Double-PIN type detector, preparation method and application

By using a dual PIN-type structure and junction capacitor in series in the detector, the problem of excessively long response time of the colloidal quantum dot detector is solved, which significantly improves the response speed and maintains the optical signal quantity, which significantly improves the detector's performance.

CN119069567APending Publication Date: 2024-12-03HUAZHONG UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311787567.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The response time of existing colloidal quantum dot detectors is too long, mainly due to the resistance capacitance time caused by excessive junction capacitance, which is a challenge to increase the detector response speed without reducing the amount of light.

Method used

The dual PIN detector structure is adopted to reduce the junction capacitance through series connection of junction capacitance, shorten the response time, and maintain high external quantum efficiency. The structure consists of bottom electrode, 1-N layer, 1-I layer, 1 -P-type layer, tunneling layer, sacrificial layer, 2-N-type layer, 2-I-type layer, 2-P-type layer and top electrode, and the materials include indium tin oxide, zinc oxide, PbSe colloidal quantum dot film, PbS -EDT film, gold, silver, aluminum, titanium and C60.

Benefits of technology

The response time is shortened by 50%, the gain bandwidth product is doubled, and the high external quantum efficiency is maintained, which significantly improves the performance of the detector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069567A_ABST
    Figure CN119069567A_ABST
Patent Text Reader

Abstract

The invention discloses a double-PIN type detector, a preparation method and application, and belongs to the technical field of photoelectric detectors. The structure of the double-PIN type detector sequentially comprises a bottom electrode, a 1-N type layer, a 1-I type layer, a 1-P type layer, a tunneling layer, a sacrificial layer, a 2-N type layer, a 2-I type layer, a 2-P type layer and a top electrode from bottom to top. Wherein the bottom electrode is made of indium tin oxide, the top electrode is made of gold, the 1-N type layer and the 2-N type layer are made of zinc oxide, the 1-I type layer and the 2-I type layer are PbSe colloidal quantum dot films, the tunneling layer is made of gold, the sacrificial layer is made of C60, and when the thicknesses of the 1-N type layer and the 2-N type layer are the same, the sacrificial layer is made of C60. When the thicknesses of the 1-I type layer and the 2-I type layer are the same and the thicknesses of the 1-P type layer and the 2-P type layer are the same, the light response time of the double-PIN type detector is the shortest. Compared with a traditional single-PIN detector, the double-PIN detector provided by the invention has the advantages that the response speed is increased by more than one time, the gain bandwidth product is also increased by one time, and more excellent detection performance is embodied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of photoelectric detectors, and in particular to a dual-PIN type detector, a preparation method and an application thereof. Background Art

[0002] LiDAR (LiDAR) is a radar system that uses laser beams to detect target characteristics such as position and velocity. It is widely used in autonomous driving, industrial production, augmented reality, and contactless ranging. The LiDAR detector is a time-of-flight (ToF) detector, which calculates the distance between the object and the detector by measuring the time it takes for a light beam to be emitted from the source and reflected by the detector. The response speed of the ToF detector directly determines the distance detection accuracy of LiDAR. Therefore, a high-response detector is particularly important for LiDAR.

[0003] PIN diode detectors are the mainstream device structure for time-of-flight detectors. They are widely used due to their low operating bias voltage and compact device structure. For PIN diode detectors, the response time is primarily determined by the transit time between photogenerated carriers and their collection by the electrodes, as well as the resistance-capacitance time (RC) formed by the junction capacitance and series resistance.

[0004] In recent years, lead-based colloidal quantum dot materials have been widely used to prepare short-wave infrared chips due to their advantages such as absorption coverage of the short-wave infrared band, high absorption coefficient, and easy silicon-based integration, demonstrating the excellent performance of lead-based colloidal quantum dot materials in photoelectric conversion. However, the long response time of colloidal quantum dot detectors has hindered their application in time-of-flight detectors. In colloidal quantum dot detectors, the carrier transit time ranges from a few nanoseconds to more than ten nanoseconds, which is sufficient to meet the requirements of the detector for centimeter to decimeter ranging, but the resistance-capacitance time is long, usually in the order of hundreds of nanoseconds to microseconds, resulting in a long response time of colloidal quantum dot detectors. The long resistance-capacitance time is mainly caused by the excessive junction capacitance in the detector, so it is necessary to reduce the junction capacitance to shorten the resistance-capacitance time. The common means of reducing junction capacitance are: (1) reducing the device area; (2) increasing the thickness of the device junction region; among them, although reducing the device area can significantly improve the response speed of the device, the amount of light signal received by the device will also be significantly reduced, making it more susceptible to circuit noise; while increasing the thickness of the device junction region reduces the resistance-capacitance time, it will lead to a significant increase in the transit time.

[0005] Therefore, how to improve the response speed of the detector without reducing the amount of light signal received by the detector is a technical problem that needs to be solved urgently. Summary of the Invention

[0006] To address the shortcomings of the aforementioned prior art, this application provides a dual-PIN detector, preparation method, and application. Compared to traditional PIN detectors, this dual-PIN detector reduces junction capacitance by connecting junction capacitors in series without reducing device area, thereby shortening response time while maintaining a high external quantum efficiency. Test results show that the dual-PIN detector provided in this application has a response time 50% shorter than that of traditional PIN detectors, while doubling its gain-bandwidth product.

[0007] To achieve the above objectives, this application provides the following technical solutions:

[0008] In the first aspect, an embodiment of the present application provides a dual PIN type detector, wherein the dual PIN type detector structure comprises, from bottom to top, a bottom electrode, a 1-N type layer, a 1-I type layer, a 1-P type layer, a tunneling layer, a sacrificial layer, a 2-N type layer, a 2-I type layer, a 2-P type layer and a top electrode.

[0009] Furthermore, the material of the bottom electrode is indium tin oxide (ITO), the material of the top electrode is gold (Au), and the thickness of the bottom electrode and the top electrode is 20-100 nm.

[0010] Furthermore, the material of the 1-N type layer and the 2-N type layer is zinc oxide (ZnO), and the thickness of the 1-N type layer and the 2-N type layer is 50 to 300 nm.

[0011] Furthermore, the 1-I type layer and the 2-I type layer are PbSe colloidal quantum dot films, and the thickness of the 1-I type layer and the 2-I type layer is 50 to 800 nm.

[0012] Furthermore, the 1-P type layer and the 2-P type layer are PbS-EDT thin films, and the thickness of the 1-P type layer and the 2-P type layer is 20 to 100 nm.

[0013] Furthermore, the material of the tunneling layer is at least one of gold, silver, aluminum, titanium and indium tin oxide (ITO), and the thickness of the tunneling layer is 1 to 6 nm.

[0014] Furthermore, the material of the sacrificial layer is C60, and the thickness of the sacrificial layer is 1-20 nm.

[0015] Preferably, the difference in thickness between the 1-N type layer and the 2-N type layer is between -10% and 10%. More preferably, the thickness of the 1-N type layer and the 2-N type layer are the same.

[0016] Preferably, the thickness difference between the 1-I type layer and the 2-I type layer is in the range of -10% to 10%. More preferably, the thickness of the 1-I type layer and the 2-I type layer are the same.

[0017] Preferably, the difference in thickness between the 1-P type layer and the 2-P type layer is between -10% and 10%. More preferably, the thickness of the 1-P type layer and the 2-P type layer are the same.

[0018] In a second aspect, an embodiment of the present application provides a method for preparing the aforementioned dual-PIN detector, comprising:

[0019] A 1-N type layer is prepared on the bottom electrode; a 1-I type layer is prepared on the 1-N type layer; a 1-P type layer is prepared on the 1-I type layer; a tunneling layer is prepared on the 1-P type layer; a sacrificial layer is prepared on the tunneling layer; a 2-N type layer is prepared on the sacrificial layer; a 2-I type layer is prepared on the 2-N type layer; a 2-N type layer is prepared on the 2-I type layer; and a top electrode layer is prepared on the 2-N type layer; wherein the material of the bottom electrode is indium tin oxide (ITO), the material of the top electrode is gold (Au), the thickness of the bottom electrode and the top electrode is 20 to 100 nm; the material of the 1-N type layer and the 2-N type layer is zinc oxide (ZnO ), the thickness of the 1-N type layer and the 2-N type layer is 50 to 300 nm; the 1-I type layer and the 2-I type layer are PbSe colloidal quantum dot films, and the thickness of the 1-I type layer and the 2-I type layer is 50 to 800 nm; the 1-P type layer and the 2-P type layer are PbS-EDT films, and the thickness of the 1-P type layer and the 2-P type layer is 20 to 100 nm; the material of the tunneling layer is at least one of gold, silver, aluminum, titanium and indium tin oxide (ITO), and the thickness of the tunneling layer is 1 to 6 nm; the material of the sacrificial layer is C60, and the thickness of the sacrificial layer is 1 to 20 nm.

[0020] Furthermore, the thickness difference between the 1-N type layer and the 2-N type layer is -10% to 10%, the thickness difference between the 1-I type layer and the 2-I type layer is -10% to 10%, and the thickness difference between the 1-P type layer and the 2-P type layer is -10% to 10%.

[0021] On the third aspect, the embodiments of the present application provide the application of the aforementioned dual PIN type detector in the preparation of a time-of-flight detector or a laser radar.

[0022] This application provides a dual-PIN detector and a preparation method, which, compared with the prior art, has at least the following beneficial effects:

[0023] The dual-PIN detector provided in this application has a response speed that is more than doubled compared to a traditional single-PIN detector, and its gain-bandwidth product is also doubled, while maintaining the same external quantum efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present application will be further described in detail below with reference to the accompanying drawings and preferred embodiments. However, those skilled in the art will appreciate that these drawings are drawn only for the purpose of explaining the preferred embodiments and therefore should not be construed as limiting the scope of the present application. In addition, unless otherwise specified, the drawings are merely schematic representations of the composition or structure of the described objects and may contain exaggerated representations. The drawings are not necessarily drawn to scale.

[0025] Figure 1 This is a schematic diagram of the structure of a dual PIN type detector provided in an embodiment of the present application.

[0026] Figure 2 This is a schematic diagram of the structure of a single PIN type detector provided in an embodiment of the present application.

[0027] Figure 3 This is the AC equivalent circuit diagram of the dual PIN detector provided in an embodiment of the present application.

[0028] Figure 4 A diagram of the pulse signal response time test system provided in an embodiment of the present application.

[0029] Figure 5 These are the pulse signal response curves of the single PIN detector and the dual PIN detector provided in the embodiments of the present application under different electrode areas.

[0030] Figure 6 Comparison results of the pulse signal response time of the single PIN detector and the dual PIN detector provided in the embodiments of the present application under different electrode areas.

[0031] Figure 7 The photoresponsivity test results of the dual-PIN detector with I-type layers of different thicknesses provided in the embodiments of the present application.

[0032] Figure 8 This is a comparison of the responsivity of the single PIN detector and the dual PIN detector provided in the embodiments of the present application to light sources of different wavelengths.

[0033] Figure 9 The current density results of the dual PIN detector provided in the embodiment of the present application generated by light in different wavelength ranges.

[0034] Figure 10 Comparison results of expected light absorption of dual-PIN and 3-PIN detectors obtained by Lumerical FDTD simulation provided in the embodiments of the present application. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the following, in conjunction with the accompanying drawings and embodiments, further describes the concept of this application and the technical effects produced, so as to fully understand the purpose, features and effects of this application. It should be understood that the specific embodiments described herein are only used to explain this application and are not used to limit this application. Other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of this application.

[0036] In this embodiment, a novel dual-PIN detector structure is fabricated by combining junction capacitances in series, building upon the structure of a conventional single-PIN detector. This dual-PIN detector reduces junction capacitance without reducing the area of ​​a conventional PIN detector, thereby shortening the detector's response time. Furthermore, the dual-PIN detector's external quantum efficiency is comparable to that of a single-PIN detector.

[0037] Based on this, an embodiment of the present application provides a dual PIN-type detector, in which the detector structure is, from bottom to top, a bottom electrode, a 1-N-type layer, a 1-I-type layer, a 1-P-type layer, a tunneling layer, a sacrificial layer, a 2-N-type layer, a 2-I-type layer, a 2-P-type layer, and a top electrode.

[0038] In some embodiments, the material of the bottom electrode is indium tin oxide (ITO), the material of the top electrode is gold (Au), and the thickness of the bottom electrode and the top electrode is 20-100 nm.

[0039] In some embodiments, the material of the 1-N type layer and the 2-N type layer is zinc oxide (ZnO), and the thickness of the 1-N type layer and the 2-N type layer is 50-300 nm.

[0040] In some embodiments, the type-1-I layer and the type-2-I layer are PbSe colloidal quantum dot thin films, and the thickness of the type-1-I layer and the type-2-I layer is 50 to 800 nm. In some preferred embodiments, the thickness of the type-1-I layer and the type-2-I layer is 359 nm.

[0041] In some embodiments, the 1-P type layer and the 2-P type layer are PbS-EDT thin films, and the thickness of the 1-P type layer and the 2-P type layer is 20-100 nm.

[0042] In some embodiments, the tunneling layer is made of at least one of gold, silver, aluminum, titanium, and indium tin oxide (ITO), and the thickness of the tunneling layer is 1-6 nm.

[0043] In some embodiments, the material of the sacrificial layer is C60, and the thickness of the sacrificial layer is 1-20 nm.

[0044] In some embodiments, the thickness difference between the 1-N type layer and the 2-N type layer is -10% to 10%, the thickness difference between the 1-I type layer and the 2-I type layer is -10% to 10%, and the thickness difference between the 1-P type layer and the 2-P type layer is -10% to 10%.

[0045] In some more preferred embodiments, the 1-N type layer and the 2-N type layer have the same thickness, the 1-I type layer and the 2-I type layer have the same thickness, and the 1-P type layer and the 2-P type layer have the same thickness.

[0046] Based on this, an embodiment of the present application provides a preparation method for the aforementioned dual PIN type detector, comprising: preparing a 1-N type layer on a bottom electrode; preparing a 1-I type layer on the 1-N type layer; preparing a 1-P type layer on the 1-I type layer; preparing a tunneling layer on the 1-P type layer; preparing a sacrificial layer on the tunneling layer; preparing a 2-N type layer on the sacrificial layer; preparing a 2-I type layer on the 2-N type layer; preparing a 2-N type layer on the 2-I type layer; preparing a top electrode layer on the 2-N type layer; wherein the material of the bottom electrode is indium tin oxide (ITO), the material of the top electrode is gold (Au), the thickness of the bottom electrode and the top electrode is 20 to 100 nm; the 1-N type layer and The material of the 2-N type layer is zinc oxide (ZnO), and the thickness of the 1-N type layer and the 2-N type layer is 50 to 300 nm; the 1-I type layer and the 2-I type layer are PbSe colloidal quantum dot films, and the thickness of the 1-I type layer and the 2-I type layer is 50 to 800 nm; the 1-P type layer and the 2-P type layer are PbS-EDT films, and the thickness of the 1-P type layer and the 2-P type layer is 20 to 100 nm; the material of the tunneling layer is at least one of gold, silver, aluminum, titanium and indium tin oxide (ITO), and the thickness of the tunneling layer is 1 to 6 nm; the material of the sacrificial layer is C60, and the thickness of the sacrificial layer is 1 to 20 nm.

[0047] In some embodiments, the thickness difference between the 1-N type layer and the 2-N type layer is -10% to 10%, the thickness difference between the 1-I type layer and the 2-I type layer is -10% to 10%, and the thickness difference between the 1-P type layer and the 2-P type layer is -10% to 10%.

[0048] In some more preferred embodiments, the 1-N type layer and the 2-N type layer have the same thickness, the 1-I type layer and the 2-I type layer have the same thickness, and the 1-P type layer and the 2-P type layer have the same thickness.

[0049] Based on this, an embodiment of the present application provides an application of the aforementioned dual PIN type detector in the preparation of a time-of-flight detector or a laser radar.

[0050] The following will illustrate the outstanding substantial features and significant progress of the technical solution of this application compared with the prior art through more specific embodiments.

[0051] 1. Preparation of double PIN detector

[0052] The dual-PIN detector provided in the embodiment of the present application has two PIN layers, namely a front PIN layer and a rear PIN layer, wherein the front PIN layer includes the aforementioned "1-P type layer, 1-I type layer, 1-N type layer", and the rear PIN layer includes "2-P type layer, 2-I type layer, 2-N type layer". The embodiment of the present application connects the two PIN layers in series, inserts electrodes at both ends of the two PIN layers, and separates the two PIN layers with a tunneling layer and a sacrificial layer, thus constructing a structure such as Figure 1 The double PIN detector shown in the figure is more effective than the traditional PIN structure detector (such as Figure 2 As shown in FIG, the double PIN detector has 5 more layers of material. In the process of constructing the double PIN detector in the embodiment of the present application, the following is adopted: Figure 1 As shown in the structure diagram, the corresponding layers are prepared in order from top to bottom to finally form a complete double PIN type detector. The specific steps include:

[0053] (1) Preparation of 1-N type layer on substrate (bottom electrode)

[0054] The substrate (bottom electrode) material of the present application embodiment is indium tin oxide (ITO), purchased from Xi'an Baolait Co., Ltd. The 1-N type layer is prepared by magnetron sputtering, and a ZnO target is vacuum magnetron sputtered on the bottom electrode. The method is as follows: the bottom electrode is installed on the substrate of the magnetron sputtering chamber, the sputtering power is set to 200W, and the pre-sputtering time is 5 minutes. At this time, the substrate baffle is in the closed state; after the 5-minute pre-sputtering is completed, the substrate baffle and the timing button are pressed at the same time, and the timing is 30 minutes. When the flow meter reading is less than 1 SCCM, the pressure is restored to 10 5 pa, open the hatch and remove the sputtered device (device 1).

[0055] (2) Prepare a 1-I type layer on the 1-N type layer of device 1

[0056] The specific method is as follows: dissolve oleic acid-coated PbSe quantum dots in n-octane at a concentration of 6 mg / ml to obtain a PbSe quantum dot-n-octane solution; weigh 0.92 g of lead iodide (PbI2) and 0.295 g of lead bromide (PbBr2), and completely dissolve them in 10 ml of DMF (N, N-dimethylformamide) solution; add the same volume of quantum dot-n-octane solution and DMF solution of PbI2 and PbBr2 into a container, shake for 40 seconds, and then let it stand to separate. The upper layer is transparent. , the lower layer is black; the supernatant is removed, and the remaining solution is washed with n-octane to obtain a DMF solution of PbSe quantum dots containing iodide ions and bromide ions; the DMF solution of PbSe quantum dots is centrifuged, and the liquid is drained to obtain PbSe quantum dots in the form of black powder; the quantum dots are dissolved in a mixed solvent of n-butylamine and DMF (volume ratio of 1:1), and the solution is aspirated with a pipette and spin-coated on the surface of the 1-N layer. After the spin coating is completed, annealing is performed for 10 minutes to obtain device 2 with a 1-I layer.

[0057] In the embodiments of the present application, the oleic acid-coated PbSe quantum dots cannot be directly spin-coated onto the device after dissolution. This is because the long-chain oleic acid ligands cause the quantum dots to be spaced relatively large. When the carriers generated by absorbed photons encounter the high potential barrier of oleic acid, the transition probability is greatly reduced, and the carriers have difficulty jumping between quantum dots. As a result, the number of carriers transmitted out of the active layer is extremely small, and the external quantum efficiency of the device is extremely low. Therefore, it is necessary to perform ligand exchange on the PbSe quantum dots with oleic acid ligands, replacing the oleic acid ligands with iodide ions and bromide ions with smaller potential barriers.

[0058] (3) Prepare a 1-P type layer on the 1-I type layer of device 2

[0059] The specific method is as follows: first, a layer of PbS quantum dots with an exciton absorption peak at 880nm is spin-coated on the surface of the 1-I layer of device two. Then, an acetonitrile solution with a concentration of 0.01% EDT is added to the surface, and the solution is spin-coated on the surface of device two after the EDT and the quantum dots are fully combined. Two layers of acetonitrile are spin-coated on the surface of device two to clean other residual ligands on the surface, thereby obtaining device three with a 1-P type layer.

[0060] (4) Preparation of tunneling layer on the 1-P type layer of device 3

[0061] The present embodiment adopts a thermal evaporation coating method to prepare the tunneling layer. The principle is: by heating the metal (such as gold particles) to evaporate and deposit at a certain rate onto the substrate with a lower temperature, the effect of coating the substrate surface is achieved. The specific method is: the evaporated gold particles are placed on a tungsten boat, the device to be prepared is attached to the substrate with high-temperature resistant tape, the substrate is mounted on the top of the chamber, the hatch is closed, and the molecular pump is evaporating to a vacuum of 5×10 -3Under pa, start pressing the evaporation power supply, control the evaporation rate to 0.02nm / s, wait until the deposition thickness of thermal evaporation reaches 1nm, turn off the power supply, and after the air pressure in the cabin returns to atmospheric pressure, open the cabin door and remove device 4 coated with the tunneling layer.

[0062] (5) Prepare a sacrificial layer on the tunneling layer of device 4

[0063] Referring to the thermal evaporation coating method in step (4), the C60 powder material is heated so that it evaporates and deposits on the surface of the tunneling layer of device four at a certain rate to form a sacrificial layer, wherein the evaporation rate is controlled to 0.02 nm / s and the thermal evaporation deposition thickness is 7 nm; finally, device five coated with a sacrificial layer is formed.

[0064] (6) Preparation of 2-P type layer, 2-I type layer, and 2-N type layer

[0065] By adopting the method for preparing the 1-N type layer in step (1), a 2-N type layer is prepared on the surface of the sacrificial layer of device five, thereby obtaining device six having a 2-N type layer; by adopting the method for preparing the 1-I type layer in step (2), a 2-I type layer is prepared on the surface of the 2-N type layer of device six, thereby obtaining device seven having a 2-I type layer; by adopting the method for preparing the 1-type layer in step (3), a 2-P type layer is prepared on the surface of the 2-I type layer of device six, thereby obtaining device eight having a 2-P type layer.

[0066] (7) Prepare the top electrode on the 2-P type layer of device 8

[0067] The thermal evaporation coating method in step (4) is used to heat the gold particles so that they evaporate and deposit at a certain rate onto the 2-P type layer to prepare the top electrode; ultimately, a complete detector, namely a dual PIN type detector, is obtained.

[0068] In the embodiment of the present application, the thickness difference between the 1-N type layer and the 2-N type layer in the dual PIN structure is controlled to be -10% to 10%, the thickness difference between the 1-I type layer and the 2-I type layer is controlled to be -10% to 10%, and the thickness difference between the 1-P type layer and the 2-P type layer is controlled to be -10% to 10%. Maintaining the same thickness between the 1-N type layer and the 2-N type layer, between the 1-I type layer and the 2-I type layer, and between the 1-P type layer and the 2-P type layer, respectively, optimizes the optical response of the dual PIN detector. Figure 3The equivalent circuit diagram of a dual-PIN detector is shown. Taking the I-type layer as an example, a specific analysis is performed. Assuming the thickness of the 1-I-type layer is x1 and the thickness of the 2-I-type layer is x2, when x1>x2, the detector capacitance is dominated by the junction capacitance represented by x1, while the overall detector response speed is dominated by the 2-I-type layer (determined by the junction capacitance with a smaller photocurrent). Compared to a single-PIN detector with a single I-type layer of x1 thickness, the reduction in junction capacitance is determined by the thickness of x2. The closer x2 is to x1, the greater the reduction in junction capacitance and the faster the photoresponse speed. Therefore, when x1=x2, that is, when the thickness of the 1-I-type and 2-I-type layers is the same, the detector achieves optimal photoresponse. Similarly, maintaining the same thickness between the 1-N-type and 2-N-type layers, and between the 1-P-type and 2-P-type layers, optimizes the detector's photoresponse.

[0069] 2. Comparison of optical response between single PIN detector and double PIN detector

[0070] The light response time of the double PIN detector prepared by the above method and the traditional single PIN detector was tested in the embodiment of the present application. Figure 4 As shown; wherein, the 1-P type layer, 2-P type layer of the dual PIN detector and the P type layer material of the single PIN detector are all PbS-EDT thin films, and the thickness is 20nm; the 1-I type layer, 2-I type layer of the dual PIN detector and the I type layer material of the single PIN detector are all PbSe colloidal quantum dot thin films, and the thickness is 50nm; the 1-N type layer, 2-N type layer and the N type layer material of the dual PIN detector are all zinc oxide, and the thickness is 50nm; the bottom electrode material of the dual PIN detector and the single PIN detector is indium tin oxide, and the thickness is 20nm; the top electrode material of the dual PIN detector and the single PIN detector is gold, and the thickness is 20nm; the tunneling layer material of the dual PIN detector is gold, and the thickness is 1nm; the sacrificial layer material of the dual PIN detector is C60, and the thickness is 5nm.

[0071] Figure 5 The photoresponse pulse curves of single PIN detector and double PIN detector are shown. The graph shows the photoresponse pulse curves obtained by testing electrodes with different areas. From left to right, the electrode area is 0.03mm 2 , 0.13mm 2 , 0.50mm 2 , 2.01mm 2 , 3.14mm 2 .

[0072] The pulse width corresponding to the point where the light response pulse curve drops to half peak height is taken as the response time of the detector, and the response time graph under different electrode areas is drawn, as shown in the figure. Figure 6 As shown, from Figure 6 It can be seen that the response time of the four electrodes of different areas of the dual-PIN detector provided in the embodiment of the present application is significantly shorter than that of the traditional single-PIN detector, indicating that the dual-PIN detector can reduce the junction capacitance of the detector by connecting a PIN structure layer in series on the basis of the traditional single-PIN structure, thereby shortening the light response time of the detector and reflecting better detection performance.

[0073] 3. Influence of detector absorption layer thickness on detector responsivity

[0074] Photoresponsivity is an important factor in measuring the performance of a detection device. It is defined as the ratio of the photocurrent generated by the detection device under illumination conditions to the light power incident on the detector, demonstrating the detector's ability to convert optical signals into electrical signals. The embodiment of the present application verifies the effect of the thickness of the light-absorbing layer (I-type layer) on the photoresponsivity of the detector. The specific method is: the aforementioned method is used to sequentially prepare dual-PIN detectors with I-type layers (including 1-I-type layer and 2-I-type layer) of 51nm, 194nm, 359nm, and 600nm thicknesses, respectively. The other structures of the four dual-PIN detectors remain consistent, wherein the materials of the 1-P-type layer and the 2-P-type layer are both PbS-EDT thin films with a thickness of 20nm, the materials of the 1-N-type layer and the 2-N-type layer are both zinc oxide with a thickness of 50nm, the materials of the bottom electrode and the top electrode are indium tin oxide and gold, respectively, with a thickness of 20nm, the tunneling layer material of the dual-PIN detector is gold with a thickness of 1nm, and the material of the sacrificial layer of the dual-PIN detector is C60 with a thickness of 5nm; the photoresponsivity values ​​of the four dual-PIN detectors are tested respectively.

[0075] Figure 7 This is the photoresponsivity of the dual-PIN detector under conditions of different absorption layer thicknesses. It can be seen from the figure that when the thickness of the absorption layer (1-I type layer and 2-I type layer) is 359nm, the photoresponsivity of the dual-PIN detector is the highest.

[0076] The present invention also tests the responsivity of the double PIN structure and single PIN detector with the thickness of the I-type layer of 359nm under different wavelength conditions. The test results are as follows: Figure 8 As shown. Figure 8It can be seen that when the target band to be detected is in the range of 1550-1650nm, the improved dual-PIN detector has a higher light response than the combed single-PIN detector, which means that the dual-PIN detector can improve the light response while having a faster response speed, and will not cause a loss in external quantum efficiency. The reason for this effect is that in a single-PIN detector, the absorbed light accounts for a small proportion compared to the total incident light, and part of the light leaves the detector in the form of transmission. The dual-PIN structure utilizes this part of the light and constructs a new reflective optical circuit through the high reflective properties of the top electrode (metal), while assisting optical interference under a specific film thickness to enhance absorption, so that the light response of the upper and lower layers is the same. In addition, from Figure 8 It can also be seen that under the irradiation of visible light with a wavelength of 365~780nm, the light response of the dual-PIN detector is significantly lower than that of the single-PIN detector, indicating that the dual-PIN detector can achieve the purpose of resisting visible light interference.

[0077] Figure 9 The figure shows the current density results of the dual-PIN detector under light in different wavelength ranges. It can be seen from the figure that under light with a wavelength of 1550nm, the density of the current converted by the detector is the highest. As time goes by, its current density does not decrease. Under visible light illumination of 365-780nm, the density of the current converted by the detector is lower, indicating that visible light has little interference on the dual-PIN detector during detection.

[0078] 4. Verification of photoresponsivity of multi-PIN detectors

[0079] In the embodiment of the present application, the photoresponsivity of detectors with a dual-PIN structure and a 3-PIN structure is simulated and tested using the Lumerical FDTD method, wherein the materials and thicknesses of the functional layers of the dual-PIN structure and the 3-PIN structure detectors remain the same, and the thickness of the type I layer (absorbance) is 359 nm.

[0080] The simulation test results are as follows Figure 10As shown, the photoresponsivity of a detector with a 3-PIN structure is significantly lower than that of a dual-PIN structure. This is because the front PIN structure layer blocks the light absorption effect of the rear PIN structure layer. The entire photoelectric circuit in the detector is determined by the PIN structure layer with the lowest light-to-current conversion. The dual-PIN structure detector achieves a photoresponsivity that is not lower than that of the single-PIN structure by adjusting the film thickness to match the front and rear PIN junctions. If the film thickness continues to increase, the photoresponsivity will decrease. If the 3-PIN structure is to achieve the same photoresponsivity as the single-PIN structure, its corresponding optimal film thickness needs to be smaller than that of the dual-PIN structure. Therefore, under the same film thickness conditions, such as a film thickness above 359nm, the photoresponsivity of the 3-PIN structure detector will be lower than that of the dual-PIN structure. At the same time, the effect of reducing the junction capacitance and thus the photoresponse time by connecting multiple PIN structure layers in series is not obvious. In the actual detection device preparation process, stress exists between each layer and the previous layer. In the process of preparing 3-PIN structure detectors, it is observed that the multi-layer stack is damaged by stress, making it difficult to prepare a good device.

[0081] In summary, compared with the traditional single PIN detector and 3 PIN detector, the double PIN detector provided in the embodiment of the present application has the best light response effect.

[0082] The present application has been described in detail above. Specific examples have been used in this application to illustrate the principles and implementation methods of this application. The description of the above embodiments is only intended to help understand this application and its core ideas. It should be noted that, for those skilled in the art, without departing from the principles of this application, various improvements and modifications may be made to this application, and such improvements and modifications also fall within the scope of protection of the claims of this application.

Claims

1. A dual PIN type detector, characterized in that: The dual PIN detector structure comprises, from bottom to top, a bottom electrode, a 1-N type layer, a 1-I type layer, a 1-P type layer, a tunneling layer, a sacrificial layer, a 2-N type layer, a 2-I type layer, a 2-P type layer and a top electrode.

2. The dual PIN detector according to claim 1, characterized in that: The material of the bottom electrode is indium tin oxide; the material of the 1-N type layer and the 2-N type layer is zinc oxide; the 1-I type layer and the 2-I type layer are PbSe colloidal quantum dot films, and the 1-P type layer and the 2-P type layer are PbS-EDT films; the material of the tunneling layer is at least one of gold, silver, aluminum, titanium and indium tin oxide; the material of the sacrificial layer is C60; and the material of the top electrode is gold.

3. The dual PIN type detector according to claim 2, characterized in that: The material of the tunneling layer is gold.

4. The dual PIN type detector according to claim 1, characterized in that: The thickness of the bottom electrode and the top electrode is 20 to 100 nm; the thickness of the 1-N type layer and the 2-N type layer is 50 to 300 nm; the thickness of the 1-I type layer and the 2-I type layer is 50 to 800 nm; the thickness of the 1-P type layer and the 2-P type layer is 20 to 100 nm; and the thickness of the tunneling layer is 1 to 6 nm.

5. The dual PIN type detector according to claim 4, characterized in that: The thickness of the 1-I type layer and the 2-I type layer was 359 nm.

6. The dual PIN type detector according to claim 1, characterized in that: The thickness difference between the 1-N type layer and the 2-N type layer is -10% to 10%, the thickness difference between the 1-I type layer and the 2-I type layer is -10% to 10%, and the thickness difference between the 1-P type layer and the 2-P type layer is -10% to 10%.

7. The dual PIN type detector according to claim 6, characterized in that: The 1-N type layer and the 2-N type layer have the same thickness, the 1-I type layer and the 2-I type layer have the same thickness, and the 1-P type layer and the 2-P type layer have the same thickness.

8. The method for preparing the dual PIN type detector according to claim 1, characterized in that: The following steps are involved: A 1-N type layer is prepared on the bottom electrode by magnetron sputtering; a 1-I type layer is prepared on the 1-N type layer by spin coating; a 1-P type layer is prepared on the 1-I type layer by spin coating; a tunneling layer is prepared on the 1-P type layer by thermal evaporation coating; a sacrificial layer is prepared on the tunneling layer by thermal evaporation coating; a 2-N type layer is prepared on the sacrificial layer by magnetron sputtering; a 2-I type layer is prepared on the 2-N type layer by spin coating; a 2-N type layer is prepared on the 2-I type layer by spin coating; a top electrode layer is prepared on the 2-N type layer by thermal evaporation coating; wherein the material of the bottom electrode is indium tin oxide, the material of the top electrode is gold, and the bottom electrode and the top electrode are The thickness of the electrode is 20 to 100 nm; the material of the 1-N type layer and the 2-N type layer is zinc oxide, and the thickness of the 1-N type layer and the 2-N type layer is 50 to 300 nm; the 1-I type layer and the 2-I type layer are PbSe colloidal quantum dot films, and the thickness of the 1-I type layer and the 2-I type layer is 50 to 800 nm; the 1-P type layer and the 2-P type layer are PbS-EDT films, and the thickness of the 1-P type layer and the 2-P type layer is 20 to 100 nm; the material of the tunneling layer is at least one of gold, silver, aluminum, titanium and indium tin oxide, and the thickness of the tunneling layer is 1 to 6 nm; the material of the sacrificial layer is C60, and the thickness of the sacrificial layer is 1 to 20 nm.

9. The preparation method according to claim 8, characterized in that: The thickness difference between the 1-N type layer and the 2-N type layer is -10% to 10%, the thickness difference between the 1-I type layer and the 2-I type layer is -10% to 10%, and the thickness difference between the 1-P type layer and the 2-P type layer is -10% to 10%.

10. Use of the dual PIN type detector according to any one of claims 1 to 7 in the preparation of a time-of-flight detector or a laser radar.