Method for constructing high-temperature rapid fracture model of SiC ceramic block material with hole defects
By simulating the bending strength of SiC ceramic block material in Abaqus software and determining the parameters of the Brittle cracking model, the life problem of ceramic materials under high temperature conditions is solved, and the reliability and applicability of the model is improved.
Patent Information
- Application Number
- CN202410537380.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-12-03
AI Technical Summary
The problem of turbine blade life of existing ceramic materials under high-temperature service conditions has not been effectively solved, especially the constitutive model and its parameters are insufficiently determined under low strain rate loading conditions, resulting in uncertainty in the long-term application of ceramic materials.
The three-point bending experimental model of SiC ceramic block material containing hole defects was established in Abaqus software using Python language. By simulating the bending strength under different elastic modulus E and ultimate tensile strength UTS, the key parameters of the Brittle cracking model were determined. , and then build a high-temperature rapid fracture model.
It improves the reliability of the mechanical behavior analysis of SiC ceramic block materials under high temperature conditions, provides reference for service requirements under different conditions, meets national standards and test conditions, and enhances the reliability of the model.
Smart Images

Figure CN119066901A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material constitutive models, and in particular to a method for constructing a high-temperature rapid fracture model of a SiC ceramic block material containing void defects. Background Art
[0002] Gas turbines are free-flow rotating machines that can convert thermal energy into mechanical work. They are widely used in mechanical devices such as jet aircraft and compressors. Turbines are the core components of gas turbines, and turbine blades are an important part of turbines. In the past, deformed high-temperature alloys have always been a common material for manufacturing turbine blades, but the pursuit of high thrust-to-weight ratios by aircraft engines means that the performance of deformed high-temperature alloys can no longer meet the increasingly high temperature and performance requirements of turbine blades. Ceramic materials have excellent high-temperature resistance and low density, and ceramic materials are gradually being used in turbine blade applications. Among ceramic materials, SiC, Si3N4, Al2O3 and other materials are widely used because of relatively comprehensive research on them.
[0003] There are two common ceramic constitutive models. One is used to describe the response of ceramics to high strain rate loading, such as the Deshpande-Evans, Johnson-Holmquist (JH), Rajendran-Grove and Wilkins models. The other is used to describe the response of ceramics to low strain rate loading, such as the rapid fracture model, namely the Brittle Cracking model.
[0004] At present, the method of establishing the JH model for materials under high strain rate loading conditions is widely used and has been studied more fully. For example, in the paper "Research on Key Parameters of Johnson-Holmquist Constitutive Model of Concrete" published by Xiong Yibo et al. in "Engineering Mechanics", the JH model is widely used in the problem of strong dynamic loads of concrete and the lack of its reliable parameters is studied. By analyzing the sensitivity of parameters and statistical analysis of previous literature, and then verifying it by actual measurement, the key parameters in the JH model of concrete are obtained. In "JH-2 Model and Its Application in Numerical Simulation of Low-Speed Impact of Al2O3 Ceramics" published by Yang Zhenqi et al. in "Explosion and Shock", the JH-2 constitutive model describing the dynamic damage of ceramic materials and the determination of its parameters are discussed.
[0005] However, the life of turbine blades under high-temperature service conditions does not meet the premise of generating large strains in a short period of time. Therefore, the existing JH model and other models under high strain rate loading conditions are not applicable when exploring issues such as the life of turbine blades. The constitutive model under low strain rate loading conditions should be selected. However, the determination of constitutive models and their parameters under low strain rate loading conditions is still insufficient, especially the lack of key parameter determination methods for the Brittle cracking model, which brings uncertainty to the long-term application of ceramic materials. Summary of the invention
[0006] The object of the present invention is to provide a method for constructing a high-temperature rapid fracture model of a SiC ceramic bulk material containing void defects, thereby facilitating the reliability analysis of the SiC ceramic bulk material in practical applications.
[0007] The technical solution to achieve the purpose of the present invention is:
[0008] A method for constructing a high-temperature rapid fracture model of a SiC ceramic bulk material containing void defects comprises the following steps:
[0009] (1) Obtaining sample hole information, including the location and volume of each hole;
[0010] (2) Conduct a three-point bending test to obtain the bending strength of the sample;
[0011] (3) Using Python language for secondary development, a three-point bending experimental model of SiC ceramic block material with hole defects was established in Abaqus software according to the hole position and volume;
[0012] (4) Simulate the bending strength test of the specimen under different elastic modulus E and ultimate tensile strength UTS conditions in Abaqus software;
[0013] (5) By comparing the bending strength obtained from the simulation test with the measured bending strength, the elastic modulus E and the ultimate tensile strength UTS of the sample are determined, that is, the two parameters of the rapid fracture model are determined, and the rapid fracture model can be established.
[0014] Compared with the prior art, the present invention has the following significant advantages:
[0015] (1) Abaqus was used to analyze and predict the bending strength of the sample under different elastic modulus E and ultimate tensile strength UTS conditions, and compared with the measured values to determine the key parameters of the rapid fracture model. The influence of uncertain factors such as the microstructure in the material on the overall is reflected in the elastic modulus E and ultimate tensile strength UTS as a whole, which can provide a reference for the service requirements of SiC ceramic block materials under different conditions. (2) The hole data was preprocessed to improve the efficiency of Abaqus simulation within the error range. (3) The Brittle cracking model was used under low strain loading conditions, which meets national standards and test conditions, and is consistent with the actual long-term use conditions. The model reliability is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is an industrial CT scan image of specific embodiment 1 of the present invention.
[0017] Figure 2 This is a schematic diagram of the Brittle cracking model. DETAILED DESCRIPTION
[0018] The following is a detailed description of an embodiment of the present invention in conjunction with the accompanying drawings. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0019] In view of the above-mentioned defects of the prior art, the present invention provides a method for constructing a high-temperature rapid fracture model of a SiC ceramic block material containing void defects, thereby facilitating the study of the mechanical behavior of the SiC ceramic block material when serving at high temperatures.
[0020] The purpose of the present invention is achieved by adopting the following technical solutions:
[0021] Step 1, obtaining the sample hole information, including the position and volume of each hole;
[0022] Combination Figure 1 After the SiC ceramic bulk material sample is scanned by industrial CT, the real hole data obtained by the scan is preprocessed: starting from the first hole, the distances of the remaining holes with this hole in the X, Y, and Z directions are compared respectively, and the holes with a distance difference of less than 20μm are treated as having the same corresponding coordinates.
[0023] Step 2: Conduct a high temperature three-point bending test to obtain the bending strength of the sample;
[0024] Step 3: Using Python language, a three-point bending experimental model of SiC ceramic block material containing hole defects is established in Abaqus software according to the hole position and volume obtained in step 1.
[0025] Step 4, simulating the bending strength of the specimen under different elastic modulus E and ultimate tensile strength UTS conditions in Abaqus software;
[0026] For the three definitions in the Brittle cracking model, three sets of parameters need to be entered:
[0027] ①Brittle cracking
[0028] Two lines of data need to be entered to define the tensile strength of the material and the linear softening of the stress-strain relationship of the material after the tensile strength is reached.
[0029] First row: tensile strength, corresponding fracture strain to the tensile strength (set to 0).
[0030] Second row: The tensile stress after fracture is 0, and the corresponding fracture strain is 1e-5.
[0031] ②Brittle shear option
[0032] Two rows of data need to be entered to define the softening behavior of the material in the shear direction.
[0033] First row: ratio of shear stress to tensile strength at fracture (set to 1), and the corresponding strain (set to 0).
[0034] Second row: After fracture, the shear stress is 0, and the corresponding fracture strain is 1e-5.
[0035] ③Brittle failure option
[0036] Define the element failure behavior, i.e. the element deletion criteria. Enter a row of data: 1e-5. This means that the material fails and the element is deleted when the fracture strain is 1e-5.
[0037] It is preliminarily believed that the elastic modulus E of SiC under high temperature conditions is [100,500] GPa, and the ultimate tensile strength UTS ranges from [400,900] MPa. Figure 2 In the Brittle cracking model, the bending strength simulation test was carried out with different combinations of UTS and E.
[0038] Step 5: By comparing the bending strength obtained from the simulation test with the measured bending strength, the elastic modulus E and the ultimate tensile strength UTS of the sample can be determined, and a rapid fracture model can be established.
[0039] The UTS corresponding to the relative error between the simulated value and the measured value of the specimen obtained in step 4 is less than 10% is the model parameter value. If there are multiple sets of suitable UTS, the UTS with the smallest absolute error is selected. If the simulated bending strength obtained within the E and UTS range in step 4 has a large error with the actual value, the E and UTS ranges can be appropriately expanded within a reasonable range to increase simulation tests.
[0040] Example 1: Determination of Brittle Cracking Model for SiC Ceramic No. 1 at 1200°C
[0041] Step 1: Obtain the sample hole location and volume data
[0042] Use industrial CT to scan the complete sample, obtain the hole position and volume data, store them in original_data.xlsx, and run the following code in Python to preprocess the data for position adjustment:
[0043]
[0044]
[0045] Among them, N_Hole represents the number of holes in the file; HoleX represents the current hole X coordinate; HoleY represents the current hole Y coordinate; HoleZ represents the current hole Z coordinate.
[0046] Step 2: Conduct a high temperature three-point bending test to obtain the actual bending strength of the sample
[0047] The sample used in step 1 was subjected to a fracture toughness test and its measured fracture toughness value was 332 MPa.m 0.5 .
[0048] Step 3: Using Python language, a three-point bending experimental model of SiC ceramic block material containing hole defects is established in Abaqus software according to information such as hole position and volume.
[0049] In Python, call the python code corresponding to the command in Abaqus software to construct a specimen with the same size as the specimen (length 18mm*width 3mm*height 4mm), and delete the material of the corresponding position and size in the specimen according to the hole data processed in step 1. The above codes are all in Python language and interpreted and executed in Abaqus.
[0050] Step 4: Simulate the bending strength of the specimen under different elastic modulus E and ultimate tensile strength UTS conditions in Abaqus software
[0051] For the three definitions in the Brittle cracking model in Abaqus, three sets of parameters need to be entered:
[0052] ①Brittle cracking
[0053] Two lines of data need to be entered to define the tensile strength of the material and the linear softening of the stress-strain relationship of the material after the tensile strength is reached.
[0054] First row: tensile strength, corresponding fracture strain to the tensile strength (set to 0).
[0055] Second row: The tensile stress after fracture is 0, and the corresponding fracture strain is 1e-5.
[0056] ②Brittle shear option
[0057] Two rows of data need to be entered to define the softening behavior of the material in the shear direction.
[0058] First row: ratio of shear stress to tensile strength at fracture (set to 1), and the corresponding strain (set to 0).
[0059] Second row: After fracture, the shear stress is 0, and the corresponding fracture strain is 1e-5.
[0060] ③Brittle failure option
[0061] Define the element failure behavior, i.e. the element deletion criteria. Enter a row of data: 1e-5. This means that the material fails and the element is deleted when the fracture strain is 1e-5.
[0062] By searching the website (http: / / www.matweb.com) and combining experiments, the elastic modulus E is preliminarily determined to be in the range of [100,500] GPa and the ultimate tensile strength UTS is in the range of [400,900] MPa.
[0063] In the Brittle cracking model, UTS was set to 600, 650, 700, 750, 800, and 850 MPa, and E was set to 100, 140, 180, and 220 GPa, respectively. Mechanical analysis was performed at 1200°C to obtain the simulated bending strength.
[0064] Step 5: Obtain the elastic modulus and ultimate tensile strength of the specimen and establish a rapid fracture model
[0065] Taking into account the error caused by the preprocessing of the hole data and the accidental errors in other experimental operations, the parameters corresponding to the predicted values within the error range of 10% are considered to be the actual parameters. The comparison between some predicted values and measured values obtained in step 4 is shown in Table 1.
[0066] Table 1E is the comparison between the predicted four-point bending strength of SiC ceramics at 1200℃ and the experimental results at different UTS at 410GPa. Prediction: MPa, relative error, %
[0067]
[0068] Therefore, it can be obtained that the elastic modulus of the SiC ceramic bulk material at 1200°C is 410 GPa, and the ultimate tensile strength is 400 MPa, that is, the ultimate tensile strength and elastic modulus of the rapid fracture model are determined.
[0069] Example 2: Determination of Brittle Cracking Model for SiC Ceramic No. 2 at 1100°C
[0070] Step 1: Obtain the location and size data of the sample hole
[0071] Use industrial CT to scan the complete sample, obtain the hole location and size data, store it in original_data.xlsx, and run the following code in Python to preprocess the data.
[0072]
[0073]
[0074] Among them, N_Hole represents the number of holes in the file; HoleX represents the current hole X coordinate; HoleY represents the current hole Y coordinate; HoleZ represents the current hole Z coordinate.
[0075] Step 2: Conduct a high temperature three-point bending test to obtain the actual bending strength of the sample
[0076] The sample used in step 1 was subjected to a fracture toughness test and its measured fracture toughness value was 332 MPa.m 0.5 .
[0077] Step 3: Using Python language, a three-point bending experimental model of SiC ceramic block material containing hole defects is established in Abaqus software according to information such as hole position and size.
[0078] In Python, call the python code corresponding to the command in Abaqus software to construct a specimen with the same size as the specimen (length 18mm*width 3mm*height 4mm), and delete the material of the corresponding position and size in the specimen according to the hole data processed in step 1. The above codes are all in Python language and interpreted and executed in Abaqus.
[0079] Step 4: Simulate the bending strength of the specimen under different elastic modulus E and ultimate tensile strength UTS conditions in Abaqus software
[0080] For the three definitions in the Brittle cracking model in Abaqus, three sets of parameters need to be entered:
[0081] ①Brittle cracking
[0082] Two lines of data need to be entered to define the tensile strength of the material and the linear softening of the stress-strain relationship of the material after the tensile strength is reached.
[0083] First row: tensile strength, corresponding fracture strain to the tensile strength (set to 0).
[0084] Second row: The tensile stress after fracture is 0, and the corresponding fracture strain is 1e-5.
[0085] ②Brittle shear option
[0086] Two rows of data need to be entered to define the softening behavior of the material in the shear direction.
[0087] First row: ratio of shear stress to tensile strength at fracture (set to 1), and the corresponding strain (set to 0).
[0088] Second row: After fracture, the shear stress is 0, and the corresponding fracture strain is 1e-5.
[0089] ③Brittle failure option
[0090] Define the element failure behavior, i.e. the element deletion criteria. Enter a row of data: 1e-5. This means that the material fails and the element is deleted when the fracture strain is 1e-5.
[0091] It is preliminarily believed that the elastic modulus E ranges from [100,500] GPa and the ultimate tensile strength UTS ranges from [400,900] MPa.
[0092] In the Brittle cracking model, UTS was taken as 600, 650, 700, 750, 800, and 850 MPa, and E was taken as 100, 140, 180, and 220 GPa, respectively, and fracture toughness simulation experiments were carried out at 1100°C.
[0093] Step 5: Obtain the elastic modulus and ultimate tensile strength of the sample, and obtain the rapid fracture model. Compare the different fracture toughness prediction values obtained from step 4 with the fracture toughness measured values obtained from step 2. Considering the error caused by the preprocessing of the hole data and the accidental errors in other experimental operations, the parameters corresponding to the predicted values within the error range of 10% are considered to be the actual parameters. The comparison of some predicted values and measured values obtained in step 4 is shown in Table 2.
[0094] Table 2E shows the comparison between the predicted four-point bending strength of SiC ceramics at 1100°C and the experimental results at different UTS at 400 GPa.
[0095] Prediction: MPa, relative error, %
[0096]
[0097] Therefore, it can be obtained that the elastic modulus of the SiC ceramic bulk material at 1100°C is 400 GPa, and the ultimate tensile strength is 600 MPa, and the rapid fracture model is determined based on these two parameters.
[0098] The above embodiments are two preferred implementation cases of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for constructing a high-temperature rapid fracture model of SiC ceramic bulk material containing void defects, characterized in that: The steps include: (1) Obtaining sample hole information, including the location and volume of each hole; (2) Conduct a three-point bending test to obtain the bending strength of the sample; (3) Using Python language for secondary development, a three-point bending experimental model of SiC ceramic block material with hole defects was established in Abaqus software according to the hole position and volume; (4) Simulate the bending strength test of the specimen under different elastic modulus E and ultimate tensile strength UTS conditions in Abaqus software; (5) By comparing the bending strength obtained from the simulation test with the measured bending strength, the elastic modulus E and the ultimate tensile strength UTS of the sample can be determined, and a rapid fracture model can be established.
2. The method according to claim 1, characterized in that Obtaining sample hole information: After industrial CT scanning, preprocess the real hole data obtained by scanning: starting from the first hole, compare the distances of the remaining holes with the hole in the X, Y, and Z directions respectively. Holes with a distance difference of less than 20 μm are treated as having the same corresponding coordinates.
3. The method according to claim 1, characterized in that The Brittle cracking model was adopted as the rapid fracture model.
4. The method according to claim 3, characterized in that For the three definitions in the Brittle cracking model, three sets of parameters need to be entered: ①Brittle cracking Two lines of data need to be entered to define the tensile strength of the material and the linear softening of the stress-strain relationship of the material after the tensile strength is reached. First row: tensile strength, the fracture strain corresponding to the tensile strength is set to 0; Second row: tensile stress after fracture is 0, and the corresponding fracture strain is 1e-5; ②Brittle shear option Two rows of data need to be entered to define the softening behavior of the material in the shear direction; First row: the ratio of shear stress to tensile strength at fracture is set to 1, and the corresponding strain is set to 0; Second row: the shear stress after fracture is 0, and the corresponding fracture strain is 1e-5; ③Brittle failure option Define the unit failure behavior, that is, the unit deletion criterion; enter a line of data: 1e-5, which means that the material fails when the fracture strain is 1e-5 and the unit is deleted; In the Brittle cracking model, bending strength simulation tests were carried out with different combinations of UTS and E.
5. The method according to claim 1, characterized in that The UTS corresponding to the relative error between the simulated and measured values of the two samples is less than 10% is taken as the model parameter value. If there are multiple sets of suitable UTS, the UTS of the set with the smallest absolute error is taken.