Silicon carbide chip, semiconductor device, and method for manufacturing silicon carbide chip
By designing specific angles and curvatures on the sides and main surfaces of the silicon carbide chip, and using multi-beam laser technology and annealing treatment during the slicing process, the problem of insufficient stability during the slicing process is solved, improving the durability of the chip and Connection strength.
Patent Information
- Application Number
- CN202410697711.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-19
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
During the semiconductor chip manufacturing process, the slicing process is not reliable enough, resulting in insufficient stability and robustness of the chip, which is prone to cracking and damage.
By designing specific angles and radius of curvature between the sides and main surface of the silicon carbide chip, and using multi-beam laser slicing technology during the slicing process, the depth and width of the slice saw and the adjustment of the laser beam during the annealing process The shape is to form a circular side wall, reducing the formation and uniform distribution of intermetallic compounds and reducing stress.
Improves the stability and robustness of silicon carbide chips, reduces the possibility of cracking and damage, and enhances the durability and connection strength of the chip.
Smart Images

Figure CN119069513A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of semiconductors, and in particular, to a silicon carbide chip, a semiconductor device, and a method for manufacturing the silicon carbide chip. Background Art
[0002] During the manufacture of semiconductor devices, individual components are usually processed on a wafer scale. Thereafter, the wafer is singulated into individual semiconductor chips. Generally, methods are being sought by which the slicing process can be improved, resulting in more reliable semiconductor chips. Summary of the invention
[0003] It is an object of the present invention to provide an improved semiconductor chip and an improved method for forming a semiconductor chip.
[0004] According to an embodiment, the above objects are achieved by the claimed subject matter according to the independent claims. Further developments are defined in the dependent claims.
[0005] According to an embodiment, a silicon carbide chip includes a first main surface, a second main surface and a side surface, wherein an angle α between the side surface and a horizontal plane measured in the silicon carbide material is greater than 78°, the angle α being measured in a region adjacent to the second main surface.
[0006] According to another embodiment, a silicon carbide chip includes a first main surface, a second main surface, a side surface, and an intermetallic compound layer adjacent to the side surface. The intermetallic compound layer has a thickness of less than 2 μm in a region separated from the second main surface by a distance of less than 20 μm, the thickness being measured in a direction parallel to the first main surface.
[0007] According to another embodiment, a silicon carbide chip includes a first main surface, a second main surface, and a side surface. A radius of curvature of an intersection between the second main surface and the side surface is greater than 0.5 μm.
[0008] A semiconductor device may include the silicon carbide chip as described above, a lead frame, and a solder material. The second main surface of the silicon carbide chip is arranged adjacent to the lead frame and is connected to the lead frame using the solder material.
[0009] According to an embodiment, a method for manufacturing a silicon carbide chip may include: defining a slicing kerf in a first main surface of a workpiece, and increasing the depth of the slicing kerf to obtain an opening. The method may further include: further increasing the depth of the opening to a position less than 20% of the thickness of the workpiece relative to a second main surface of the workpiece, performing an annealing process to increase the width of the slicing kerf, and further increasing the depth of the opening to singulate the workpiece into silicon carbide chips. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The accompanying drawings are included to provide a further understanding of embodiments of the invention, and the accompanying drawings are incorporated into and constitute a part of this specification. The accompanying drawings illustrate embodiments of the invention and are used to explain the principles together with the description. Other embodiments of the invention and many expected advantages will be readily understood as they become better understood by reference to the detailed description below. The elements of the accompanying drawings are not necessarily drawn to scale relative to each other. Like reference numerals designate corresponding similar parts.
[0011] Figures 1A to 1D A cross-sectional view illustrating a silicon carbide chip and a semiconductor device including the silicon carbide chip is shown.
[0012] Figure 2 It is an explanatory diagram for explaining the effects according to the embodiment.
[0013] Figures 3A to 3E is a cross-sectional view of a workpiece when the method according to the embodiment is performed.
[0014] Figure 4 The method according to the embodiment is summarized. DETAILED DESCRIPTION
[0015] In the following detailed description, reference is made to the accompanying drawings, which form a part of the detailed description and in which are illustrated by way of illustration specific embodiments in which the invention may be practiced. In this regard, directional terms such as "top", "bottom", "front", "rear", "above", "on", "above", "head", "tail", etc. are used with reference to the orientation of the drawings being described. Since the components of embodiments of the invention can be placed in many different orientations, the directional terms are used for illustrative purposes and are in no way limiting. It should be understood that other embodiments may be used and structural or logical changes may be made without departing from the scope defined by the claims.
[0016] The description of the embodiments is not restrictive. In particular, elements of the embodiments described below may be combined with elements of different embodiments.
[0017] The terms "wafer", "substrate" or "semiconductor substrate" used in the following description may include any semiconductor-based structure having a semiconductor surface. Wafers and structures may be understood to include silicon, silicon on insulator (SOI), silicon on sapphire (SOS), doped and undoped semiconductors, epitaxial layers of silicon supported by a base semiconductor foundation, and other semiconductor structures. Within the present disclosure, the above terms may specifically refer to silicon carbide (SiC).
[0018] The terms "lateral" and "horizontal" as used in this specification may describe an orientation parallel or essentially parallel (ie deviating by at most ±5°) to a first surface of a substrate or semiconductor body. This can be, for example, the surface of a wafer or die.
[0019] The term “vertical” as used in this specification may describe an orientation arranged perpendicular to a first surface of a substrate or semiconductor body.
[0020] Figure 1A A silicon carbide chip 15 according to an embodiment is shown. The silicon carbide chip 15 includes a first main surface 110, a second main surface 120, and a side surface 115. Semiconductor components such as transistors, diodes, and others (not shown) may be arranged in the silicon carbide chip 15. For example, the semiconductor components may be arranged in a region adjacent to the first main surface 110.
[0021] Typically, the size of the silicon carbide chip 15 may be approximately 8 mm 2 , for example, less than (3mm*3mm). However, less than 1mm 2 Or higher than 8mm 2 Chip sizes of may also be possible. The total thickness of the silicon carbide substrate may be greater than 50 μm or greater than 80 μm or greater than 100 μm. The thickness of the silicon carbide chip 15 may be less than 250 μm or less than 200 μm or less than 150 μm or less than 130 μm.
[0022] According to an embodiment, the silicon carbide chip 15 may be mounted to the lead frame 100, thus forming the semiconductor device 10. In this case, the second main surface 120 may be arranged on the side facing the lead frame 100. For example, the solder material 105 may include a suitable alloy (e.g., AuSn alloy, CuSn alloy, or NiSn alloy), and may be used to electrically and physically connect the silicon carbide chip 15 to the lead frame 100. In addition, the molding material 108 may be used to encapsulate the silicon carbide chip 15.
[0023] like Figure 1A As shown in , the angle α between the side 115 and the horizontal direction measured in the silicon carbide material may be greater than 78°. According to other embodiments, the angle α may be greater than 80° or greater than 84°. The angle α is measured in the area adjacent to the second main surface 120. Therefore, in the area adjacent to the second main surface 120, the side 115 may extend at an angle α relative to the horizontal plane (e.g., the xy plane). The side 115 does not need to be a straight line or a flat plane. According to implementation, the side 115 may be slightly curved, and the angle α may be measured between the tangent line of the side 115 and the horizontal plane. According to other implementations, the portion of the side 115 adjacent to the second main surface 120 may be a straight line, and the angle α is measured between this portion of the side 115 and the horizontal plane. For example, this portion of the side 115 may be separated from the second main surface 120 by a distance of less than 30 μm.
[0024] For example, the angle α may be measured between the side surface 115 and the second major surface 120. According to another embodiment, Figure 1B As shown in , the second main surface 120 may include an inclined portion 121, which may be adjacent to the side 115. The angle β between the inclined portion 121 and the horizontal plane may be greater than 5°. The angle β is measured outside the silicon carbide material. Figure 1A and 1B A comparison of α and β shows that the angle α is measured inside the silicon carbide material, while the angle β is measured outside the silicon carbide material. The angle β may be less than 30°.
[0025] When Figure 1B When the second major surface 120 shown in FIG. 1 includes an inclined portion 121 , the total angle between the side surface 115 and the inclined portion 121 of the second major surface may be equal to α + β. For example, (α + β) may be greater than 90°, such as less than 150°.
[0026] When β=0° (i.e., the second major surface 120 does not include the inclined portion 121), the angle between the second major surface 120 and the side surface 115 may be greater than 78°, greater than 80°, or greater than 84°. For example, the angle between the second major surface 120 and the side surface may be less than 102°, less than 100°, or less than 94°.
[0027] like Figure 1A As further shown in FIG. 1 , according to an embodiment, the side 115 may include a step portion 112. The step portion 112 may be or may include a horizontal portion that extends toward the inner portion of the silicon carbide chip 15. The step portion is arranged on a side facing the first main surface 110. For example, the lateral width s of the step portion may be greater than approximately 5 μm. The lateral width of the step portion may be less than 30 μm or less than 20 μm. The lateral width s of the step portion 112 may correspond to a distance between a lower portion of the side 115 close to the second main surface 120 (e.g., having a distance of at most 30 μm from the second main surface) and an upper portion of the side adjacent to the first main surface 110. In addition, a vertical distance h from the step portion 112 to the first main surface 110 may be less than approximately 20 μm. The vertical distance h may be greater than 1 μm or greater than 2 μm or greater than 5 μm.
[0028] The silicon carbide chip 15 may further include a back metallization layer 123. For example, the back metallization layer 123 may include a suitable alloy. For example, the back metallization layer 123 may include AuSn, CuSn or NiSn. In addition, the silicon carbide chip 15 may include a front metallization layer (not shown).
[0029] according to Figure 1CIn the embodiment shown in FIG. 1 , the radius of curvature r of the intersection between the second main surface 120 and the side surface 115 may be greater than 0.5 μm, or greater than 0.8 μm, or greater than 1.0 μm. In more detail, Figure 1C A tangent circle 122 is shown drawn about point A so as to be tangent to both the second major surface 120 and the side surface 115. The tangent circle 122 may have a radius r greater than 0.5 μm, or greater than 0.8 μm, or greater than 1.0 μm. Figure 1C The other elements of the silicon carbide chip 15 shown in FIG. Figure 1A and 1B The elements shown are similar or identical.
[0030] According to another embodiment, Figure 1D As shown in , the intermetallic compound 109 can be formed adjacent to the side 115 of the silicon carbide chip 15. For example, using a laser dicing method (e.g., dicing using a multi-beam laser), the silicon carbide chip 15 can be singulated from the wafer. During this dicing process, due to the large amount of energy induced in the silicon carbide chip 15, the intermetallic compound 109 can be generated from the back metallization layer 123. The intermetallic compound 109 can be deposited on the side 115 of the silicon carbide chip 15. As shown in FIG. Figure 1D As shown in , for example, the thickness t of the intermetallic compound 109 can be measured in a horizontal direction (e.g., in a direction parallel to the xy plane). In a distance d of less than 20 μm (or in a distance of less than 30 μm) relative to the second main surface 120, the thickness t of the intermetallic compound 109 can be less than 2 μm (or less than 1.5 μm or less than 1 μm). For example, the intermetallic compound may include the backside metallization 123 ( Figure 1A and 1C For example, the intermetallic compound may include any of Sn, Au, Cu, Si, O, C, and Ni.
[0031] As will be clearly understood, the above reference Figure 1A , 1B The elements described in , 1C and 1D can be combined arbitrarily.
[0032] Figure 2The diagram illustrates stresses that may exist when the silicon carbide chip 15 is attached to the lead frame 100 via the solder material 105. For example, the lead frame 100 may include copper. The solder material 105 may include a suitable alloy, such as AuSn, CuSn, or NiSn. When the silicon carbide chip is attached to the lead frame 100, the solder material 105 may extrude. As a result, concentrated stresses 23 may exist in the small contact area between the solder extrusion and the side 115. In addition, thermomechanical stresses 21 may be induced by the interaction between the conditions of the lead frame 100, the solder extrusion, and the side 115. In addition, induced tensile stresses 22 may exist inside the silicon carbide chip 15. As described above with reference to Figures 1A to 1D With the particular shape of the sidewall 115 discussed (eg, the angle of the sidewall or a fillet with a specified radius of curvature), these stresses can be reduced. As a result, cracking and damage to the silicon carbide chip 15 can be reduced.
[0033] In the following, reference will be made to Figures 3A to 3E A method of manufacturing a single silicon carbide chip 15 is explained at the same time, the method including singulating a workpiece 16 into single silicon carbide chips 15 .
[0034] The method may include a laser sectioning process using a multi-beam laser (MBL). According to the MBL method, a single laser beam may be shaped into multiple partial beams having a certain diameter and a certain distance using a diffractive optical element ("DOE"). For example, the diffractive optical element may determine the shape of the desired intensity pattern. By adjusting the distance between the partial beams, the fluence (i.e., energy per area) may be determined.
[0035] Figure 3A A workpiece 16 is shown, which may correspond to or include two adjacent silicon carbide chips 15, which have a first main surface 110 and a second main surface 120. A dicing kerf 125 is defined in the first main surface 110. For example, using a first MBL process, using a first intensity pattern, the dicing kerf 125 may be defined. The width w of the dicing kerf 125 may be greater than 8 μm or greater than 10 μm. The width w is measured in the horizontal direction. The depth h1 of the dicing kerf 125 may be greater than 10 μm, for example, greater than 13 μm. Thereafter, as Figure 3B As shown in , the depth of the slicing kerf 125 may extend locally to define the opening 126. For example, the depth h2 may be greater than 0.5*the thickness of the workpiece measured in the vertical direction.
[0036] Afterwards, refer to Figure 3C, the fluence of the partial beam of the slicing laser is greatly increased. Therefore, the depth of the opening 126 is further extended to a depth not much before the second main surface 120 of the workpiece 16. For example, then, the distance between the opening and the second main surface may be less than 20% (or less than 15% or less than 10%) of the thickness of the silicon carbide substrate. The distance between the opening and the second main surface may be greater than 2% (or greater than 3% or greater than 5%) of the thickness of the silicon carbide substrate. For example, the distance between the opening and the second main surface may be less than 15μm or less than 10μm, and greater than 3μm or even greater than 5μm. Due to this extension of the opening 126, the following situation may be possible: penetration to the second main surface 120 is not completed.
[0037] Afterwards, refer to Figure 3D , an annealing process may be performed. Due to the annealing, the heat affected zone and the recast material may be removed. The annealing process may be performed at a greater width of the intensity pattern of the multi-beam irradiation. As a result, the upper width f of the slicing saw kerf 125 is 1 It may be larger than 25 μm, for example larger than 30 μm.
[0038] Thereafter, the intensity pattern with a small diameter f 2 Another laser process is performed to extend the opening 126 to the second major surface 120 of the workpiece 16. For example, 2 It may be less than 5 μm. For example, the shape of the laser beam used to perform such a laser process may be adjusted to form such an intensity pattern. Figure 3E An example of a resulting workpiece is shown. As can be seen, individual silicon carbide chips 15 are separated.
[0039] Reference Figure 3E The better controlled energy impact of the described process on the second major surface 120 helps to form a rounded sidewall shape. In addition, less intermetallic compounds 109 can be formed on the side 115, and / or the intermetallic compounds 109 formed on the side 115 can be more evenly distributed. The rounded shape is more robust against the impact of solder extrusion. Therefore, chipping of the substrate material can be avoided.
[0040] Due to the form of the side surface 115 and the interconnection between the side surface 115 and the second main surface 120 as already mentioned Figures 1A to 1D As described, the formation of the intermetallic compound 109 on the side surface 115 can be influenced. As a result, the chip robustness can be significantly increased.
[0041] Figure 4Summarize the method according to the embodiment. As illustrated, the method for manufacturing a silicon carbide chip may include: defining S100 a slicing kerf in a first main surface of a workpiece, and increasing S110 the depth of the slicing kerf to obtain an opening. In addition, the method may include: further increasing S120 the depth of the opening to a position less than 20% of the thickness of the workpiece relative to the second main surface of the workpiece, performing S130 an annealing process to increase the width of the slicing kerf, and further increasing S140 the depth of the opening to singulate the workpiece into silicon carbide chips.
[0042] Although embodiments of the present invention are described above, it is apparent that additional embodiments may be implemented. For example, additional embodiments may include any subcombination of the features recited in the claims or any subcombination of the elements described in the examples given above. Therefore, the spirit and scope of the appended claims should not be limited to the description of the embodiments contained herein.
Claims
1. A silicon carbide chip, comprising: a first major surface, a second major surface, and Side, where An angle α between the side surface and a horizontal plane measured in the silicon carbide material is greater than 78°, the angle α being measured in a region adjacent to the second main surface. 2 . The silicon carbide chip according to claim 1 , wherein the angle α is greater than 80°. The silicon carbide chip as claimed in claim 2 , wherein the angle α is greater than 84°.
4. The silicon carbide chip as claimed in any one of the preceding claims, wherein the second main surface is horizontal.
5. The silicon carbide chip according to any one of claims 1 to 3, wherein the second main surface comprises an inclined portion adjacent to the side surface, an angle β between the inclined portion and the horizontal plane being greater than 5°, the angle β being measured outside the silicon carbide material. 6 . The silicon carbide chip as claimed in claim 1 , wherein the angle α is measured at a distance of less than 30 μm relative to the second main surface.
7. A silicon carbide chip as claimed in any one of the preceding claims, obtainable using a laser slicing process.
8. A silicon carbide chip, comprising: a first major surface, The second main surface, Side, and An intermetallic compound layer is adjacent to the side surface, wherein the intermetallic compound layer has a thickness of less than 2 μm in a region spaced less than 20 μm from the second main surface, the thickness being measured in a direction parallel to the first main surface.
9. A silicon carbide chip, comprising: a first major surface, a second major surface, and Side, where The radius of curvature of the intersection between the second main surface and the side surface is greater than 0.5 μm. 10 . The silicon carbide chip according to claim 9 , wherein the radius of curvature is greater than 1.0 μm.
11. The silicon carbide chip according to any one of the preceding claims, further comprising: A step portion, located at a distance h less than 20 μm measured from the first major surface, extends in the horizontal direction to a lateral width s of at least 5 μm.
12. A semiconductor device comprising: A silicon carbide chip as claimed in any one of the preceding claims, lead frame, and Solder materials, wherein the second main surface of the silicon carbide chip is arranged adjacent to the lead frame and is connected to the lead frame using the solder material.
13. A method for manufacturing a silicon carbide chip, comprising: defining a slicing kerf in a first major surface of the workpiece, increasing the depth of the slicing cut to obtain an opening; further increasing the depth of the opening to a position less than 20% of the thickness of the workpiece relative to the second major surface of the workpiece; performing an annealing process to increase the width of the slicing kerf; and The depth of the opening is further increased to singulate the workpiece into silicon carbide chips.
14. The method of claim 13, performed using a multi-beam laser.