Semiconductor structure and forming method thereof
By etching the initial conductive layer with a metal oxide mask layer with an etching window in integrated circuit manufacturing, the problem of difficulty in controlling the morphology of the open side wall is solved, and the high reliability and yield of the semiconductor structure are achieved.
Patent Information
- Application Number
- CN202310602595.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-03
AI Technical Summary
During the manufacturing process of integrated circuits, the morphology of the open side wall is not easy to control, which affects the reliability and yield of the semiconductor structure.
The initial conductive layer is etched by a metal oxide mask layer with an etching window. The high etching rate of the metal oxide mask layer avoids the problem of poor morphology of the conductive layer after etching, and ensures the conductive layer morphology. It is good, and then an excellent word line structure is formed to avoid short-connection between the word line structure and the gate structure of the peripheral region.
The reliability and yield of the semiconductor structure are improved, and the short-circuit problem is avoided by optimizing the morphology of the conductive layer, and the performance of the semiconductor structure is improved.
Smart Images

Figure CN119069347A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to the field of semiconductor technology, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] The manufacturing process of semiconductor structures including integrated circuits involves processes such as photolithography, etching, and thin film deposition. Through photolithography and etching processes, at least one opening (including trenches, through holes, and contact windows, etc.) can be etched in the target etching layer to form target structures, such as gate lines, bit lines, memory cells, and metal interconnect structures.
[0003] As integrated circuits develop towards smaller sizes, the characteristic size of patterns and the spacing between patterns continue to shrink. There are some very serious problems in the method of forming openings. For example, the profile of the opening sidewall is difficult to control, and the morphology of the opening has a certain impact on the reliability and yield of the semiconductor structure. Summary of the invention
[0004] The embodiments of the present disclosure provide a semiconductor structure and a method for forming the same, which are at least beneficial to improving the reliability and yield of the semiconductor structure.
[0005] On the one hand, an embodiment of the present disclosure provides a method for forming a semiconductor structure, including: providing a substrate; forming an initial conductive layer on the substrate, the initial conductive layer including an initial conductive layer of a first zone and an initial conductive layer of a second zone that are adjacent to each other; forming a metal oxide mask layer having an etching window on a top surface of the initial conductive layer away from the substrate, the etching window exposing the top surface of the initial conductive layer of the first zone; removing a portion of the thickness of the initial conductive layer of the first zone through the etching window, and the remaining initial conductive layer of the first zone serves as the first conductive layer, and the initial conductive layer of the second zone serves as the second conductive layer, the side surface of the second conductive layer is connected to the top surface of the first conductive layer, and the angle between the side surface and the top surface of the first conductive layer is within a preset range; and removing the metal oxide mask layer.
[0006] In some embodiments, a first etching condition is used to remove a portion of the thickness of the initial conductive layer in the first region, and the process gas of the first etching condition includes at least hydrogen fluoride.
[0007] In some embodiments, the process gas of the first etching condition further includes ozone.
[0008] In some embodiments, the process temperature of the first etching condition is 240° C. to 260° C.
[0009] In some embodiments, a hydrofluoric acid solution is used to remove the metal oxide mask layer, and the volume ratio of hydrofluoric acid to water in the hydrofluoric acid solution is 1:220 to 1:180.
[0010] In some embodiments, the material of the metal oxide mask layer includes zirconium oxide.
[0011] In some embodiments, forming a metal oxide mask layer having an etching window includes: forming an initial metal oxide layer 120 on the top surface of the initial conductive layer away from the substrate by a spin coating process; and patterning the initial metal oxide layer 120 to form a metal oxide mask layer.
[0012] In some embodiments, the method for forming a semiconductor structure also includes: performing a first etching process, wherein the first etching process removes a portion of the thickness of the first conductive layer so that the maximum thickness of the first conductive layer is a first preset value; and performing a second etching process, wherein the second etching process removes a portion of the thickness of the second conductive layer so that the maximum thickness of the second conductive layer is a second preset value.
[0013] In some embodiments, the first etching process is the same as the second etching process.
[0014] In some embodiments, the substrate includes a first part and a second part adjacent to each other, the top surface of the first part is lower than the top surface of the second part, the initial conductive layer of the second region is located on the second part and on a portion of the first part adjacent to the second part; the second etching process includes: exposing the top surface of the second part.
[0015] In some embodiments, after the second etching process is performed, a height difference between a top surface of the remaining second conductive layer and a top surface of the second portion is within a first range.
[0016] In some embodiments, the first range is 17 nm to 21 nm.
[0017] In some embodiments, after performing the first etching process and the second etching process, the method for forming a semiconductor structure further includes: forming a third conductive layer on a top surface of the first conductive layer, and the first conductive layer, the second conductive layer and the third conductive layer constitute a word line structure.
[0018] In some embodiments, the step of forming a third conductive layer includes: forming an initial third conductive layer on the top surface of the first conductive layer and the top surface of the second conductive layer, the initial third conductive layer including a first portion of the initial third conductive layer located on the first conductive layer and a second portion of the initial third conductive layer located on the second conductive layer; removing the second portion of the initial third conductive layer, and removing a partial thickness of the initial third conductive layer of the first portion, with the remaining first portion of the initial third conductive layer serving as the third conductive layer.
[0019] On the other hand, the embodiments of the present disclosure also provide a semiconductor structure prepared by using any of the above-mentioned semiconductor structure formation methods, the semiconductor structure comprising: a substrate; an adjacent first conductive layer and a second conductive layer, the top surface of the second conductive layer is higher than the top surface of the first conductive layer, the side surface of the second conductive layer is connected to the top surface of the first conductive layer, and the angle between the side surface and the top surface of the first conductive layer is within a preset range.
[0020] The technical solution provided by the embodiments of the present disclosure has at least the following advantages: in a method for forming a semiconductor structure, a metal oxide mask layer with an etching window is used to etch an initial conductive layer of a partial thickness of a first region. Because under the same etching conditions, the initial conductive layer has a higher etching rate than the metal oxide mask layer, the metal oxide mask layer is used as a mask layer for etching the initial conductive layer, which is beneficial to avoiding the problem of poor morphology of the initial conductive layer after etching caused by consumption of the mask layer in the etching process, that is, ensuring that the first conductive layer and the second conductive layer have good morphology, thereby making the word line structure formed using the first conductive layer and the second conductive layer have a better morphology, avoiding short circuit between the word line structure and the gate structure of the peripheral region, which is beneficial to improving the reliability and yield of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] One or more embodiments are exemplarily illustrated by pictures in the corresponding drawings, and these exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the pictures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the traditional technology, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figures 1 to 14 A schematic diagram of the steps of a method for forming a semiconductor structure provided in an embodiment of the present disclosure. DETAILED DESCRIPTION
[0023] As known from the background art, the morphology of the opening formed by local etching has a certain influence on the reliability and yield of the semiconductor structure.
[0024] The disclosed embodiments provide a semiconductor structure and a method for forming the same. In the method for forming the semiconductor structure, a metal oxide mask layer having an etching window is used to etch an initial conductive layer of a first region of partial thickness. Since the initial conductive layer has a higher etching rate than the metal oxide mask layer under the same etching conditions, the metal oxide mask layer is used as a mask layer for etching the initial conductive layer, which is beneficial for avoiding the problem of poor morphology of the initial conductive layer after etching caused by consumption of the mask layer in the etching process, that is, ensuring that the first conductive layer and the second conductive layer have good morphology, thereby making the word line structure formed by using the first conductive layer and the second conductive layer have better morphology, avoiding short circuit between the word line structure and the gate structure of the peripheral region, which is beneficial for improving the reliability and yield of the semiconductor structure.
[0025] The following will describe the various embodiments of the present disclosure in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present disclosure, many technical details are provided in order to enable the reader to better understand the embodiments of the present disclosure. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solutions claimed in the embodiments of the present disclosure can be implemented.
[0026] Figures 1 to 14 A schematic diagram of the steps of a method for forming a semiconductor structure provided in an embodiment of the present disclosure.
[0027] refer to Figure 1 The method for forming a semiconductor structure includes: providing a substrate 100. In some embodiments, the substrate 100 may be a structure manufactured from an initial substrate and formed with an isolation structure, an active region 103 and a dielectric layer.
[0028] refer to Figure 1 In some embodiments, the isolation structure may include a silicon nitride layer 105 and a silicon oxide layer 104 , and the dielectric layer may include a silicon oxide layer 104 .
[0029] In some embodiments, the material of the initial substrate may be silicon. In other embodiments, the material of the initial substrate may also be a material that can be directly used in the manufacturing process to produce semiconductor devices, for example, the material of the substrate 100 may be at least one of silicon on insulating substrate (SOI), germanium, silicon carbide, gallium arsenide, or sapphire.
[0030] In some embodiments, reference Figure 1 The substrate 100 includes a first portion 101 and a second portion 102 adjacent to each other, and the top surface of the first portion 101 of the substrate is lower than the top surface of the second portion 102 of the substrate. In some embodiments, the first portion 101 of the substrate is used to form an array region of a memory chip, and the second portion 102 of the substrate is used to form a peripheral region of the memory chip.
[0031] refer to Figure 2 , an initial conductive layer 110 is formed on the substrate, the initial conductive layer 110 includes an initial conductive layer 111 in the adjacent first region and an initial conductive layer 112 in the second region, the initial conductive layer 112 in the second region is located on the second portion 102 of the substrate, and is located on a portion of the first portion 101 of the substrate adjacent to the second portion 102 of the substrate. The initial conductive layer 111 in the first region is used to form a subsequent first conductive layer, the initial conductive layer 112 in the second region is used to form a subsequent second conductive layer, the first conductive layer and the second conductive layer are used to form a word line structure, the top surface of the portion of the word line structure formed by the second conductive layer is higher than the top surface of the remaining word line structure, so that when a conductive plug is formed on the portion of the word line structure with a higher top surface, it is beneficial to achieve good contact between the conductive plug and the word line structure, thereby reducing the difficulty of manufacturing the semiconductor structure and improving the performance of the semiconductor structure.
[0032] In some embodiments, the initial conductive layer 110 may be formed by a deposition process, for example, the initial conductive layer 110 may be formed by a magnetron sputtering process, a chemical vapor deposition process, or an atomic layer deposition process. In some embodiments, due to the different top surface heights of the underlying film layers, the top surface flatness of the initial conductive layer 110 formed by the deposition process may be poor, and the initial conductive layer 110 with poor top surface flatness may affect the subsequent patterning process. Therefore, after the initial conductive layer 110 is formed by the deposition process, the method for forming the semiconductor structure further includes: flattening the initial conductive layer 110 with poor top surface flatness, so that the top surface of the initial conductive layer 110 has better flatness. In some implementations, the top surface of the initial conductive layer 110 may be flattened by a chemical mechanical polishing process.
[0033] It should be noted that the top surface of the initial conductive layer 110 is the surface of the initial conductive layer 110 away from the substrate, and the height of the top surface of the initial conductive layer 110 is the height of the top surface of the initial conductive layer 110 in the direction from the substrate to the initial conductive layer 110. The direction from the substrate to the initial conductive layer 110 can be defined as the first direction X.
[0034] In some embodiments, the material of the initial conductive layer 110 is titanium nitride, which has excellent conductivity and corrosion resistance. Using titanium nitride to form a word line structure is beneficial to improving the conductivity and reliability of the word line structure.
[0035] In some embodiments, reference Figure 2The substrate includes a first portion 101 and a second portion 102 adjacent to each other. The top surface of the first portion 101 of the substrate is lower than the top surface of the second portion 102 of the substrate. The initial conductive layer 112 of the second region is located on the second portion 102 of the substrate, and on the first portion 101 of the substrate adjacent to the second portion 102 of the substrate. Along the first direction X, the thickness L1 of the initial conductive layer 110 on the second portion 102 of the substrate can be 10nm to 30nm, for example, 12nm, 15nm, 20nm or 25nm. In this way, on the one hand, it is conducive to ensuring that the initial conductive layer 110 completely covers the top surface of the substrate, thereby reducing the difficulty of subsequent patterning of the initial conductive layer 110; on the other hand, it avoids the waste of production materials caused by forming an overly thick initial conductive layer 110 on the second portion 102 of the substrate.
[0036] In some embodiments, reference Figure 2 The maximum thickness L2 of the initial conductive layer 110 on the first portion 101 of the substrate may be 200 nm to 240 nm, for example, 205 nm, 215 nm, 218 nm or 230 nm.
[0037] refer to Figures 3 to 5 , a metal oxide mask layer 121 having an etching window 122 is formed on the top surface of the initial conductive layer 110 away from the substrate, and the etching window 122 exposes the top surface of the initial conductive layer 111 in the first region. The metal oxide mask layer 121 having the etching window 122 is used as a mask layer for etching the initial conductive layer 110. It should be noted that in the related art, a photoresist is used as a mask layer for etching the initial conductive layer 110, and the etching process of the initial conductive layer 110 consumes the photoresist, which may result in a step-like structure between the etched initial conductive layer 110 and the unetched initial conductive layer 110, resulting in a poor morphology of the etched initial conductive layer 110. In the method for forming a semiconductor structure provided in the embodiment of the present disclosure, since the material of the metal oxide mask layer 121 is a metal oxide and the material of the initial conductive layer 110 is a conductive material, the properties of the metal oxide and the properties of the conductive material are quite different. Under the same etching conditions, the initial conductive layer 110 has a higher etching rate than the metal oxide mask layer 121. The metal oxide mask layer 121 serves as a mask layer for etching the initial conductive layer 110, which helps to avoid the problem of poor morphology of the initial conductive layer 110 after etching caused by consumption of the photoresist layer in the etching process, that is, to ensure that the first conductive layer and the second conductive layer have good morphology, thereby making the word line structure formed by the first conductive layer and the second conductive layer have better morphology.
[0038] It should be noted that the reference Figure 1, the second part 102 of the substrate 100 is used to form the peripheral area of the memory chip. The top surface 103a of the active area 103 of the second part 102 of the substrate 100 needs to be exposed in the subsequent process steps, so as to form a gate structure of the peripheral area in contact with the top surface 103a of the active area 103 of the second part 102. When the top surface of the partial word line structure formed by the second conductive layer is higher, if the morphology of the partial word line structure formed by the second conductive layer is poor, the subsequent process of exposing the top surface 103a of the active area 103 of the peripheral area may simultaneously expose the partial word line structure formed by the second conductive layer, thereby causing the gate structure of the peripheral area to be short-circuited with the partial word line structure formed by the second conductive layer, which affects the reliability and yield of the semiconductor structure. Therefore, the embodiment of the present disclosure uses the first conductive layer and the second conductive layer to form a word line structure with a better morphology, which is beneficial to avoid the short circuit between the word line structure and the gate structure of the peripheral area, thereby improving the reliability and yield of the semiconductor structure.
[0039] In some embodiments, the material of the metal oxide mask layer 121 includes zirconium oxide. Since the process of etching the initial conductive layer 110 has a lower etching rate for zirconium oxide, and zirconium oxide has a better gap filling ability, the metal oxide mask layer 121 formed by using zirconium oxide has high flatness and better coverage. Zirconium oxide is used as a mask layer for etching the initial conductive layer 110, and the morphology of the initial conductive layer 110 after etching can be accurately controlled, which is beneficial to improving the performance of the semiconductor structure.
[0040] In some embodiments, reference Figure 5 , along the first direction X, the thickness L3 of the metal oxide mask layer 121 may be 8nm to 12nm, for example, 8.5nm, 9nm, 10nm or 11nm. If the thickness of the metal oxide mask layer 121 is too thick, it may cause waste of manufacturing materials. If the thickness of the metal oxide mask layer 121 is too thin, it cannot effectively protect the initial conductive layer 110 below the metal oxide mask layer 121. Therefore, setting the thickness of the metal oxide mask layer 121 within the range of 8nm to 12nm is conducive to avoiding waste of manufacturing materials and ensuring effective protection of the initial conductive layer 110 below the metal oxide mask layer 121.
[0041] In some embodiments, the step of forming the metal oxide mask layer 121 having the etching window 122 includes: referring to Figure 3, the initial metal oxide layer 120 is formed by spin coating on the top surface of the initial conductive layer 110 away from the substrate. That is to say, the metal oxide mask layer 121 formed subsequently is a SOMH (Spin on metal hardmask) layer, which not only has high flatness, but also has good gap filling performance, high hardness and low stress, is not prone to warping, and has low stress damage to the underlying film layer.
[0042] After forming the initial metal oxide layer 120, the initial metal oxide layer 120 is patterned to form a metal oxide mask layer 121. In some embodiments, referring to Figures 4 to 5 A photoresist mask layer 130 can be formed on the initial metal oxide layer 120, and the photoresist mask layer 130 has an etching window that exposes a portion of the initial metal oxide layer 120. The etching window of the photoresist mask layer 130 corresponds to the etching window 122 of the subsequently formed metal oxide mask layer 121. The initial metal oxide layer 120 exposed by the etching window is removed using the photoresist mask layer 130 to expose the top surface of the initial conductive layer 111 in the first region, and then the photoresist mask layer 130 is removed, and the remaining initial metal oxide layer 120 serves as the metal oxide mask layer 121.
[0043] In some embodiments, the material of the initial metal oxide layer 120 is zirconium oxide, and the material of the initial conductive layer 110 is titanium nitride. A hydrofluoric acid solution may be used to remove the initial metal oxide layer 120 exposed by the photoresist mask layer 130. The volume ratio of hydrofluoric acid to water in the hydrofluoric acid solution may be 1:220 to 1:180, for example, 1:200. Using a hydrofluoric acid solution with a volume ratio of hydrofluoric acid to water in the range of 1:220 to 1:180 to remove zirconium oxide is beneficial to avoid consumption of titanium nitride under the zirconium oxide.
[0044] refer to Figures 5 and 6, a portion of the initial conductive layer 111 of the first region is removed through the etching window 122 of the metal oxide mask layer 121, and the remaining initial conductive layer 111 of the first region is used as the first conductive layer 140, and the initial conductive layer 112 of the second region is used as the second conductive layer 141, and the side surface of the second conductive layer 141 is connected to the top surface of the first conductive layer 140, and the angle A between the side surface of the second conductive layer 141 and the top surface of the first conductive layer 140 is within a preset range. The first conductive layer 140 and the second conductive layer 141 formed by the metal oxide mask layer 121 avoid the formation of a step-like structure at the connection between the first conductive layer 140 and the second conductive layer 141, that is, the first conductive layer 140 and the second conductive layer 141 are ensured to have good morphology, so that the word line structure formed by the first conductive layer 140 and the second conductive layer 141 has a better morphology, which is beneficial to avoid the short circuit between the word line structure and the gate structure in the peripheral area, and thus is beneficial to improve the yield of the semiconductor structure.
[0045] In some embodiments, the preset range may be 0° to 30°.
[0046] In some embodiments, reference Figure 6 The height difference L4 between the top surface of the first conductive layer 140 and the top surface of the second conductive layer 141 is in the range of 60 nm to 80 nm. For example, the height difference L4 may be 65 nm or 70 nm.
[0047] In some embodiments, the material of the initial conductive layer is titanium nitride, and the material of the metal oxide mask layer 121 is zirconium oxide. In some embodiments, the initial conductive layer of the first region of partial thickness can be removed by a first etching condition, and the process gas of the first etching condition includes at least: hydrogen fluoride. In some embodiments, the process gas of the first etching condition also includes: ozone. In some embodiments, the process temperature of the first etching condition is 240°C to 260°C, for example, it can be 245°C, 250°C or 255°C. Hydrogen fluoride and ozone have a higher etching rate for titanium nitride at a process temperature of 240°C to 260°C, and have a lower etching rate for materials such as zirconium oxide, silicon nitride, silicon oxide, hafnium oxide and aluminum oxide. In this way, the first etching condition is used to achieve efficient selective etching of the initial conductive layer, which is conducive to avoiding the etching process of removing the initial conductive layer from causing heavier etching damage to other structures on the substrate.
[0048] refer to Figure 7, remove the metal oxide mask layer 121. In some embodiments, a hydrofluoric acid solution may be used to remove the metal oxide mask layer 121. The volume ratio of hydrofluoric acid to water in the hydrofluoric acid solution may be 1:220 to 1:180, for example, 1:220, 1:210, 1:200 or 1:190. In some embodiments, the material of the metal oxide mask layer 121 is zirconium oxide. The hydrofluoric acid solution with a volume ratio of hydrofluoric acid to water of 1:220 to 1:180 has a higher etching rate for zirconium oxide, and has a lower etching rate for materials such as silicon oxide, silicon nitride and titanium nitride. The above etching conditions are used to remove zirconium oxide, which is beneficial to avoid causing heavy etching damage to structures other than the metal oxide mask layer 121 on the substrate.
[0049] In some embodiments, reference Figure 8 , the method for forming a semiconductor structure also includes: performing a first etching process, the first etching process removes a portion of the thickness of the first conductive layer 140, so that the maximum thickness L5 of the first conductive layer 140 is a first preset value; performing a second etching process, the second etching process removes a portion of the thickness of the second conductive layer 141, so that the maximum thickness L6 of the second conductive layer 141 is a second preset value. The first etching process and the second etching process are used to further etch the remaining initial conductive layer on the substrate, so that the thickness of the first conductive layer 140 is reduced to the desired first preset value, and the thickness of the second conductive layer 141 is reduced to the desired second preset value. It should be noted that the maximum thickness L5 of the first conductive layer 140 is the maximum thickness of the first conductive layer 140 along the first direction X, and the maximum thickness L6 of the second conductive layer 141 is the maximum thickness of the second conductive layer 141 along the first direction X.
[0050] In some embodiments, the first preset value is 100 nm to 120 nm, for example, 100 nm, 105 nm, 110 nm or 115 nm. In some embodiments, the second preset value is 170 nm to 190 nm, for example, 170 nm, 175 nm, 180 nm or 185 nm.
[0051] In some embodiments, the first etching process is the same as the second etching process, that is, the first conductive layer 140 and the second conductive layer 141 are etched under the same etching conditions and in the same process steps, which is helpful to reduce the difficulty of forming the semiconductor structure.
[0052] It should be noted that the reference Figure 8 The second etching process includes: removing the second conductive layer 141 on the second portion 102 of the substrate to expose the top surface of the second portion 102 of the substrate.
[0053] In some embodiments, reference Figure 8After the second etching process, a height difference L7 between the top surface of the remaining second conductive layer 141 and the top surface of the second portion 102 is within the first range. Among them, the top surface of the second conductive layer 141 is the surface of the second conductive layer 141 away from the substrate. If the height difference L7 between the top surface of the second conductive layer 141 and the top surface of the second part 102 is too small, it may cause the material of the second conductive layer 141 to remain on the second part 102 of the substrate, thereby affecting the subsequent formation of other structures on the second part 102 of the substrate; if the height difference L7 between the top surface of the second conductive layer 141 and the top surface of the second part 102 is too large, it may cause the top surface of the second part 102 of the substrate to be etched, and even expose the active area 103 in the second part 102 of the substrate that was originally covered with the silicon oxide layer 104, causing serious process damage to the second part 102 of the substrate. Therefore, setting the height difference L7 between the top surface of the remaining second conductive layer 141 and the top surface of the second part 102 within the first range is conducive to alleviating the impact of the process steps of processing the first part 101 of the substrate on the second part 102 of the substrate.
[0054] In some embodiments, the first range is 17 nm to 21 nm, for example, 17 nm, 17.5 nm, 18 nm or 19 nm.
[0055] In some embodiments, after performing the first etching process and the second etching process, referring to Figures 9 to 11 The method for forming the semiconductor structure further includes: forming a third conductive layer 160 on the top surface of the first conductive layer 140, and the first conductive layer 140, the second conductive layer 141 and the third conductive layer 160 constitute a word line structure.
[0056] In some embodiments, the third conductive layer 160 is used to adjust the work function difference between the word line structure and the channel region of the transistor, and the first conductive layer 140 and the second conductive layer 141 are used to improve the conductivity of the word line structure. In some embodiments, the material of the third conductive layer 160 can be polysilicon. Compared with metal materials, polysilicon is easier to change the work function value by doping with different properties, and then the work function difference between the word line structure and the channel region of the transistor can be adjusted by adjusting the work function value.
[0057] In some embodiments, reference Figures 9 to 11, the step of forming the third conductive layer includes: forming an initial third conductive layer 150 on the top surface of the first conductive layer 140 and the top surface of the second conductive layer 141, the initial third conductive layer 150 includes a first portion of the initial third conductive layer 151 located on the first conductive layer 140 and a second portion of the initial third conductive layer 152 located on the second conductive layer 141; removing the second portion of the initial third conductive layer 152, and removing a portion of the thickness of the first portion of the initial third conductive layer 151, and the remaining first portion of the initial third conductive layer 151 is used as the third conductive layer 160. In some embodiments, the initial third conductive layer 150 is also formed on the top surface of the second portion 102 of the substrate, and the initial third conductive layer 150 on the second portion 102 of the substrate is defined as the initial third conductive layer 153 of the third portion, and the step of forming the third conductive layer 160 also includes: removing the third portion of the initial third conductive layer 153.
[0058] In some embodiments, the initial third conductive layer 150 may be formed by a deposition process. Fig. 9 The height difference of the top surface of the structure located at the bottom of the initial third conductive layer 150 causes the top surface flatness of the initial third conductive layer 150 formed by the deposition process to be poor. Therefore, the method for forming the semiconductor structure may further include: referring to Fig.10 The top surface of the initial third conductive layer 150 is planarized by using a chemical mechanical polishing process.
[0059] refer to Fig.11 In some embodiments, along the first direction X, the thickness of the third conductive layer 160 is 13 nm to 17 nm, for example, 14 nm, 15 nm, 16 nm or 16.9 nm.
[0060] Continue to refer Fig.11 In some embodiments, in the step of forming the third conductive layer 160, the etching process for removing the initial third conductive layer 150 also partially etches the top of the second conductive layer 141. The thickness of the second conductive layer 141 consumed by the etching process for removing the initial third conductive layer 150 may be in the range of 2 nm to 4 nm, for example, 3 nm.
[0061] refer to Figure 12 to Figure 14 In some embodiments, the method for forming a semiconductor structure further includes: forming a covering layer 180 covering the word line structure. In some embodiments, the material of the covering layer 180 can be silicon nitride. Fig.12 , a deposition process may be used to form an initial capping layer 170 on the top surface of the word line structure away from the substrate and on the top surface of the second portion 102 of the substrate, referring to Figure 13 to Figure 14, the top surface of the initial covering layer 170 is planarized, and the initial covering layer 170 is etched to remove the initial covering layer 170 formed on the top surface of the second portion 102 of the substrate, and a certain thickness of the initial covering layer 170 is retained on the word line structure as a covering layer 180.
[0062] In the method for forming a semiconductor structure provided in the above-mentioned embodiment, a metal oxide mask layer with an etching window is used to etch the initial conductive layer of a partial thickness of the first area. Because under the same etching conditions, the initial conductive layer has a higher etching rate than the metal oxide mask layer, the metal oxide mask layer is used as a mask layer for etching the initial conductive layer, which is beneficial to avoid the problem of poor morphology of the initial conductive layer after etching caused by consumption of the mask layer in the etching process, that is, to ensure that the first conductive layer and the second conductive layer have good morphology, thereby making the word line structure formed using the first conductive layer and the second conductive layer have better morphology, avoiding short circuit between the word line structure and the gate structure in the peripheral area, which is beneficial to improving the reliability and yield of the semiconductor structure.
[0063] Accordingly, the present disclosure also provides a semiconductor structure on the other hand, which can be formed by the semiconductor structure forming method provided by the above embodiment. It should be noted that the parts that are the same or corresponding to the above embodiment can refer to the detailed description of the above embodiment, and will not be repeated below.
[0064] refer to Fig.14 The semiconductor structure includes: a substrate; a first conductive layer 140 and a second conductive layer 141 adjacent to each other, the top surface of the second conductive layer 141 is higher than the top surface of the first conductive layer 140, the side surface of the second conductive layer 141 is connected to the top surface of the first conductive layer 140, and the angle A between the side surface of the second conductive layer 141 and the top surface of the first conductive layer 140 is within a preset range. The first conductive layer 140 and the second conductive layer 141 are used to form a word line structure, and the top surface of a part of the word line structure formed by the second conductive layer 141 is higher than the top surface of the remaining word line structure. In this way, when a conductive plug is formed on a part of the word line structure with a higher top surface, it is beneficial to achieve good contact between the conductive plug and the word line structure, thereby reducing the difficulty of manufacturing the semiconductor structure and improving the performance of the semiconductor structure. The angle A between the side surface of the second conductive layer 141 and the top surface of the first conductive layer 140 is within a preset range, which is beneficial to avoid short circuit between the word line structure and the gate structure in the peripheral area, thereby improving the yield of the semiconductor structure.
[0065] refer to Fig.14 In some embodiments, the semiconductor structure further includes a third conductive layer 160 , and the first conductive layer 140 , the second conductive layer 141 and the third conductive layer 160 constitute a word line structure.
[0066] It can be understood by those skilled in the art that the above-mentioned embodiments are specific examples for realizing the present disclosure, and in practical applications, various changes can be made to them in form and details without departing from the spirit and scope of the present disclosure. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present disclosure, so the protection scope of the present disclosure shall be based on the scope defined in the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; forming an initial conductive layer on the substrate, wherein the initial conductive layer includes an initial conductive layer in a first region and an initial conductive layer in a second region adjacent to each other; forming a metal oxide mask layer having an etching window on a top surface of the initial conductive layer away from the substrate, wherein the etching window exposes the top surface of the initial conductive layer in the first region; A portion of the thickness of the initial conductive layer in the first region is removed through the etching window, and the remaining initial conductive layer in the first region is used as the first conductive layer, and the initial conductive layer in the second region is used as the second conductive layer, and the side surface of the second conductive layer is connected to the top surface of the first conductive layer, and the angle between the side surface and the top surface of the first conductive layer is within a preset range; The metal oxide mask layer is removed.
2. The method for forming a semiconductor structure according to claim 1, wherein: A first etching condition is adopted to remove a partial thickness of the initial conductive layer in the first region, and the process gas of the first etching condition at least includes: hydrogen fluoride.
3. The method for forming a semiconductor structure according to claim 2, wherein: The process gas of the first etching condition also includes: ozone.
4. The method for forming a semiconductor structure according to claim 2 or 3, characterized in that: The process temperature of the first etching condition is 240° C. to 260° C.
5. The method for forming a semiconductor structure according to claim 1, wherein: The metal oxide mask layer is removed by using a hydrofluoric acid solution, wherein the volume ratio of hydrofluoric acid to water in the hydrofluoric acid solution is 1:220 to 1:
180.
6. The method for forming a semiconductor structure according to claim 1, wherein: The material of the metal oxide mask layer includes zirconium oxide.
7. The method for forming a semiconductor structure according to claim 1, wherein: Forming the metal oxide mask layer having the etching window comprises: Forming an initial metal oxide layer 120 on the top surface of the initial conductive layer away from the substrate by a spin coating process; The initial metal oxide layer 120 is patterned to form the metal oxide mask layer.
8. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the semiconductor structure further comprises: Performing a first etching process, wherein the first etching process removes a portion of the thickness of the first conductive layer so that a maximum thickness of the first conductive layer is a first preset value; A second etching process is performed, wherein the second etching process removes a portion of the thickness of the second conductive layer so that the maximum thickness of the second conductive layer is a second preset value.
9. The method for forming a semiconductor structure according to claim 8, characterized in that: The first etching process is the same as the second etching process.
10. The method for forming a semiconductor structure according to claim 8, wherein: The substrate comprises a first portion and a second portion adjacent to each other, a top surface of the first portion is lower than a top surface of the second portion, and the initial conductive layer of the second region is located on the second portion and on a portion of the first portion adjacent to the second portion; The second etching process includes: exposing a top surface of the second portion.
11. The method for forming a semiconductor structure according to claim 10, characterized in that: After the second etching process is performed, a height difference between a top surface of the remaining second conductive layer and a top surface of the second portion is within a first range.
12. The method for forming a semiconductor structure according to claim 11, characterized in that: The first range is 17 nm to 21 nm.
13. The method for forming a semiconductor structure according to claim 8, wherein: After performing the first etching process and the second etching process, the method for forming the semiconductor structure further includes: forming a third conductive layer on the top surface of the first conductive layer, and the first conductive layer, the second conductive layer and the third conductive layer constitute a word line structure.
14. The method for forming a semiconductor structure according to claim 13, wherein: The step of forming the third conductive layer comprises: forming an initial third conductive layer on the top surface of the first conductive layer and the top surface of the second conductive layer, wherein the initial third conductive layer includes a first portion of the initial third conductive layer located on the first conductive layer and a second portion of the initial third conductive layer located on the second conductive layer; The initial third conductive layer of the second portion is removed, and a portion of the thickness of the initial third conductive layer of the first portion is removed, and the remaining initial third conductive layer of the first portion serves as the third conductive layer.
15. A semiconductor structure, characterized in that: The semiconductor structure is manufactured by the method for forming a semiconductor structure according to any one of claims 1 to 14, and the semiconductor structure comprises: substrate; The first conductive layer and the second conductive layer are adjacent to each other, the top surface of the second conductive layer is higher than the top surface of the first conductive layer, the side surface of the second conductive layer is connected to the top surface of the first conductive layer, and the angle between the side surface and the top surface of the first conductive layer is within a preset range.