coating the sensing layer solution onto the modified layer, and obtaining the sensing layer after cross-linking and curing.

[0018] The method for preparing the sensing layer mentioned above, wherein the modified layer is obtained by grafting a hydrophilic organic high molecular polymer on the working electrode of the flexible electrode by plasma initiation, comprises:

[0019] After the flexible electrode is treated with air plasma, the flexible electrode is immersed in a hydrophilic organic polymer aqueous solution with a concentration of 25 to 40 mg / mL and a temperature of 35 to 40° C. for 14 to 20 hours, and then the electrode is immersed in purified water for 20 to 30 hours and then taken out and dried for 30 to 40 minutes to form the modified layer on the working electrode of the flexible electrode.

[0020] The method for preparing the sensing layer, wherein the sensing layer solution is drop-coated onto the modified layer, and the sensing layer is obtained after cross-linking and curing, comprises the following steps:

[0021] S2.1, preparing a sensing layer solution: using solvent A to prepare a mixed solution of redox polymer, tool enzyme, crosslinking agent A, and magnesium aluminum silicate, and mixing them thoroughly to obtain a sensing layer solution; the solvent A is HEPES buffer or TES buffer; preferably, the concentration of the HEPES buffer is 5 to 20 mmol / L, and the pH is 7.5 to 8.2;

[0022] S2.2, preparing the sensing layer: drop-coating the prepared sensing layer solution onto the surface of the modified layer obtained in step S1, and cross-linking and curing at a temperature of 20 to 30° C. for 20 to 28 hours to obtain the sensing layer.

[0023] The third aspect of the present invention provides an electrochemical sensor, comprising: a flexible electrode, wherein the flexible electrode comprises a substrate, a working electrode, a counter electrode and a reference electrode, wherein:

[0024] The working electrode and the counter electrode are respectively arranged on both sides of the substrate, a dielectric layer is arranged on the side of the counter electrode away from the substrate, the reference electrode is arranged on the side of the working electrode away from the substrate, the dielectric layer is arranged between the working electrode and the reference electrode, and the dielectric layer is arranged on the side of the reference electrode away from the working electrode;

[0025] The surface of the working electrode has an exposed portion without a dielectric layer and a reference electrode, and the surface of the exposed portion is coated with a modified layer and a sensing layer in sequence;

[0026] It also includes a diffusion restriction layer, which wraps the sensing layer and the exposed parts of the dielectric layer, the reference electrode, and the counter electrode;

[0027] The modified layer and the sensing layer are the modified layer and the sensing layer described in any one of the above items, or are the modified layer and the sensing layer prepared according to the preparation method described in any one of the above items.

[0028] Preferably, the electrochemical sensor described above,

[0029] The diffusion limiting layer is derived from a polymer containing a nitrogen heterocyclic group and a crosslinking agent B;

[0030] The polymer containing nitrogen heterocyclic groups is selected from one or more of polyvinyl pyridine, polyvinyl pyrrole, polyvinyl pyridine-styrene copolymer, and polyvinyl pyridine-styrene copolymer modified with sulfonic acid groups;

[0031] The crosslinking agent B is selected from one or more of triglycidyl p-aminophenol, polyethylene glycol diglycidyl ether, tetraepoxypropyl-4,4'-diaminodiphenylmethane, tri(4-hydroxyphenyl)methane triglycidyl ether, and glycerol triglycidyl ether; preferably, the crosslinking agent B is polyethylene glycol diglycidyl ether with MW=200Da-5000Da, preferably MW=200Da;

[0032] The mass ratio of the polymer containing nitrogen heterocyclic groups to the crosslinking agent B is 7-9.9:0.1-3, preferably 9:1.

[0033] A fourth aspect of the present invention provides a method for preparing the electrochemical sensor, comprising the following steps:

[0034] S3, immersing the flexible electrode with the sensing layer obtained in step S2 in the outer membrane solution of the diffusion limiting layer, taking it out and curing it at a temperature of 20-35° C. to form a diffusion limiting layer, thereby obtaining the electrochemical sensor.

[0035] Preferably, step S3 comprises the following steps:

[0036] S3.1, preparing a diffusion-restricting layer outer membrane solution: using solvent B as solvent, preparing a mixed solution of a polymer containing nitrogen heterocyclic groups and a crosslinking agent B to obtain a diffusion-restricting layer outer membrane solution; the solvent B is a TES buffer solution, or a mixed solution of anhydrous ethanol and a HEPES buffer solution, preferably, the solvent B is obtained by mixing anhydrous ethanol and a HEPES buffer solution in a volume ratio of 2 to 10:1, the concentration of the HEPES buffer solution is 5 to 20 mmol / L, and the pH is 7.5 to 8.2; the concentration of the polymer containing nitrogen heterocyclic groups in the diffusion-restricting layer outer membrane solution is 40 to 80 mg / ml, preferably 50 to 70 mg / ml;

[0037] S3.2, preparing a diffusion-restricting layer: immersing the flexible electrode with a sensing layer obtained in step S2 in the diffusion-restricting layer outer membrane solution for multiple times, preferably 2 to 5 times, with an interval of 6 to 20 minutes between each time, and curing at a temperature of 20 to 35°C for 40 to 55 hours to form a diffusion-restricting layer to obtain the electrochemical sensor.

[0038] The redox polymer is a compound represented by the chemical structural formula (I):

[0039]

[0040] In formula (I), R 1 and R 2 Each independently represents a connecting bond, and R 1 and R 2 Same or different;

[0041] M represents a transition metal;

[0042] L 1 , L 2 , L 3 , L 4 , L 5 and L 6 Each independently represents a ligand, the ligand is a heterocyclic ring, and is coordinated with M through a heteroatom of the heterocyclic ring;

[0043] X represents a self-assembling group;

[0044] Y represents an anion,

[0045] a represents an integer; b represents the number of anions, which is a natural number; wherein b>a+1;

[0046] n, m and r represent natural numbers, and the sum of n, m and r is greater than 20;

[0047] e, g and f represent integers;

[0048] The self-assembling group is selected from one of the following groups which are substituted or unsubstituted by a substituent:

[0049]

[0050] Wherein, c and d are integers from 1 to 16;

[0051] The substituents of the self-assembling group are selected from benzyl bromide, benzyl chloride, -F, -Cl, -Br, -I, -NO 2 , -COOH, -SO 3 H, -NH 2 , -OH, an alkoxy group having 1 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms.

[0052] The beneficial effects of the present invention are:

[0053] First, a hydrophilic organic polymer is grafted onto the surface of the working electrode. The hydrophilic organic polymer will self-assemble and composite with magnesium aluminum silicate. The hydrophilic organic polymer is adsorbed between the magnesium aluminum silicate sheet structure, and there is a hydrogen bond between the two. The self-assembly of the two components will make the surface of magnesium aluminum silicate smoother. The composite modified magnesium aluminum silicate has excellent gel properties and rheological properties, which can make the sensing layer solution drip on the electrode surface with a consistent wetting angle, which can effectively reduce the agglomeration phenomenon between the enzyme and the redox polymer, avoid the formation of larger particle aggregates between particles, and evenly flatten the surface of the sensing layer to ensure the consistency of the drip area. A uniformly dispersed sensing layer can be obtained with a good film-forming effect, thereby reducing the loss of enzyme activity and improving the consistency, stability and accuracy of the sensor. The restricted diffusion layer on the sensor is biocompatible, which can broaden the sensor's monitorable range, reduce the interference of non-specific adsorbed proteins, and improve the timeliness and stability of the sensor. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 These are scanning electron micrographs of the sensing layer solution: (ab) scanning electron micrographs of magnesium aluminum silicate, (c) scanning electron micrograph of a mixture of magnesium aluminum silicate and polyethylene glycol, and (d) scanning electron micrograph of self-assembled modified magnesium aluminum silicate.

[0055] Figure 2 Detection results of the wetting angle of the sensing layer solution: (a) the wetting angle of the sensing layer solution of self-assembled modified magnesium aluminum silicate, (b) the wetting angle of the sensing layer solution mixed with magnesium aluminum silicate and polyethylene glycol, (c) the wetting angle of the sensing layer solution without polyethylene glycol, (d) the wetting angle of the sensing layer solution without magnesium aluminum silicate.

[0056] Figure 3 The following are electron micrographs of the sensing layer surface: (a) electron micrograph of the sensing layer surface after modification, (b) electron micrograph of the sensing layer surface mixed with magnesium aluminum silicate and polyethylene glycol, (c) electron micrograph of the sensing layer surface without magnesium aluminum silicate, and (d) electron micrograph of the sensing layer surface without polyethylene glycol.

[0057] Figure 4 These are the sensitivity consistency test results of the sensing layer: (a) sensitivity consistency of the sensing layer of self-assembled modified magnesium aluminum silicate, (b) sensitivity consistency of the sensing layer of a mixture of magnesium aluminum silicate and polyethylene glycol, (c) sensitivity consistency of the sensing layer without magnesium aluminum silicate, and (d) sensitivity consistency of the sensing layer without polyethylene glycol.

[0058] Figure 5The following are the 15-day stability test results of the sensing layer: (a) 15-day stability of the modified sensing layer, (b) 15-day stability of the sensor mixed with magnesium aluminum silicate and polyethylene glycol, (c) 15-day stability of the sensor without magnesium aluminum silicate in the sensing layer, and (d) 15-day stability of the sensor without polyethylene glycol in the sensing layer.

[0059] Figure 6 It is the linear spectrum (0-25mM) of the sensor containing modified magnesium aluminum silicate in the sensing layer.

[0060] Figure 7 It is a linear spectrum (0-25mM) of the sensor mixed with magnesium aluminum silicate and polyethylene glycol.

[0061] Figure 8 It is the linear spectrum (0-25mM) of the sensor without magnesium aluminum silicate in the sensing layer.

[0062] Fig. 9 It is the linear spectrum of the sensor without polyethylene glycol in the sensing layer (0-25mM).

[0063] Fig.10 It is a human experimental map of a sensor containing modified magnesium aluminum silicate in the sensing layer in an implantable continuous glucose monitoring system.

[0064] Fig.11 This is a human experimental graph of a sensor mixed with magnesium aluminum silicate and polyethylene glycol in an implantable continuous glucose monitoring system.

[0065] Fig.12 This is a human experimental graph of a sensor without magnesium aluminum silicate in the sensing layer in an implantable continuous glucose monitoring system.

[0066] Fig.13 This is a human experimental map of a sensor without polyethylene glycol in the sensing layer in an implantable continuous glucose monitoring system.

[0067] Fig.14 Schematic diagram of the structure of a conventional flexible electrode (a) and the sensor of the present invention (b). DETAILED DESCRIPTION

[0068] The present invention will be further described below in conjunction with embodiments, but the present invention is not limited thereto.

[0069] The experimental methods in the following examples are conventional methods unless otherwise specified.

[0070] Main materials and reagents:

[0071] Glucose oxidase: CAS number: 9001-37-0, 120U / mg.

[0072] Polyethylene glycol diglycidyl ether: CAS number: 26403-72-5.

[0073] Magnesium aluminum silicate: white composite colloidal substance, CAS No.: 71205-22-6, models include but are not limited to HS-100, HV-101, HV-102, YK-R, YK-101, YK-200. Model HV-101 is used in the examples and comparative examples of the present invention.

[0074] Sulfonic acid group-modified polyvinylpyridine-styrene copolymer: prepared according to the method in US Pat. No. 6,932,894B2.

[0075] Redox polymer: The redox polymers used in Examples 1-5 and Comparative Examples 1-3 are all self-assembled redox polymers a prepared in Example 1 of Chinese Patent ZL 202210837308.6 (CN 115215953 B), and their chemical structure is shown in Formula (II):

[0076]

[0077] Example 1

[0078] 1. Electrode pretreatment:

[0079] The flexible electrode was treated with air plasma (flow rate 150 mL / min, power 100 W, vacuum degree 50 Pa) for 5 minutes. The electrode was then immersed in a 30 mg / mL polyethylene glycol aqueous solution (37° C.) for 16 hours, and then immersed in purified water for 24 hours and then taken out and dried for 35 minutes to form a modified layer on the flexible electrode, i.e., a flexible electrode with a modified layer. Specifically, the modified layer was formed on the working electrode of the flexible electrode.

[0080] 2. Preparation of Sensing Layer:

[0081] Using 10mmol / L HEPES (4-hydroxyethylpiperazineethanesulfonic acid) buffer at pH=8.0 as solvent, 5mg / mL redox polymer, 40mg / mL glucose oxidase, 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da) (as a cross-linking agent) and 5mg / mL magnesium aluminum silicate were prepared respectively, and the four prepared solutions were mixed, and the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether, and magnesium aluminum silicate in the mixed solution was 39%:31%:25%:5%. After vortexing for 30 minutes, a sensing layer solution was obtained, in which the concentration of the redox polymer was 3.69mg / ml. 0.2μL was evenly dropped onto the modified layer on the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., a flexible electrode with a sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0082] Magnesium aluminum silicate itself is an inorganic substance with a lamellar structure. The lamellar structure is combined with the hydroxyl groups (-OH) of the hydrophilic grafted polymer (such as polyethylene glycol) by hydrogen bonding forces. Under certain conditions, it spontaneously organizes or aggregates to form a relatively ordered and stable structure. This process is usually called self-assembly, that is, the process of spontaneous combination due to various chemical bonding forces.

[0083] 3. Preparation of the outer membrane of the diffusion-restricting layer:

[0084] Anhydrous ethanol and 10mmol / L HEPES buffer with pH=8.0 were mixed in a volume ratio of 4:1 as solvents to prepare 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0085] Example 2

[0086] 1. Electrode pretreatment:

[0087] The flexible electrode was treated with air plasma (flow rate 150 mL / min, power 100 W, vacuum degree 50 Pa) for 5 minutes. The electrode was then immersed in a 25 mg / mL polyethylene glycol solution (36° C.) for 20 hours, and then immersed in purified water for 20 hours and then taken out and dried for 30 minutes to form a modified layer on the flexible electrode, i.e., a flexible electrode with a modified layer. Specifically, the modified layer was formed on the working electrode of the flexible electrode.

[0088] 2. Preparation of Sensing Layer:

[0089] Using 20mmol / L HEPES buffer at pH=7.5 as solvent, 5mg / mL redox polymer, 40mg / mL glucose oxidase, 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da) (as a cross-linking agent) and 5mg / mL magnesium aluminum silicate were prepared respectively, and the four prepared solutions were mixed, and the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether, and magnesium aluminum silicate in the mixed solution was 40%:45%:14%:1%, and after vortexing for 30 minutes, a sensing layer solution was obtained, in which the concentration of the redox polymer was 4.05mg / ml. 0.2μL was evenly dropped onto the modified layer on the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., a flexible electrode with a sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0090] 3. Preparation of the outer membrane of the diffusion-restricting layer:

[0091] Anhydrous ethanol and 5mmol / L HEPES buffer with pH=8.2 were mixed in a volume ratio of 4:1 as solvents to prepare 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0092] Example 3

[0093] 1. Electrode pretreatment:

[0094] The flexible electrode was treated with air plasma (flow rate 150 mL / min, power 100 W, vacuum degree 50 Pa) for 5 minutes. The electrode was then immersed in a 40 mg / mL polyethylene glycol solution (39° C.) for 14 hours, and then immersed in purified water for 30 hours and then taken out and dried for 40 minutes to form a modified layer on the flexible electrode, i.e., a flexible electrode with a modified layer. Specifically, the modified layer was formed on the working electrode of the flexible electrode.

[0095] 2. Preparation of Sensing Layer:

[0096] Using 5mmol / L HEPES buffer at pH=8.2 as solvent, 5mg / mL redox polymer, 40mg / mL glucose oxidase, 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da) (as a cross-linking agent) and 5mg / mL magnesium aluminum silicate were prepared respectively, and the four prepared solutions were mixed, and the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether, and magnesium aluminum silicate in the mixed solution was 15%:45%:30%:10%. After vortexing for 30 minutes, a sensing layer solution was obtained, in which the concentration of the redox polymer was 2.05mg / ml. 0.2μL was evenly dropped onto the modified layer on the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., a flexible electrode with a sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0097] 3. Preparation of the outer membrane of the diffusion-restricting layer:

[0098] Anhydrous ethanol and 15mmol / L HEPES buffer with a pH value of 7.8 were mixed in a volume ratio of 4:1 as solvents to prepare a 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and a 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0099] Example 4

[0100] 1. Electrode pretreatment:

[0101] The flexible electrode was treated with air plasma (flow rate 150 mL / min, power 100 W, vacuum degree 50 Pa) for 5 minutes. The electrode was then immersed in a 35 mg / mL polyethylene glycol solution (40° C.) for 16 hours, and then immersed in purified water for 26 hours and then taken out and dried for 30 minutes to form a modified layer on the flexible electrode, i.e., a flexible electrode with a modified layer. Specifically, the modified layer was formed on the working electrode of the flexible electrode.

[0102] 2. Preparation of Sensing Layer:

[0103] Using 15mmol / L HEPES buffer at pH=7.7 as solvent, 5mg / mL redox polymer, 40mg / mL glucose oxidase, 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da) (as a cross-linking agent) and 5mg / mL magnesium aluminum silicate were prepared respectively, and the four prepared solutions were mixed, and the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether, and magnesium aluminum silicate in the mixed solution was 40%:20%:30%:10%. After vortexing for 30 minutes, a sensing layer solution was obtained, in which the concentration of the redox polymer was 3.42mg / ml. 0.2μL was evenly dropped onto the modified layer on the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., a flexible electrode with a sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0104] 3. Preparation of the outer membrane of the diffusion-restricting layer:

[0105] Anhydrous ethanol and 20mmol / L HEPES buffer with a pH value of 7.5 were mixed in a volume ratio of 4:1 as a solvent, and a 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and a 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution were prepared respectively. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and the polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, and the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0106] Example 5

[0107] 1. Electrode pretreatment:

[0108] The flexible electrode was treated with air plasma (flow rate 150 mL / min, power 100 W, vacuum degree 50 Pa) for 5 minutes. The electrode was then immersed in a 32 mg / mL polyethylene glycol solution (35° C.) for 17 hours, and then immersed in purified water for 26 hours and then taken out and dried for 40 minutes to form a modified layer on the flexible electrode, i.e., a flexible electrode with a modified layer. Specifically, the modified layer was formed on the working electrode of the flexible electrode.

[0109] 2. Preparation of Sensing Layer:

[0110] Using 20mmol / L HEPES buffer at pH=8.2 as solvent, 5mg / mL redox polymer, 40mg / mL glucose oxidase, 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da) (as a cross-linking agent) and 5mg / mL magnesium aluminum silicate were prepared respectively, and the four prepared solutions were mixed, and the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether, and magnesium aluminum silicate in the mixed solution was 40%:45%:5%:10%. After vortexing for 30 minutes, a sensing layer solution was obtained, in which the concentration of the redox polymer was 3.53mg / ml. 0.2μL was evenly dropped onto the modified layer on the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., a flexible electrode with a sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0111] 3. Preparation of the outer membrane of the diffusion-restricting layer:

[0112] Anhydrous ethanol and 20mmol / L HEPES buffer with a pH of 8.2 were mixed in a volume ratio of 4:1 as a solvent to prepare a 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and a 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0113] Comparative Example 1

[0114] 1. Electrode pretreatment:

[0115] The flexible electrode was treated with air plasma (flow rate 150 mL / min, power 100 W, vacuum degree 50 Pa) for 5 minutes. The electrode was then immersed in a 30 mg / mL polyethylene glycol aqueous solution (37° C.) for 16 hours, and then immersed in purified water for 24 hours and then taken out and dried for 35 minutes to form a modified layer on the flexible electrode, i.e., a flexible electrode with a modified layer. Specifically, the modified layer was formed on the working electrode of the flexible electrode.

[0116] 2. Preparation of sensing layer without magnesium aluminum silicate:

[0117] 8mmol / L HEPES buffer at pH=7.5 was used as solvent to prepare 5mg / mL redox polymer, 40mg / mL glucose oxidase and 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da), and the prepared solution was mixed, the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether and magnesium aluminum silicate in the mixed solution was 39%:31%:30%, and the sensing layer solution was obtained after vortex oscillation for 30 minutes, wherein the concentration of the redox polymer was 3.99mg / ml. 0.2μL was evenly dropped onto the modified layer on the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., the flexible electrode with the sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0118] 3. Preparation of the outer membrane of the diffusion-restricting layer:

[0119] Anhydrous ethanol and 12mmol / L HEPES buffer with a pH value of 7.8 were mixed in a volume ratio of 4:1 as solvents to prepare a 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and a 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0120] Comparative Example 2

[0121] 1. Preparation of sensing layer without hydrophilic polymer grafting:

[0122] Using 10mmol / L HEPES buffer at pH=8.0 as solvent, 5mg / mL redox polymer, 40mg / mL glucose oxidase, 25mg / mL polyethylene glycol diglycidyl ether (MW=400Da) and 5mg / mL magnesium aluminum silicate were prepared, and the four prepared solutions were mixed, and the mass ratio of redox polymer, solute glucose oxidase, polyethylene glycol diglycidyl ether and magnesium aluminum silicate in the mixed solution was 40%:45%:5%:10%, and after vortex oscillation for 30 minutes, a sensing layer solution was obtained, in which the concentration of the redox polymer was 3.53mg / ml. 0.2μL was evenly dripped onto the working electrode surface of the flexible electrode using a microinjector (1μL), and the sensing layer, i.e., a flexible electrode with a sensing layer, was obtained after cross-linking and curing at an oven temperature of 25°C for 24 hours.

[0123] 2. Preparation of the outer membrane of the diffusion-restricting layer:

[0124] Anhydrous ethanol and 10mmol / L HEPES buffer with pH=8.0 were mixed in a volume ratio of 4:1 as solvents to prepare 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0125] Comparative Example 3

[0126] 1. Preparation of sensing layer mixed with magnesium aluminum silicate and polyethylene glycol:

[0127] A mixed solution of magnesium aluminum silicate and polyethylene glycol was prepared with a 5 mmol / L HEPES buffer solution at pH=8.2 as a solvent, wherein the concentration of magnesium aluminum silicate in the mixed solution was 5 mg / mL and the concentration of polyethylene glycol was 30 mg / mL. In addition, 5 mg / mL redox polymer, 40 mg / mL glucose oxidase, 25 mg / mL polyethylene glycol diglycidyl ether (MW=400Da) and a mixed solution of magnesium aluminum silicate and polyethylene glycol were mixed, wherein the mass ratio of the redox polymer, the solute glucose oxidase, the polyethylene glycol diglycidyl ether, and the magnesium aluminum silicate and polyethylene glycol in the mixed solution was 42%:45%:5%:8%, and the sensing layer solution was obtained after vortex oscillation for 30 minutes, wherein the concentration of the redox polymer was 4.22 mg / mL. Use a microinjector (1 μL) to transfer 0.2 μL of the solution and evenly apply it to the working electrode surface of the flexible electrode. After cross-linking and curing for 24 hours in an oven at 25°C, the sensing layer, i.e., the flexible electrode having the sensing layer, is obtained.

[0128] 2. Preparation of the outer membrane of the diffusion-restricting layer:

[0129] Anhydrous ethanol and 5mmol / L HEPES buffer with pH=8.2 were mixed in a volume ratio of 4:1 as solvents to prepare 90mg / mL sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and 20mg / mL polyethylene glycol diglycidyl ether (MW=200Da) solution. The prepared sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution and polyethylene glycol diglycidyl ether (MW=200Da) solution were mixed to obtain a diffusion-restricting layer outer membrane solution, wherein the mass ratio of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer solution to the polyethylene glycol diglycidyl ether in the mixed solution was 90%:10%, wherein the concentration of the sulfonic acid group-modified polyvinyl pyridine-styrene copolymer was 60mg / mL. The flexible electrode with the sensing layer is immersed in the outer membrane solution of the diffusion limiting layer for 10 seconds each time. After taking it out, it is dried for 10 minutes to evaporate the solvent, and then the immersion operation is repeated for a total of 4 times. After completion, it is cured in an oven at a temperature of 25°C for 48 hours to obtain the desired sensor.

[0130] Comparison of Examples 1-5 and Comparative Examples 1-3

[0131] In Examples 1-5, except for the different mass ratios of the raw materials in the sensing layer (as shown in Table 1), the other preparation methods are exactly the same. The mass ratios of Examples 1-5 and Comparative Examples 1-2 in Table 1 are the mass ratios of redox polymer: glucose oxidase: polyethylene glycol diglycidyl ether: magnesium aluminum silicate in the sensing layer; the mass ratio of Comparative Example 3 is the mass ratio of redox polymer: glucose oxidase: polyethylene glycol diglycidyl ether: magnesium aluminum silicate-polyethylene glycol in the sensing layer.

[0132] The difference between Comparative Example 1 and Example 1 is that magnesium aluminum silicate is not added when preparing the sensing layer, and the other steps are exactly the same. The difference between Comparative Example 2 and Example 5 is that step "1. Electrode pretreatment" of Example 5 is not performed, and the sensing layer is directly prepared on the electrode, and the other steps are exactly the same. The difference between Comparative Example 3 and Example 5 is that the hydrophilic organic high molecular polymer (polyethylene glycol) is not grafted separately, but polyethylene glycol is mixed with magnesium aluminum silicate when preparing the sensing layer, and the mass ratio of the substances is also different.

[0133] Table 1

[0134] Example Mass ratio of each substance in the sensing layer Example 1 39:31:25:5 Example 2 40:45:14:1 Example 3 15:45:30:10 Example 4 40:20:30:10 Example 5 40:45:5:10 Comparative Example 1 39:31:30:0 Comparative Example 2 40:45:5:10 Comparative Example 3 42:45:5:8

[0135] Example 6: Scanning electron microscope observation and wetting angle test

[0136] The test objects are as follows:

[0137] The modified sensing layer solution in this embodiment refers to the sensing layer solution in Example 1. During the test, 2-3 drops of the sensing layer solution are applied to the electrode that has completed the electrode pretreatment in step 1 of Example 1, and then the wetting angle of the droplets is measured using an SDC-BOS wetting angle tester. The sensing layer solution mixed with magnesium aluminum silicate and polyethylene glycol in Table 3 is the sensing layer solution of Comparative Example 3; the sensing layer solution without hydrophilic polymer in Table 4 is the sensing layer solution of Comparative Example 2; the sensing layer solution without magnesium aluminum silicate in Table 5 is the sensing layer solution of Comparative Example 1.

[0138] The magnesium aluminum silicate solution, the mixed solution of magnesium aluminum silicate and polyethylene glycol, and the modified sensing layer solution were observed by scanning electron microscopy: the hydrophilic organic polymer polyethylene glycol of the present invention is grafted on the surface of the working electrode and self-assembles with magnesium aluminum silicate. It can be seen that magnesium aluminum silicate has a lamellar structure. Figure 1 (ab), while the lamellar blocks of magnesium aluminum silicate mixed with polyethylene glycol are larger ( Figure 1 c), the structure is tighter, and its gelling and rheological properties are poorer. Figure 1 d indicates that polyethylene glycol is adsorbed between the self-assembled modified magnesium aluminum silicate sheet structures, and there is a hydrogen bond between the two. The self-assembly of the two components will make the surface of magnesium aluminum silicate smoother, thereby having excellent gel properties and rheological properties, which can effectively reduce the agglomeration phenomenon between the enzyme and the redox polymer and reduce the loss of enzyme activity.

[0139] The excellent rheological properties allow the sensing layer solution to have a smaller wetting angle when dripped on the electrode surface. The SDC-BOS wetting angle tester was used to measure the solution dripped on the electrode surface. Figure 2 As shown, the wetting angle formed by the sensing layer solution after modification ( Figure 2 a) is significantly smaller than the wetting angle of the sensing layer solution mixed with magnesium aluminum silicate and polyethylene glycol ( Figure 2b), Wetting angle of the sensing layer solution without polyethylene glycol ( Figure 2 c) and the wetting angle of the sensing layer solution without magnesium aluminum silicate ( Figure 2 d). The results in Table 2 show that the wetting angles of the modified solutions after multiple tests are highly consistent. By comparing Tables 3, 4 and 5, it can be seen that the wetting angle of the sensing layer solution formed by self-assembly modification is better than that of the other three sensing layer solutions, which can produce a better film-forming effect, thereby improving the consistency and stability of the sensor.

[0140] Table 2 Wetting angle of the modified sensing layer solution

[0141] Number of experiments Wetting angle (mean) Wetting angle (left) Wetting angle (right) 1 45.747 45.434 46.06 2 45.4165 45.598 45.235 3 45.574 45.789 45.359 4 45.5225 45.821 45.224 5 45.473 45.198 45.748 6 45.3715 45.532 45.211 7 45.664 45.875 45.453 8 45.6165 45.321 45.912 9 45.5025 45.582 45.423 10 46.2545 46.638 45.871

[0142] Table 3 Wetting angle of the sensing layer solution mixed with magnesium aluminum silicate and polyethylene glycol

[0143] Number of experiments Wetting angle (mean) Wetting angle (left) Wetting angle (right) 1 54.169 54.236 54.102 2 56.7625 56.954 56.571 3 55.21 54.099 56.321 4 54.847 55.457 54.237 5 55.745 54.644 56.846 6 57.938 57.187 58.689 7 56.0715 55.798 56.345 8 54.343 54.741 53.945 9 57.994 57.663 58.325 10 57.3455 57.142 57.549

[0144] Table 4 Wetting angle of solution without hydrophilic polymer sensing layer

[0145] Number of experiments Wetting angle (mean) Wetting angle (left) Wetting angle (right) 1 102.976 103.254 102.698 2 99.2605 98.045 100.476 3 104.2665 103.174 105.359 4 101.2605 102.157 100.364 5 100.3375 99.654 101.021 6 100.892 100.635 101.149 7 102.067 103.089 101.045 8 104.558 103.671 105.445 9 98.3355 99.112 97.559 10 103.3715 103.044 103.699

[0146] Table 5 Wetting angle of the solution without magnesium aluminum silicate sensing layer

[0147]

[0148]

[0149] The solutions in Tables 2-5 were respectively dripped onto the working electrode surface of the electrode, and after cross-linking and curing (25° C.) for 24 hours, an electrode with a sensing layer was obtained, which was observed under a scanning electron microscope: the modified sensing layer of the present invention ( Figure 3 a) The film-forming effect is better, the surface of the sensing layer is flat and porous, and there are few cracks in the film layer; while the sensing layer mixed with magnesium aluminum silicate and polyethylene glycol ( Figure 3 b) There are many surface cracks; Figure 3 c and Figure 3 d proves that the sensing layer lacking magnesium aluminum silicate or polyethylene glycol has serious agglomeration phenomenon.

[0150] Example 7: Sensor performance test

[0151] In this embodiment, the sensor containing modified magnesium aluminum silicate in the sensing layer refers to the sensor prepared in the above embodiment, the sensor without magnesium aluminum silicate in the sensing layer refers to the sensor prepared in Comparative Example 1, the sensor without polyethylene glycol in the sensing layer refers to the sensor prepared in Comparative Example 2, and the sensor mixed with magnesium aluminum silicate and polyethylene glycol refers to the sensor prepared in Comparative Example 3.

[0152] 1. Sensitivity consistency test of the sensing layer

[0153] The sensor prepared in Example 1 and the comparative example was tested: the part of the sensor covering the outer membrane of the diffusion-restricting layer (5 mm) was immersed in a transparent sample bottle containing 10 mM glucose solution, and the solution was kept at a constant temperature of 37°C. The sensor was connected to the Chenhua 1000c electrochemical workstation, and the sensor sensitivity was tested using the chronoamperometry (it), and the curve of the test current value changing with time was plotted. Figure 4 c is the sensitivity difference spectrum of the sensor without magnesium aluminum silicate in the sensing layer. The sensitivity range of the sensor in 10mM sugar solution is 0.78-1.85nA / mM, and the coefficient of variation CV is 19.27%. Figure 4 b shows the coefficient of variation of the sensor mixed with magnesium aluminum silicate and polyethylene glycol, CV, which is 14.08%. Figure 4 a. The sensitivity distribution range of the sensor with modified magnesium aluminum silicate added to the sensing layer is more concentrated, within the range of 1.01-1.48nA / mM, and the coefficient of variation CV is 9.81%. It can be seen that modified magnesium aluminum silicate can effectively reduce the agglomeration phenomenon between enzymes and redox polymers, which helps to obtain a uniformly dispersed sensing layer, thereby improving the consistency of the sensitivity of the biosensor.

[0154] 2. Sensing layer stability test

[0155] The sensor prepared in Example 2 and the comparative example was tested: the part of the sensor covering the outer membrane of the diffusion-restricting layer (5 mm) was immersed in a transparent sample bottle containing 10 mM glucose solution, and the solution was kept at a constant temperature of 37° C. The sensor was connected to the Chenhua 1000c electrochemical workstation, and the sensor stability test was performed using the chronoamperometry (it), and the curve of the current value changing with time within 15 days was tested. Figure 5 The glucose sensor with modified magnesium aluminum silicate added to the middle sensing layer was tested for stability for 15 days in vitro. Taking the first day as the benchmark, the current value decayed by ≤13% within 15 days. The current decay of the sensor mixed with magnesium aluminum silicate and polyethylene glycol reached 23%, and the glucose sensor without magnesium aluminum silicate or polyethylene glycol added to the sensing layer was tested for stability in vitro. The current of the sensor decayed by 34% and 32% respectively in 15 days. Magnesium aluminum silicate has good adsorption properties and can expose more enzyme active sites with its special crystal structure - silicon-oxygen tetrahedron. The modified magnesium aluminum silicate can make the sensing layer solution drop coated on the electrode surface with a consistent wetting angle, which has a better film-forming effect, thereby improving the stability of the sensor.

[0156] 3. Sensor Linear Spectrum

[0157] The sensor prepared in Example 3 and the comparative example was tested: the part of the sensor covering the outer membrane of the diffusion-restricting layer (5 mm) was immersed in a transparent sample bottle containing PBS buffer, and the solution was kept at a constant temperature of 37°C. The sensor was connected to the Chenhua 1000c electrochemical workstation, and the sensor linearity test was performed using the chronoamperometry (it). After each test period of the sensor, the solution was replaced with a glucose solution with an increasing concentration gradient (0-25 mM). Figure 6 The linear spectrum of the sensor with modified magnesium aluminum silicate in the sensing layer is shown in Figure 2. Figure 7 This is the linear spectrum of the sensor mixed with magnesium aluminum silicate and polyethylene glycol. Figure 8 and 9 The linear spectra of sensors without magnesium aluminum silicate and polyethylene glycol in the sensing layer are shown in the figure. As shown in the figure, the current value of the sensor modified with magnesium aluminum silicate in the glucose solution with a concentration of 0-25mM changes significantly with the solution concentration gradient, and the linear relationship is very good. The linear fitting coefficient R 2 Reach 99.7%. Linear fitting coefficient R of the sensor mixed with magnesium aluminum silicate and polyethylene glycol 2 The linear relationship of the sensor without magnesium aluminum silicate or polyethylene glycol in the sensing layer is poor in the glucose solution with a concentration of 0-25 mM, and the current gradient change is not obvious. The linear fitting coefficient R 2 Only 96.5% and 96.3%.

[0158] 4. Human Experimental Map of Sensors in Implantable Continuous Glucose Monitoring Systems

[0159] The detection object is the sensor prepared in Example 4 and the comparative example: the biosensor covered with the outer membrane of the diffusion-restricting layer is applied to the implantable continuous glucose monitoring system, such as Fig.10 As shown. In the 14-day continuous human test, the sensitivity of the sensor was very stable, and the dynamic glucose concentration (curve) monitored by it did not decay, which was highly consistent with the results of fingertip blood glucose detection (dots). At the same time, the human test results were compared with a foreign brand of dynamic blood glucose meter. The blood glucose value of the dynamic blood glucose meter was very close to the dynamic glucose concentration (curve), and the monitoring results of the two were consistent. Fig.11 The sensor made of magnesium aluminum silicate and polyethylene glycol showed that only part of the data in the body could match the fingertip blood sugar value, and there was still a gap compared with competing products. Fig.12 and 13 In human trials, the blood glucose values ​​monitored by biosensors that do not contain magnesium aluminum silicate or polyethylene glycol are significantly different from those measured by fingertip blood glucose and a foreign brand of continuous blood glucose meter, and the monitoring time can only last for 7-10 days.

[0160] Example 8: Electrochemical sensor structure of the present invention

[0161] Conventional flexible electrode structures such as Fig.14 As shown in a, it is prepared by stacking electrodes.

[0162] The biosensor for electrochemical detection of the present invention is prepared according to the method of Examples 1-5, and is obtained by sequentially loading a modification layer, a sensing layer, and a diffusion restriction layer on the basis of a conventional flexible electrode. The structure of the biosensor of the present invention is as follows: Fig.14 As shown in b, it includes: a flexible electrode, the flexible electrode includes a substrate, a working electrode, a counter electrode and a reference electrode, wherein the working electrode and the counter electrode are respectively arranged on both sides of the substrate, and a dielectric layer is arranged on the side of the counter electrode away from the substrate; a reference electrode is arranged on the side of the working electrode away from the substrate, a dielectric layer is arranged between the working electrode and the reference electrode, and a dielectric layer is arranged on the side of the reference electrode away from the working electrode, and the surface of the working electrode has an exposed portion without a dielectric layer and a reference electrode, and the surface of the exposed portion is loaded with a modified layer and a sensing layer in sequence from the inside to the outside, and a diffusion restriction layer is also arranged on the surface of the flexible electrode, and the diffusion restriction layer wraps the sensing layer and the exposed portions of the dielectric layer, the reference electrode and the counter electrode.

[0163] The present invention does not particularly limit the materials of the working electrode, the counter electrode and the reference electrode, and they may be the working electrode, the counter electrode and the reference electrode commonly used in the field of electrochemical sensor technology. Specifically, the conductive materials of the working electrode, the counter electrode and the reference electrode may be one or a combination of two or more of graphite, graphene, nanocarbon, carbon nanotubes and silver / silver chloride.

Claims

1. A sensing layer containing self-assembled modified magnesium aluminum silicate for preparing an electrochemical sensor, the electrochemical sensor comprising a flexible electrode, characterized in that: The sensing layer is formed by drop-coating a sensing layer solution that can be self-assembled and modified with the modified layer on a modified layer obtained by grafting a hydrophilic organic high molecular polymer on a working electrode of the flexible electrode; The sensing layer solution comprises a redox polymer, a tool enzyme, a crosslinking agent A, and magnesium aluminum silicate, and the mass ratio of the redox polymer: the tool enzyme: the crosslinking agent A: the magnesium aluminum silicate is 15-40: 20-45: 5-30: 1-10.

2. The sensing layer according to claim 1, characterized in that: The hydrophilic organic high molecular polymer is selected from one or more of polyallylamine, polyethylene glycol, polyethyleneimine, polyamide-amine dendrimer, and poly(L-lysine); The redox polymer is a redox polymer containing a transition metal, and the transition metal includes ruthenium, rhodium, and osmium; The tool enzyme is selected from glucose dehydrogenase, glucose oxidase, uricase, lactate oxidase, and cholesterol oxidase; The crosslinking agent A is selected from one or more of 1,4-butanediol diglycidyl ether, poly(dimethylsiloxane)-diglycidyl ether, glutaraldehyde, polyethylene glycol diglycidyl ether, tetraepoxypropyl-4,4-diaminodiphenylmethane or glycerol triglycidyl ether; preferably, the crosslinking agent A is polyethylene glycol diglycidyl ether with MW=200Da-5000Da, preferably MW=400Da.

3. The sensing layer according to claim 1, characterized in that: The mass ratio of the redox polymer: tool enzyme: cross-linking agent A: magnesium aluminum silicate is 35-40:20-35:20-30:4-10, preferably 35-40:25-35:25-30:5-10, and more preferably 39:31:25:5; The concentration of the redox polymer in the sensing layer solution is 2-5 mg / ml, preferably 2-4.5 mg / ml, and more preferably 3.0-4.5 mg / ml.

4. A method for preparing a sensing layer, wherein the sensing layer is a sensing layer containing self-assembled modified magnesium aluminum silicate according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: S1. Plasma-induced grafting of a hydrophilic organic polymer on a working electrode of a flexible electrode to obtain a modified layer; S2, drop-coating the sensing layer solution onto the modified layer, and obtaining the sensing layer after cross-linking and curing.

5. The preparation method according to claim 4, characterized in that: The method of obtaining a modified layer by grafting a hydrophilic organic high molecular polymer on the working electrode of the flexible electrode by plasma initiation comprises: After the flexible electrode is treated with air plasma, the flexible electrode is immersed in a hydrophilic organic polymer aqueous solution with a concentration of 25 to 40 mg / mL and a temperature of 35 to 40° C. for 14 to 20 hours, and then the electrode is immersed in purified water for 20 to 30 hours and then taken out and dried for 30 to 40 minutes to form the modified layer on the working electrode of the flexible electrode.

6. The preparation method according to claim 4, characterized in that: The step of dripping the sensing layer solution onto the modified layer and cross-linking and curing to obtain the sensing layer comprises the following steps: S2.1, preparing a sensing layer solution: using solvent A to prepare a mixed solution of redox polymer, tool enzyme, crosslinking agent A, and magnesium aluminum silicate, and mixing them thoroughly to obtain a sensing layer solution; the solvent A is HEPES buffer or TES buffer; preferably, the concentration of the HEPES buffer is 5 to 20 mmol / L, and the pH is 7.5 to 8.2; S2.2, preparing the sensing layer: drop-coating the prepared sensing layer solution onto the surface of the modified layer obtained in step S1, and cross-linking and curing at a temperature of 20 to 30° C. for 20 to 28 hours to obtain the sensing layer.

7. An electrochemical sensor, characterized in that include: A flexible electrode, comprising a substrate, a working electrode, a counter electrode and a reference electrode, wherein: The working electrode and the counter electrode are respectively arranged on both sides of the substrate, a dielectric layer is arranged on the side of the counter electrode away from the substrate, the reference electrode is arranged on the side of the working electrode away from the substrate, the dielectric layer is arranged between the working electrode and the reference electrode, and the dielectric layer is arranged on the side of the reference electrode away from the working electrode; The surface of the working electrode has an exposed portion without a dielectric layer and a reference electrode, and the surface of the exposed portion is coated with a modified layer and a sensing layer in sequence; It also includes a diffusion restriction layer, which wraps the sensing layer and the exposed parts of the dielectric layer, the reference electrode, and the counter electrode; The modified layer and the sensing layer are the modified layer and the sensing layer described in any one of claims 1 to 3 or the modified layer and the sensing layer prepared by the preparation method described in any one of claims 4 to 6.

8. The electrochemical sensor according to claim 7, characterized in that: The diffusion limiting layer is derived from a polymer containing a nitrogen heterocyclic group and a crosslinking agent B; The polymer containing nitrogen heterocyclic groups is selected from one or more of polyvinyl pyridine, polyvinyl pyrrole, polyvinyl pyridine-styrene copolymer, and polyvinyl pyridine-styrene copolymer modified with sulfonic acid groups; The crosslinking agent B is selected from one or more of triglycidyl p-aminophenol, polyethylene glycol diglycidyl ether, tetraepoxypropyl-4,4'-diaminodiphenylmethane, tri(4-hydroxyphenyl)methane triglycidyl ether, and glycerol triglycidyl ether; preferably, the crosslinking agent B is polyethylene glycol diglycidyl ether with MW=200Da-5000Da, preferably MW=200Da; The mass ratio of the polymer containing nitrogen heterocyclic groups to the crosslinking agent B is 7-9.9:0.1-3, preferably 9:

1.

9. A method for preparing an electrochemical sensor according to claim 7 or 8, characterized in that: The steps include: S3, immersing the flexible electrode with the sensing layer obtained in step S2 in the outer membrane solution of the diffusion limiting layer, taking it out and curing it at a temperature of 20-35° C. to form a diffusion limiting layer, thereby obtaining the electrochemical sensor.

10. The preparation method according to claim 9, characterized in that: The step S3 comprises the following steps: S3.1, preparing a diffusion-restricting layer outer membrane solution: using solvent B as solvent, preparing a mixed solution of a polymer containing nitrogen heterocyclic groups and a crosslinking agent B to obtain a diffusion-restricting layer outer membrane solution; the solvent B is a TES buffer solution, or a mixed solution of anhydrous ethanol and a HEPES buffer solution, preferably, the solvent B is obtained by mixing anhydrous ethanol and a HEPES buffer solution in a volume ratio of 2 to 10:1, the concentration of the HEPES buffer solution is 5 to 20 mmol / L, and the pH is 7.5 to 8.2; the concentration of the polymer containing nitrogen heterocyclic groups in the diffusion-restricting layer outer membrane solution is 40 to 80 mg / ml, preferably 50 to 70 mg / ml; S3.2, preparing a diffusion-restricting layer: immersing the flexible electrode with a sensing layer obtained in step S2 in the diffusion-restricting layer outer membrane solution for multiple times, preferably 2 to 5 times, with an interval of 6 to 20 minutes between each time, and curing at a temperature of 20 to 35°C for 40 to 55 hours to form a diffusion-restricting layer to obtain the electrochemical sensor.

Citation Information

Patent Citations

  • Self-assembled redox polymers, sensors and their preparation methods

    CN115215953B

  • Biosensor membranes composed of polymers containing heterocyclic nitrogens

    US6932894B2

  • Biosensor coating compositions and methods thereof

    CN102016060A

  • Preparation method and application of nano hydrogel

    CN112442195A