Solar cell and manufacturing method thereof

By using improved structures of doped regions and semiconductor layers in solar cells, including aluminum oxide layers and dielectric layers, problems of passivation characteristics and material costs in the prior art are solved, and efficiency improvement and process simplification are achieved.

CN119069575APending Publication Date: 2024-12-03TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202139.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-07-19
Filing Date
2020-04-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing solar cells have limitations in terms of passivation characteristics and material costs, and the manufacturing process is complex and it is difficult to improve efficiency.

Method used

Adopt an improved structure consisting of doped regions and semiconductor layers on the semiconductor substrate, including a first passivation layer and a second passivation layer, consisting of an aluminum oxide layer and a dielectric layer, respectively, to improve the passivation through hydrogen implantation and annealing processes. and simplify the manufacturing process.

Benefits of technology

It improves the passivation characteristics and efficiency of solar cells, reduces material costs, simplifies manufacturing processes, and enhances the hydrogen injection effect and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069575A_ABST
    Figure CN119069575A_ABST
Patent Text Reader

Abstract

A solar cell according to an embodiment of the present invention comprises: a first aluminum oxide layer on a first conductivity type region composed of a polycrystalline silicon layer having an n-type conductivity type and including hydrogen; and a first passivation layer on the first aluminum oxide layer and including a first dielectric layer including a material different from a material of the first aluminum oxide layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solar cell and a method for manufacturing the same, and more particularly, to a solar cell and a method for manufacturing the same with an improved structure and process. Background Art

[0002] A solar cell in which a semiconductor layer having a dopant is formed on at least one surface of a semiconductor substrate and used as a conductive type region has been proposed and used. Since the passivation characteristic of a solar cell has a great influence on efficiency, various methods for improving the passivation characteristic of a solar cell have been proposed.

[0003] U.S. Patent No. 9716204 discloses a method for manufacturing a solar cell, in which a first conductive type region and a second conductive type region for collecting different carriers are formed as semiconductor layers each having a dopant, and hydrogen is injected and passivated by a hydrogen atmosphere. However, when the first conductive type region and the second conductive type region are formed by semiconductor layers each having a dopant, the interface characteristics with the semiconductor substrate deteriorate, which may have limitations in improving the efficiency of the solar cell. In addition, when hydrogen is injected through a hydrogen atmosphere, the hydrogen injection effect may not be very large. In addition, in a structure in which electrodes are arranged on both sides, since the electrodes are completely formed on the rear surface, the material cost may increase, and there is no layer, structure, etc. provided for improving the passivation characteristics on the rear surface. Summary of the invention

[0004] Technical issues

[0005] An object of the present disclosure is to provide a solar cell capable of improving efficiency and a method for manufacturing the same.

[0006] More specifically, an object of the present disclosure is to provide a solar cell capable of improving passivation characteristics, reducing material costs, and simplifying a manufacturing process by improving a passivation structure, and a method for manufacturing the solar cell.

[0007] In particular, an object of the present disclosure is to provide a solar cell capable of improving passivation characteristics, reducing material costs and simplifying manufacturing processes by improving a passivation structure, and a method for manufacturing the solar cell according to the characteristics of a doped region and a semiconductor layer in a structure having a doped region composed of a portion of a semiconductor substrate and a semiconductor layer formed on the semiconductor substrate.

[0008] Technical Solution

[0009] A solar cell according to an embodiment of the present disclosure includes: a first passivation layer, the first passivation layer including a first aluminum oxide layer located on a first conductive type region, the first conductive type region consisting of a polysilicon layer having n-type conductivity and having hydrogen; and a first dielectric layer, the first dielectric layer being located on the first aluminum oxide layer and including a material different from the first aluminum oxide layer. In this case, the first conductive type region may be formed on a first surface of a semiconductor substrate. A first electrode electrically connected to the first conductive type region through the first passivation layer may also be included.

[0010] The first dielectric layer may include silicon nitride, silicon oxide, or silicon oxynitride.

[0011] The thickness of the first aluminum oxide layer may be smaller than the thickness of the first dielectric layer.

[0012] The hydrogen content per unit volume in the first aluminum oxide layer may be greater than the hydrogen content per unit volume in the first dielectric layer.

[0013] The solar cell may further include a silicon oxide layer between the first conductive type region and the first passivation layer.

[0014] The first surface of the semiconductor substrate may be a rear surface of the semiconductor substrate, the first electrode may include a plurality of finger electrodes extending in one direction, and the first dielectric layer may function as an anti-reflection film.

[0015] The solar cell may further include: a second conductive type region formed at or on the second surface of the semiconductor substrate and having p-type conductivity; a second passivation layer including a second aluminum oxide layer on the second conductive type region, and a second dielectric layer on the second aluminum oxide layer and including a material different from the second aluminum oxide layer; and a second electrode electrically connected to the second conductive type region through the second passivation layer.

[0016] The second conductive type region may be composed of a doped region constituting a portion of the semiconductor substrate, and the first aluminum oxide layer and the second aluminum oxide layer may have the same material, composition, and thickness.

[0017] On the other hand, a solar cell according to an embodiment of the present disclosure includes: a first conductive type region, which is formed on a first surface of a semiconductor substrate and is composed of a polysilicon layer having a first conductive type; and a second conductive type region, which is formed on a second surface of the semiconductor substrate and is composed of a doped region having a second conductive type. Here, the first passivation layer located on the first conductive type region and the second passivation layer located on the second conductive type region may have the same stacked structure. For example, the first passivation layer and the second passivation layer may each include an aluminum oxide layer located on the first conductive type region or the second conductive type region and a dielectric layer located on the aluminum oxide layer and including a material different from the aluminum oxide layer. And the solar cell may include: a first electrode, which is electrically connected to the first conductive type region through the first passivation layer; and a second electrode, which is electrically connected to the second conductive type region through the second passivation layer.

[0018] The dielectric layer may include silicon nitride, silicon oxide, or silicon oxynitride. The thickness of the aluminum oxide layer may be less than the thickness of the dielectric layer.

[0019] In addition, the method for manufacturing a solar cell according to an embodiment of the present disclosure includes the following steps: forming a first conductive type region composed of a polysilicon layer having n-type conductivity on a first surface of a semiconductor substrate; forming a passivation layer, the step of forming the passivation layer includes forming a first passivation layer on the first conductive type region; and forming an electrode, the step of forming the electrode forms a first electrode electrically connected to the first conductive type region through the first passivation layer. The step of forming the first passivation layer includes a process of forming a first aluminum oxide layer having hydrogen on the first conductive type region, and a process of forming a first dielectric layer located on the first aluminum oxide layer and including a material different from the first aluminum oxide layer.

[0020] Hydrogen included in the first aluminum oxide layer may be injected into at least one of the first conductive type region and the semiconductor substrate through an annealing process performed in at least one of the step of forming the passivation layer and the step of forming the electrode.

[0021] The method may further include the following steps: before forming the passivation layer, forming a second conductive type region at or on the second surface of the semiconductor substrate. The step of forming the passivation layer may further include forming a second passivation layer on the second conductive type region. The step of forming the second passivation layer may include a process of forming a second aluminum oxide layer on the second conductive type region, and a process of forming a second dielectric layer located on the second aluminum oxide layer and including a material different from the second aluminum oxide layer.

[0022] The process of forming the first aluminum oxide layer and the process of forming the second aluminum oxide layer may be performed together through the same process.

[0023] In the step of forming the passivation layer, the process of forming the first dielectric layer may be performed after performing the process of forming the second dielectric layer. The process of forming the second dielectric layer may include a first annealing process in which hydrogen in the first aluminum oxide layer is implanted into at least one of the first conductive type region and the semiconductor substrate.

[0024] The process of forming the first dielectric layer may be followed by a deposition process of the first dielectric layer after the first annealing process is performed.

[0025] The process of forming the first aluminum oxide layer may be performed by an atomic layer deposition method or a plasma induced chemical vapor deposition method.

[0026] The process of forming the electrode may include a second annealing process in which hydrogen in the first aluminum oxide layer is implanted into at least one of the first conductive type region and the semiconductor substrate. The first dielectric layer may serve as a capping layer to prevent external diffusion of hydrogen in the second annealing process.

[0027] The first dielectric layer may include silicon nitride, silicon oxide, or silicon oxynitride.

[0028] The method may further include the step of forming an uneven portion on the second surface of the semiconductor substrate by reactive ion etching.

[0029] Beneficial Effects

[0030] In this embodiment, since the second conductive type region composed of the doped region and the first conductive type region composed of the semiconductor layer are provided, the incident interference of light from the front surface of the semiconductor substrate can be minimized, and the degradation of the composite characteristics caused by the first conductive type region can be minimized. Thus, the characteristics of the solar cell can be improved.

[0031] In this structure, the first passivation layer located on the first conductive type region is provided with a first aluminum oxide layer and a first dielectric layer, so that the hydrogen passivation effect can be achieved through the first aluminum oxide layer while the hydrogen injection effect and reliability can be improved through the first dielectric layer. In addition, the second passivation layer located on the second conductive type region is provided with a second aluminum oxide layer and a second dielectric layer, so that field effect passivation can be achieved through the second aluminum oxide layer and reliability can be improved through the second dielectric layer.

[0032] As described above, the passivation characteristics and efficiency of the solar cell can be improved by configuring a first passivation layer and a second passivation layer having a material and a stacked structure that take into account all of the crystal structure, junction structure, and conductivity type of the first conductive type region and the second conductive type region. In particular, although the first aluminum oxide layer and the second aluminum oxide layer implement different passivations in consideration of the crystal structure, junction structure, conductivity type, etc. of the first conductive type region and the second conductive type region, they can have the same material. In addition, the first dielectric layer and the second dielectric layer can be formed thereon by the same material. The manufacturing process can be simplified by providing a first passivation layer and a second passivation layer having the same stacked structure as described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a cross-sectional view schematically illustrating a solar cell according to an embodiment of the present disclosure.

[0034] Figure 2 yes Figure 1 Schematic plan view of a solar cell shown.

[0035] Figure 3 is a cross-sectional view schematically illustrating a solar cell according to a modification example of the present disclosure.

[0036] Figure 4 is a cross-sectional view schematically illustrating a solar cell according to another modification example of the present disclosure.

[0037] Figure 5 is a schematic diagram illustrating a recombination model due to defects and fixed charge passivation for preventing it.

[0038] Figure 6 is a diagram illustrating an energy band diagram of a semiconductor substrate, a tunneling layer, and a first conductive type region in a solar cell according to an embodiment of the present disclosure.

[0039] Figure 7 is a graph illustrating an implicit open circuit voltage according to the material of the passivation layer.

[0040] Figure 8 is a cross-sectional view schematically illustrating a solar cell according to another modification example of the present disclosure.

[0041] Fig. 9 is a flow chart of a method of manufacturing a solar cell according to an embodiment of the present disclosure.

[0042] Figures 10a to 10j is a cross-sectional view illustrating a method of manufacturing a solar cell according to an embodiment of the present disclosure.

[0043] Fig.11is a cross-sectional view schematically illustrating a portion of a solar cell according to a modification of the present disclosure.

[0044] Fig.12 : is a graph illustrating the results of measuring the implicit open-circuit voltage of the solar cells according to Embodiment 1 and Comparative Examples 1 and 2.

[0045] Fig.13 (a) is a photoluminescence photograph after the first conductive type region and the second conductive type region are formed in Embodiment 1, and Fig.13 (b) is a photoluminescence photograph after the first passivation layer and the second passivation layer are formed in Embodiment 1.

[0046] Fig.14 (a) is a photoluminescence photograph after the first conductive type region and the second conductive type region are formed in Comparative Example 1, and Fig.14 (b) is a photoluminescence photograph after forming the first passivation layer and the second passivation layer in Comparative Example 1. DETAILED DESCRIPTION

[0047] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. However, needless to say, the present disclosure is not limited to these embodiments and can be modified in various forms.

[0048] In the accompanying drawings, in order to clearly and briefly describe the present disclosure, illustration of parts not related to the description is omitted, and the same reference numerals are used for the same or very similar parts throughout the specification. In the accompanying drawings, the thickness, width, etc. are enlarged or reduced to make the description clearer, and the thickness, width, etc. of the present disclosure are not limited to those shown in the accompanying drawings.

[0049] Throughout the specification, when a component is referred to as "comprising" another component, it does not exclude other components, and unless otherwise specifically stated, other components may be further included. In addition, when a portion of a layer, film, region, plate, etc. is referred to as being "on" another portion, this includes not only the case of being "directly on" another portion, but also the case of other portions being located in the middle. When the portion of a layer, film, region, plate, etc. is referred to as being "directly on" another portion, this means that no other portion is located in the middle.

[0050] Hereinafter, a solar cell and a method of manufacturing the same according to an embodiment of the present disclosure will be described in detail with reference to the accompanying drawings. In the present disclosure, the expression "first" or "second" is only used to distinguish each other, and the present disclosure is not limited thereto.

[0051] Figure 1 is a cross-sectional view schematically illustrating a solar cell according to an embodiment of the present disclosure, and Figure 2 yes Figure 1Schematic plan view of a solar cell shown.

[0052] Reference Figure 1 and Figure 2 , the solar cell 100 according to the present embodiment includes: a semiconductor substrate 110; a first conductive type region 20 formed on a first surface (e.g., rear surface) of the semiconductor substrate 110 and composed of a polysilicon layer having a first conductive type (e.g., n-type conductive type); a first passivation layer 22 located on the first conductive type region 20; and a first electrode 42 electrically connected to the first conductive type region 20 through the first passivation layer 22. In addition, the solar cell 100 according to the present embodiment may include: a second conductive type region 30 formed at or on a second surface (e.g., front surface) of the semiconductor substrate 110 and having a second conductive type (e.g., p-type conductive type); a second passivation layer 32 located on the second conductive type region 30; and a second electrode 44 electrically connected to the second conductive type region 30 through the second passivation layer 32. This will be described in more detail.

[0053] The semiconductor substrate 110 may be formed of a crystalline semiconductor. For example, the semiconductor substrate 110 may be formed of a single crystal semiconductor or a polycrystalline semiconductor (e.g., single crystal silicon or polycrystalline silicon). In particular, the semiconductor substrate 110 may be formed of a single crystal semiconductor (e.g., a single crystal semiconductor wafer, more specifically, a single crystal silicon wafer). As described above, when the semiconductor substrate 110 is formed of a single crystal semiconductor (e.g., single crystal silicon), the solar cell 100 constitutes a single crystal solar cell (e.g., a single crystal silicon solar cell). As described above, the solar cell 100 based on the semiconductor substrate 110 formed of a crystalline semiconductor having high crystallinity and fewer defects may have excellent electrical characteristics.

[0054] The semiconductor substrate 110 may include a base region 10 having a first conductivity type or a second conductivity type by including a first conductivity type dopant or a second conductivity type dopant at a relatively low doping concentration. The first conductivity type region 20 and the second conductivity type region 30 have a higher doping concentration than the base region 10, and the first conductivity type region 20 and the second conductivity type region 30 have a conductivity type different from that of the base region 10, or have the same conductivity type as the base region 10. For example, the base region 10 may have a first conductivity type (e.g., an n-type conductivity type).

[0055] The front surface and / or the rear surface of the semiconductor substrate 110 may be textured to have an uneven portion. In the present embodiment, the front surface and / or the rear surface of the semiconductor substrate 110 may have uneven portions 112 and 114 formed by texturing. When the uneven portions 112 and 114 are formed on the front surface and / or the rear surface of the semiconductor substrate 110 by such texturing, the reflectivity of light incident through the front surface and / or the rear surface of the semiconductor substrate 110 may be reduced. Therefore, the amount of light reaching the pn junction formed by the base region 10 and the second conductive type region 30 may be increased, thereby minimizing light loss.

[0056] More specifically, in the present disclosure, the uneven portions 112 and 114 may include a first uneven portion 112 formed on the front surface (front side surface) of the semiconductor substrate 110 and a second uneven portion 114 formed on the rear surface (rear side surface) of the semiconductor substrate 110. Therefore, reflection of light incident on the front and rear surfaces of the semiconductor substrate 110 can be prevented, so that light loss in the solar cell 100 having a double-sided structure as in the present embodiment can be effectively reduced. However, the present disclosure is not limited thereto. As a modified example, as Figure 3 As shown, the first uneven portion 112 may be provided on the front surface of the semiconductor substrate 110, but the second uneven portion 114 may not be provided on the rear surface of the semiconductor substrate 110. As another modification, the first uneven portion 112 may not be provided on the front surface of the semiconductor substrate 110, but the second uneven portion 114 may be provided on the rear surface of the semiconductor substrate 110. As another modification, the first uneven portion 112 and the second uneven portion 114 may not be provided on the semiconductor substrate 110.

[0057] The first uneven portion 112 located on the front surface of the semiconductor substrate 110 may include a first uneven portion 112a and a second uneven portion 112b to minimize light loss. The second uneven portion 112b may be formed on the first uneven portion 112a, more specifically, may be formed on an outer surface constituting the first uneven portion 112a, and may have a smaller size than the corresponding first uneven portion 112a. Therefore, the average size of the second uneven portion 112b may be smaller than the average size of the first uneven portion 112a, and at least one, for example, a plurality of second uneven portions 112b may be located on each outer surface constituting the first uneven portion 112a. The first uneven portion 112a and the second uneven portion 112b may be formed by different methods.

[0058] The outer surface of the first uneven portion 112a may be composed of a specific crystal plane. For example, the first uneven portion 112a may have an approximately pyramidal shape formed by four outer surfaces that are (111) planes. The first uneven portion 112a may be formed by anisotropic etching by wet etching. When the first uneven portion 112a is formed by wet etching, the first uneven portion 112a may be formed in a short time by a simple process. The process of forming the first uneven portion 112a by wet etching will be described in more detail later.

[0059] The second uneven portion 112b may be formed on the outer surface (e.g., (111) plane) of the first uneven portion 112a while having a fine size. The second uneven portion 112b may have a pointed end, but the present disclosure is not limited thereto, and the second uneven portion 112b may have a rounded end. The average size of the second uneven portion 112b may be smaller than the average size of the first uneven portion 112a. In addition, the size deviation of the second uneven portion 112b may be smaller than the size deviation of the first uneven portion 112a. This is also because the average size of the second uneven portion 112b is smaller, and also because the process of the second uneven portion 112b is performed based on isotropic etching. As described above, in the present embodiment, a uniform and fine second uneven portion 112b is formed on the outer surface of the first uneven portion 112a. The second uneven portion 112b may be formed by isotropic etching by dry etching. For example, as dry etching, reactive ion etching (RIE) may be used. According to reactive ion etching, the second uneven portion 112b may be finely and uniformly formed.

[0060] In the present embodiment, the second uneven portion 114 formed on the rear surface of the semiconductor substrate 110 may include a first uneven portion 114a. For the first uneven portion 114a of the second uneven portion 114, the description of the first uneven portion 112a of the first uneven portion 112 may be applied as it is, and its detailed description will be omitted. As described above, when the second uneven portion 114 of the semiconductor substrate 110 has only the first uneven portion 114a and has a shape different from the first uneven portion 112 having the first uneven portion 112a and the second uneven portion 112b, reflection from the front surface of the semiconductor substrate 110 having a large amount of incident light can be effectively prevented by the first uneven portion 112, and the second uneven portion 114 can have a simple structure, thereby simplifying the manufacturing process of the solar cell 100.

[0061] The present disclosure may not be limited to the shapes, average sizes, size deviations, etc. of the first uneven portion 112a, the second uneven portion 112b, and the first uneven portion 114a, and the shapes, average sizes, size deviations, etc. of the first uneven portion 112a, the second uneven portion 112b, and the first uneven portion 114a may be variously deformed. In addition, the first uneven portion 112 formed on the front surface of the semiconductor substrate 110 may not include at least one of the first uneven portion 112a and the second uneven portion 112b, or the second uneven portion 114 may have an uneven portion other than the first uneven portion 114a, or in addition, the first uneven portion 112 and the second uneven portion 114 may have different shapes, forms, etc.

[0062] One of the first conductive type region 20 and the second conductive type region 30 having a conductive type different from that of the base region 10 constitutes at least a portion of an emitter region. The emitter region forms a pn junction with the base region 10 to generate carriers by photoelectric conversion. The other of the first conductive type region 20 and the second conductive type region 30 having the same conductive type as the base region 10 constitutes at least a portion of a surface field region. The surface field region forms an electric field that prevents carriers from being lost by recombination on the surface of the semiconductor substrate 110.

[0063] In this case, various materials that can represent n-type or p-type can be used as the first conductivity type dopant or the second conductivity type dopant. As a p-type dopant, a group III element such as boron (B), aluminum (Al), gallium (Ga) or indium (In) can be used, and as an n-type dopant, a group V element such as phosphorus (P), arsenic (As), bismuth (Bi) or antimony (Sb) can be used. For example, the p-type dopant can be boron (B), and the n-type dopant can be phosphorus (P).

[0064] For example, the base region 10 may have a first conductivity type, the first conductivity type may be an n-type and the second conductivity type may be a p-type. Then, the second conductivity type region 30 forming a pn junction with the base region 10 has a p-type. When light is irradiated to these pn junctions, the electrons generated by the photoelectric effect move toward the rear surface of the semiconductor substrate 110 and are collected by the first electrode 42, and the holes move toward the front surface of the semiconductor substrate 110 and are collected by the second electrode 44. Thus, electrical energy is generated. Then, the holes, which move slower than the electrons, may move to the front surface of the semiconductor substrate 110 instead of the rear surface, so that the conversion efficiency can be improved. However, the present disclosure is not limited thereto, and the base region 10 may also have a second conductivity type.

[0065] A second conductivity type region 30 having a second conductivity type opposite to that of the base region 10 may be formed on the front surface side of the semiconductor substrate 110. The second conductivity type region 30 may form a pn junction with the base region 10 to constitute an emitter region generating carriers by photoelectric conversion.

[0066] In the present embodiment, the second conductive type region 30 may be configured as a doped region constituting a portion of the semiconductor substrate 110. Therefore, the second conductive type region 30 may be formed by a crystalline semiconductor including a second conductive type dopant. For example, the second conductive type region 30 may be formed by a single crystal semiconductor or a polycrystalline semiconductor (e.g., single crystal or polycrystalline silicon) including a second conductive type dopant. Specifically, the second conductive type region 30 may be formed by a single crystal semiconductor (e.g., a single crystal semiconductor wafer, more specifically, a single crystal silicon wafer) including a second conductive type dopant. As described above, when the second conductive type region 30 forms a portion of the semiconductor substrate 110, the bonding characteristics with the base region 10 may be improved.

[0067] In the present embodiment, the second conductive type region 30 composed of the doped region is completely formed on the front surface side of the semiconductor substrate 110. Therefore, the semiconductor layer having a crystal structure different from the crystal structure of the semiconductor substrate 110 is not located on the front surface side of the semiconductor substrate 110. Because the semiconductor layer has a low light transmittance, when the semiconductor layer is located on the semiconductor substrate 110, light loss may occur due to the semiconductor layer. In the present embodiment, the second conductive type region 30 composed of the doped region is formed in the semiconductor substrate 110, so that the problems that occur when the semiconductor layer is located on the front surface of the semiconductor substrate 110 can be prevented.

[0068] although Figure 1 The second conductive type region 30 is illustrated as having a uniform structure with a uniform doping concentration as a whole, but the present disclosure is not limited thereto. Figure 4 As shown, the second conductive type region 30 may have a selective structure. That is, the second conductive type region 30 may include a first region 301 formed in a portion corresponding to the second electrode 44 and having a second conductive type dopant with low resistance or high doping concentration, and a second region 302 located in another portion and having a second conductive type dopant with higher resistance or lower doping concentration than the first region 301. In addition, the second conductive type region 30 may be a separate semiconductor layer having a different crystal structure from the semiconductor substrate 110 and / or located on the semiconductor substrate 110 and formed separately from the semiconductor substrate 110. Various other modifications are possible.

[0069] The tunneling layer 52 may be formed on the rear surface of the semiconductor substrate 110. The tunneling layer 52 acts as a barrier to electrons and holes so that minority carriers do not pass through, and after majority carriers are accumulated in a portion adjacent to the tunneling layer 52, only majority carriers with a specific energy or greater can pass through the tunneling layer 52. In this case, due to the tunneling effect, majority carriers with energy higher than a specific energy level can easily pass through the tunneling layer 52. In addition, the tunneling layer 52 may be used as a diffusion barrier to prevent the dopant of the first conductive type region 20 from diffusing into the semiconductor substrate 110. The tunneling layer 52 may include various materials through which a plurality of carriers can tunnel, and for example, the tunneling layer 52 may include oxides, nitrides, semiconductors, conductive polymers, and the like. For example, the tunneling layer 52 may include silicon oxide, silicon nitride, silicon oxynitride, intrinsic amorphous silicon, intrinsic polysilicon, and the like. In this case, the tunneling layer 52 may be completely formed on the rear surface of the semiconductor substrate 110. Therefore, the tunneling layer 52 may be easily formed without separate patterning.

[0070] The thickness of the tunneling layer 52 may be less than the thickness of the first passivation layer 22 or the second passivation layer 32 to fully realize the tunneling effect. For example, the thickness of the tunneling layer 52 may be 10 nm or less, and may be 0.5 nm to 10 nm (more specifically, 0.5 nm to 5 nm, for example, 1 nm to 4 nm). When the thickness of the tunneling layer 52 exceeds 10 nm, tunneling cannot occur smoothly and the solar cell 100 may not work, and when the thickness of the tunneling layer 52 is less than 0.5 nm, it may be difficult to form a tunneling layer 52 with desired quality. In order to further improve the tunneling effect, the thickness of the tunneling layer 52 may be 0.5 nm to 5 nm (more specifically, 1 nm to 4 nm). However, the present disclosure is not limited thereto, and the thickness of the tunneling layer 52 may have various values.

[0071] The first conductive type region 20 may be located on the tunneling layer 52. In this case, the first conductive type region 20 may include a semiconductor (e.g., silicon) including the same first conductive type dopant as the base region 10. In the present embodiment, the first conductive type region 20 is formed on the semiconductor substrate 110 (more specifically, on the tunneling layer 52) separately from the semiconductor substrate 110, and is formed by a semiconductor layer doped with the first conductive type dopant. Therefore, the first conductive type region 20 may be formed by a semiconductor layer having a crystal structure different from that of the semiconductor substrate 110 so as to be easily formed on the semiconductor substrate 110.

[0072] The first conductive type region 20 forms a rear electric field to prevent carriers from being lost by recombination on the surface of the semiconductor substrate 110 (more precisely, the rear surface of the semiconductor substrate 110 ).

[0073] In the present embodiment, the first conductive type region 20 is completely formed on the tunneling layer 52 on the rear surface of the semiconductor substrate 110. Since the first conductive type region 20 is formed on the tunneling layer 52 to reduce the doping region formed in the semiconductor substrate 110, it is possible to effectively prevent the increase of surface recombination caused by the doping region and damage to the semiconductor substrate 110 that may occur when the doping region is formed. Therefore, the open circuit voltage of the solar cell 100 can be greatly improved by effectively preventing surface recombination. In addition, since the first conductive type region 20 is formed as a whole, a separate patterning process is not required.

[0074] The first passivation layer 22 is formed on the rear surface of the semiconductor substrate 110, more precisely, on the first conductive type region 20 located on the semiconductor substrate 110, and the first electrode 42 is formed by passing through the first passivation layer 22 (i.e., through the opening 102) and is electrically connected (e.g., in contact with) the first conductive type region 20. In addition, the second passivation layer 32 is formed on the front surface of the semiconductor substrate 110, more precisely, on the second conductive type region 30 formed in the semiconductor substrate 110, and the second electrode 44 is formed by passing through the second passivation layer 32 (i.e., through the opening 104) and is electrically connected (e.g., in contact with) the second conductive type region 30.

[0075] The first passivation layer 22 may be substantially completely formed on the rear surface of the semiconductor substrate 110 except the opening 102 corresponding to the first electrode 42. The second passivation layer 32 may be substantially completely formed on the front surface of the semiconductor substrate 110 except the opening 104 corresponding to the second electrode 44.

[0076] In the present embodiment, the first passivation layer 22 may be located on the first conductive type region 20, and may include a first aluminum oxide layer 22a having hydrogen, and a first dielectric layer 22b located on the first aluminum oxide layer 22a and including a material different from that of the first aluminum oxide layer 22a. The second passivation layer 32 may include a second aluminum oxide layer 32a located on the second conductive type region 30, and a second dielectric layer 32b located on the second aluminum oxide layer 32a and including a material different from that of the second aluminum oxide layer 32a.

[0077] Here, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a are basically composed of aluminum oxide including aluminum and oxygen, and play different roles. This is because the first aluminum oxide layer 22a is located on the first conductive type region 20 as a semiconductor layer (for example, a polycrystalline semiconductor layer, in particular, a polycrystalline semiconductor layer having n-type conductivity) on the rear surface side of the semiconductor substrate 110, and the second aluminum oxide layer 32a is located on the second conductive type region 30 formed as a part of the semiconductor substrate 110 from the front surface side of the semiconductor substrate 110. More specifically, the first aluminum oxide layer 22a positioned adjacent to the first conductive type region 20 composed of a polycrystalline semiconductor layer (in particular, an n-type polycrystalline semiconductor layer) can be used as a hydrogen injection layer for implementing hydrogen passivation by injecting hydrogen into the semiconductor substrate 110 and / or the first conductive type region 20. In addition, the second aluminum oxide layer 32a positioned adjacent to the semiconductor substrate 110 (in particular, the p-type second conductive type region 30) can be used as a fixed charge passivation layer that prevents recombination using fixed charges. This will be described in more detail after describing the first dielectric layer 22 b and the second dielectric layer 32 b .

[0078] The first dielectric layer 22b located on the first aluminum oxide layer 22a can be used as a capping layer that prevents hydrogen from being emitted to the outside during the annealing process of injecting hydrogen into the first aluminum oxide layer 22a used as a hydrogen injection layer. In addition, when the first electrode 42 has a predetermined pattern and has a double-sided light receiving structure in which light is incident on both sides, the first dielectric layer 22b can be used as an anti-reflection layer to prevent reflection of light incident on the rear surface of the semiconductor substrate 110. In addition, the first dielectric layer 22b can be used as a protective layer covering the first aluminum oxide layer 22a to protect the first aluminum oxide layer 22a from external acidic substances, etc. Therefore, compared with the case of using the first aluminum oxide layer 22a alone, when the stacked structure of the first aluminum oxide layer 22a and the first dielectric layer 22b is used, the reliability is more excellent.

[0079] The second dielectric layer 32b located on the second aluminum oxide layer 32a may be used as an anti-reflection layer that prevents reflection of light incident on the front surface of the semiconductor substrate 110. In addition, the second dielectric layer 32b may be used as a protective layer covering the second aluminum oxide layer 32a to protect the second aluminum oxide layer 32a from external acidic substances, etc. Therefore, when the stacked structure of the second aluminum oxide layer 32a and the second dielectric layer 32b is used, the reliability is more excellent compared to the case where the second aluminum oxide layer 32a is used alone.

[0080] For example, the first dielectric layer 22b may include silicon nitride, silicon oxide, or silicon oxynitride. The second dielectric layer 32b may include silicon nitride, silicon oxide, or silicon oxynitride. For example, when the first dielectric layer 22b and the second dielectric layer 32b are formed of silicon nitride, the functions of a capping layer, an anti-reflection layer, and a protective layer may be effectively performed. However, the present disclosure is not limited thereto.

[0081] In the present embodiment, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a can be formed simultaneously with the same process to have the same material, composition and thickness. As described above, even when the first aluminum oxide layer 22a and the second aluminum oxide layer 32a play different roles, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a are formed simultaneously, so the manufacturing process can be simplified. In addition, the first dielectric layer 22b and the second dielectric layer 32b can have different materials, compositions and / or thicknesses. For example, the first dielectric layer 22b and the second dielectric layer 32b can be made of the same material, but can have different compositions and / or thicknesses. This is because the first dielectric layer 22b and the second dielectric layer 32b are formed in separate processes.

[0082] However, the present disclosure is not limited thereto. Therefore, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a can be formed in different separate processes to have different materials, compositions and / or thicknesses. Alternatively, the first dielectric layer 22b and the second dielectric layer 32b can be formed simultaneously in the same process to have the same material, composition and thickness. Various other modifications are possible.

[0083] As described above, even when having the same material, composition, and thickness, the first aluminum oxide layer 22a positioned adjacent to the first conductive type region 20 composed of a polycrystalline semiconductor layer (specifically, an n-type polycrystalline silicon semiconductor layer) and the second aluminum oxide layer 32a positioned adjacent to the semiconductor substrate 110 (specifically, the p-type second conductive type region 30) can play different roles. More specifically, the first aluminum oxide layer 22a can be used as a hydrogen injection layer, and the second aluminum oxide layer 32a can be used as a fixed charge passivation layer. This will refer to Figure 5 and Figure 6 Let's describe it in more detail.

[0084] Figure 5 is a schematic diagram illustrating a recombination model due to defects (trapping sites) and fixed charge passivation for preventing it. Figure 6 is a diagram illustrating an energy band diagram of a semiconductor substrate, a tunneling layer, and a first conductive type region in a solar cell according to an embodiment of the present disclosure.

[0085] Reference Figure 5, through the holes in the valence band, the electrons in the conduction band and the unoccupied trap energy levels, the recombination caused by defects is generated, thereby deteriorating the passivation characteristics. Figure 5 As shown by the arrow (1) in the figure, the excited electron is bound to the trap level and Figure 5 As shown by the arrow (2), the electron in the trap level is combined with the hole and recombination may occur. Then, since the unoccupied trap level re-exists, the process repeats. Figure 5 The process is shown by arrows (1) and (2), and compounding can occur continuously.

[0086] Fixed charge passivation is achieved by the fixed charges included in the passivation layer being passed through Figure 5 The process shown by the arrow (1) prevents the occurrence of electron-hole recombination by unbinding the electrons bound to the trap energy level. In this case, since the unoccupied trap energy level continues to exist, the process is repeated again. Figure 5 The process is shown by arrows (1) and (2), and compounding may occur.

[0087] When the first conductive type region 20 composed of an n-type polycrystalline semiconductor layer tunnel-junctioned to the semiconductor substrate 110 through the tunnel layer 52 is provided as in the present embodiment, Figure 6 As shown, the alignment and tunnel junction connection are such that the Fermi levels of the semiconductor substrate 110 and the first conductive type region 20 have the same value. Figure 6 When the electrons in the conduction band in the semiconductor substrate 110 pass through the tunnel layer 52, they can easily move to the conduction band of the first conductive type region 20. On the other hand, the holes in the semiconductor substrate 110 do not pass through the tunnel layer 52. That is, the tunnel layer 52 serves as an energy barrier for the holes. Therefore, even if Figure 5 The electrons excited by the process shown in the arrow (1) are bound to the trap energy level, and the electrons bound to the trap energy level are released by energy such as external heat, light, etc., or occupy the trap energy level in this state, thereby preventing other electrons from being captured. Therefore, even if the electrons are bound to the trap energy level, the electrons bound to the trap energy level are not recombined, so there is no need to use fixed charge passivation to release them. Therefore, since fixed charge passivation is not required in the first conductive type region 20 composed of the n-type polycrystalline semiconductor layer connected to the semiconductor substrate 110 by the tunnel junction, the polarity of the fixed charge of the passivation layer does not need to be considered.

[0088] Therefore, even if the first aluminum oxide layer 22a having a negative fixed charge is used in the first conductive type region 20 composed of an n-type polycrystalline semiconductor layer, problems caused by fixed charge passivation do not occur. Conventionally, since aluminum oxide has a negative fixed charge, it is mainly used to achieve fixed charge passivation on a semiconductor substrate having p-type conductivity, and it is not used as a passivation layer for a polycrystalline semiconductor layer (specifically, an n-type polycrystalline semiconductor layer) as in the present embodiment. This is predicted by considering only the polarity of the fixed charge without considering the crystal structure (e.g., polycrystalline structure) and the junction structure (e.g., tunnel junction) of the conductive type region.

[0089] As described above, in the present embodiment, the first aluminum oxide layer 22a is not used as a fixed charge passivation layer. Instead, in the present embodiment, the first aluminum oxide layer 22a can be used to inject hydrogen into the semiconductor substrate 110 and / or the first conductive type region 20. The hydrogen injected into the semiconductor substrate 110 and / or the first conductive type region 20 can be combined with defects in the semiconductor substrate 110 and / or the first conductive type region 20 to reduce the defect density. Thus, the recombination of electrons and holes is effectively prevented, so that the passivation characteristics can be improved and the efficiency of the solar cell 100 can be improved.

[0090] The first aluminum oxide layer 22a made of aluminum oxide may have a relatively high hydrogen content per unit volume, and hydrogen may be effectively injected even at a thin thickness. For example, the hydrogen content per unit volume of the first aluminum oxide layer 22a may be greater than the hydrogen content per unit volume of the first dielectric layer 22b (e.g., the first dielectric layer 22b made of silicon nitride). Alternatively, the hydrogen injection effect of the first aluminum oxide layer 22a may be superior to the hydrogen injection effect of the first dielectric layer 22b (e.g., the first dielectric layer 22b made of silicon nitride). Figure 7 As shown, it can be seen that the implicit open circuit voltage Voc when aluminum oxide (AlOx) is used as a passivation layer is higher than the implicit open circuit voltage Voc when silicon nitride (SiNy) is used as a passivation layer. It can be seen that the hydrogen injection effect of the first aluminum oxide layer 22a made of aluminum oxide is better than the hydrogen injection effect of the first dielectric layer 22b made of silicon nitride. In particular, when the rear surface of the semiconductor substrate 110 has an uneven portion (e.g., the second uneven portion 114), it can be seen that the implicit open circuit voltage when aluminum oxide (AlOx) is used as a passivation layer is significantly higher than the implicit open circuit voltage when silicon nitride (SiNy) is used as a passivation layer. It can be seen that when there are many defects in the semiconductor substrate 110, aluminum oxide (AlOx) has a high effect of reducing the defect density of the semiconductor substrate 110.

[0091] As described above, the hydrogen injection effect can be improved by using the first aluminum oxide layer 22a having a high hydrogen content and an excellent hydrogen injection effect. Even at a small thickness, the first aluminum oxide layer 22a can also have an excellent hydrogen injection effect, and the hydrogen injection effect can be saturated at a certain level or higher. Therefore, the thickness of the first aluminum oxide layer 22a can be less than the thickness of the first dielectric layer 22b. Thus, while maintaining the hydrogen injection effect, the thickness of the first passivation layer 22 that must be removed when forming the first electrode 42 is reduced to simplify the formation process of the first electrode 42 and improve the contact characteristics of the first electrode 42.

[0092] On the other hand, the second aluminum oxide layer 32a has p-type conductivity and is located adjacent to the second conductivity type region 30 constituting a portion of the semiconductor substrate 110, and serves to implement fixed charge passivation by negative fixed charges. Figure 5 Recombination may continuously occur in the semiconductor substrate 110 according to the processes shown in the arrows (1) and (2) of FIG. 1 , which is to prevent the recombination of electrons and holes by releasing the binding of electrons bound to the trap energy level.

[0093] As described above, in the present embodiment, different passivation is achieved by taking into account the crystal structure, junction structure, conductivity type, etc. of the first conductive type region 20 and the second conductive type region 30, but the first aluminum oxide layer 22a and the second aluminum oxide layer 32a having the same material are provided. In addition, the first dielectric layer 22b and the second dielectric layer 32b may be provided with the same material thereon. The manufacturing process can be simplified by providing the first passivation layer 22 and the second passivation layer 32 having the same stacked structure as described above.

[0094] The first electrode 42 and the second electrode 44 may have a metal electrode layer made of various conductive materials (eg, metal) and may have various shapes.

[0095] Reference Figure 2 , the first electrode 42 may include a plurality of finger electrodes 42a that are spaced apart from each other and formed in one direction while having a constant pitch. Although the drawings illustrate that the finger electrodes 42a are parallel to each other and to the edge of the semiconductor substrate 110, the present disclosure is not limited thereto. In addition, the first electrode 42 may include a bus bar electrode 42b that is formed in a direction that intersects (e.g., is orthogonal to) the finger electrodes 42a to connect the finger electrodes 42a. Only one bus bar electrode 42b may be provided, or multiple bus bar electrodes may be provided, such as Figure 2The pitch of the finger electrodes 42a shown is larger than that of the bus bar electrodes 42b. In this case, the width of the bus bar electrode 42b may be greater than the width of the finger electrodes 42a, but the present disclosure is not limited thereto. Therefore, the width of the bus bar electrode 42b may be equal to or less than the width of the finger electrodes 42a.

[0096] The second electrode 44 may include finger electrodes 44a and bus bar electrodes 44b corresponding to the finger electrodes 42a and bus bar electrodes 42b of the first electrode 42, respectively. For the finger electrodes 44a and bus bar electrodes 44b of the second electrode 44, the contents of the finger electrodes 42a and bus bar electrodes 42b of the first electrode 42 may be applied as they are. The width and pitch of the finger electrodes 42a of the first electrode 42 may be the same as or different from the width and pitch of the finger electrodes 44a of the second electrode 44. The width of the bus bar electrodes 42b of the first electrode 42 may be the same as or different from the width of the bus bar electrodes 44b of the second electrode 44, but the bus bar electrodes 42b of the first electrode 42 and the bus bar electrodes 44b of the second electrode 44 may be arranged to have the same pitch at the same position.

[0097] As described above, when the first electrode 42 and the second electrode 44 have a constant pattern, the solar cell 100 has a double-sided light receiving structure in which light can be incident on the front surface and the rear surface of the semiconductor substrate 110. Therefore, it can help to improve the efficiency of the solar cell 100 by increasing the amount of light used in the solar cell 100. However, the present disclosure is not limited to this. Therefore, the first electrode 42 and the second electrode 44 can have different planar shapes. Various other modifications are possible.

[0098] In the present embodiment, the material or composition of the first electrode 42 may be different from the material or composition of the second electrode 44 to prevent the tunneling layer 52 from being damaged when the material included in the first electrode 42 reaches the tunneling layer 52 during the firing process. For example, the glass frit content of the first electrode 42 may be less than the glass frit content of the second electrode 44. However, the present disclosure is not limited thereto, and the glass frit content of the first electrode 42 may be equal to or greater than the glass frit content of the second electrode 44. In addition, the material or composition of the first electrode 42 may be the same as the material or composition of the second electrode 44.

[0099] Alternatively, the materials or compositions of the finger electrodes 42a and 44a and the bus bar electrodes 42b and 44b may be different from each other. For example, considering that the burn-through characteristics may be different from each other when the widths of the finger electrodes 42a and 44a and the bus bar electrodes 42b and 44b are different, the glass frit contents of the finger electrodes 42a and 44a and the bus bar electrodes 42b and 44b may be different from each other. For example, the glass frit content of the finger electrodes 42a and 44a from which carriers are to be directly collected may be less than the glass frit content of the bus bars 42b and 44b. In this case, the finger electrodes 42a and 44a are formed to be in direct contact with the conductive regions 20 and 30, and the bus bar electrodes 42b and 44b may not be in direct contact with the conductive regions 20 and 30, and may be spaced apart from the conductive type regions 20 and 30, with the first passivation layer 22 or the second passivation layer 32 interposed therebetween. However, the present disclosure is not limited thereto. Therefore, the material or composition of the finger electrodes 42 a and 44 a may be the same as that of the bus bar electrodes 42 b and 44 b .

[0100] exist Figure 2 In the embodiment, three bus bar electrodes 42b and 44b are provided based on one surface of the solar cell 10, but the present disclosure is not limited thereto. The number of the bus bar electrodes 42b and 44b may be two or more, and the number, shape, arrangement, etc. may vary according to the shape of the interconnector, ribbon, wiring material, etc. attached to the bus bar electrodes 42b and 44b.

[0101] As a modified example, Figure 8 As shown, based on one surface, the number of bus bar electrodes 42b can be 6 to 33 (for example, 8 to 33, for example, 10 to 33, in particular, 10 to 15), respectively, and can be positioned at a consistent distance from each other. Here, the bus bar electrode 42b may include a pad portion 422 having a relatively wide width and arranged in a plurality in the longitudinal direction, and may also include a line portion 421 connecting the plurality of pad portions 422 in the longitudinal direction. In addition, the first electrode 42 may also include an edge line 42c, an edge electrode portion 42d, and the like. Although in Figure 8 The first electrode 42 is mainly illustrated in the above description, but the second electrode 44 may have the same or similar shape. The edge line 42c and the edge electrode portion 42d may or may not be provided, and the shapes and arrangements thereof may be variously modified.

[0102] The solar cell 100 including the bus bar electrode 42b having such a shape can be connected to an adjacent solar cell 100 or an external circuit using a linear wiring material (interconnector). The linear wiring material may have a smaller width than a ribbon having a relatively wide width (e.g., greater than 1 mm). For example, the maximum width of the wiring member may be 1 mm or less (e.g., 500 μm or less, more particularly, 250 μm to 500 μm).

[0103] Such a wiring material may have a structure including a core layer and a solder layer formed on a surface thereof. Then, a large amount of wiring materials may be effectively attached by a process of applying heat and pressure while a plurality of wiring materials are mounted on the solar cell 100. The wiring material or the core layer included therein may include a circular portion. That is, the cross-section of the wiring member or the core layer may include a portion in which at least a portion is a circular shape, a portion of a circular shape, an elliptical shape, a portion of an elliptical shape, or a curved line.

[0104] Then, while minimizing light loss and material cost by a wiring member having a small width, the moving distance of carriers can be reduced by a large number of wiring members. As described above, the efficiency of the solar cell 100 can be improved, and the material cost due to the wiring material can be reduced by reducing the moving distance of carriers while reducing light loss.

[0105] In addition, various modifications may be made to the structure, shape, and arrangement of the first electrode 42 and the second electrode 44 and the structure and shape of wiring materials, interconnectors, ribbons, and the like connected thereto.

[0106] In the present embodiment, by providing the second conductive type region 30 composed of the doped region and the first conductive type region 20 composed of the semiconductor layer, it is possible to minimize the incident interference of light from the front surface of the semiconductor substrate 110 and minimize the degradation of the composite characteristics due to the first conductive type region 20. Therefore, the characteristics of the solar cell 100 can be improved.

[0107] In this structure, since the first passivation layer 22 located on the first conductive type region 20 (particularly, the n-type semiconductor layer) includes the first aluminum oxide layer 22a and the first dielectric layer 22b, the hydrogen passivation effect can be achieved through the first aluminum oxide layer 22a while the hydrogen injection effect can be improved through the first dielectric layer 22b and the reliability can be improved. In addition, since the second passivation layer 32 located on the second conductive type region 30 (particularly, the p-type portion of the semiconductor substrate 110) includes the second aluminum oxide layer 32a and the second dielectric layer 32b, field effect passivation can be achieved through the second aluminum oxide layer 32a and the reliability can be improved through the second dielectric layer 32b.

[0108] As described above, the first passivation layer 22 and the second passivation layer 32 are configured with materials and stacked structures that take into account all of the crystal structure, junction structure, conductivity type, etc. of the first conductive type region 20 and the second conductive type region 30, so the passivation characteristics and efficiency of the solar cell 100 can be improved. In particular, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a can take into account all of the crystal structure, junction structure, conductivity type, etc. of the first conductive type region 20 and the second conductive type region 30 to achieve different passivations, but can have the same material. In addition, the first dielectric layer 22b and the second dielectric layer 32b can be formed thereon by the same material. The manufacturing process can be simplified by providing the first passivation layer 22 and the second passivation layer 32 having the same stacked structure as described above.

[0109] Will refer to Fig. 9 and Figures 10a to 10j An embodiment of a method of manufacturing the above-described solar cell 100 is described in detail. A detailed description of the contents already described in the above description will be omitted, and components not described will be described in detail.

[0110] Fig. 9 is a flow chart of a method for manufacturing a solar cell according to an embodiment of the present disclosure, and Figures 10a to 10j is a cross-sectional view illustrating a method of manufacturing a solar cell according to an embodiment of the present disclosure.

[0111] Reference Fig. 9 According to the present embodiment, the method for manufacturing the solar cell 100 includes a tunneling layer forming step S12, a semiconductor layer forming step S14, a first etching step S16, a second etching step S18, a doping step S20, an aluminum oxide layer forming step S22, a dielectric layer forming step (a first annealing step) S24, a second annealing step S26 and an electrode forming step S28.

[0112] like Fig.10a As shown, a semiconductor substrate 110 having first uneven portions 112a and 114a is prepared. For example, the first uneven portion 112a of the first uneven portion 112 may be disposed on the front surface of the semiconductor substrate 110, and the first uneven portion 114a of the second uneven portion 114 may be disposed on the rear surface of the semiconductor substrate 110.

[0113] For example, in the present embodiment, the first uneven portions 112a and 114a may be formed by wet etching. An alkaline solution (e.g., a solution containing potassium hydroxide (KOH)) may be used as an etching solution for wet etching. According to such wet etching, the first uneven portions 112a and 114a may be formed on the surface of the semiconductor substrate 110 by a simple process in a short time. In this case, an immersion process in which the two surfaces (the front surface and the rear surface) of the semiconductor substrate 110 are etched together by immersing the semiconductor substrate 110 in an etching solution may be used. Then, since the first uneven portions 112a and 114a formed on the front and rear surfaces of the semiconductor substrate 110 may be formed together by a single immersion process, the process may be simplified.

[0114] According to this wet etching, since the first uneven portions 112a and 114a are etched according to the crystal plane of the semiconductor substrate 110, the outer surfaces of the first uneven portions 112a and 114aa are formed to have a constant crystal plane (e.g., (111) plane). Therefore, the first uneven portions 112a1 and 114a may have a pyramid shape including four (111) planes, may have an average size of micrometers, and may have a relatively large first deviation in size deviation. However, the present disclosure is not limited thereto, and the first uneven portions 112a and 114a may be formed by various methods and may have various shapes, average sizes, size deviations, etc.

[0115] In the present embodiment, since the first uneven portions 112a1 and 114a are respectively formed on both surfaces of the semiconductor substrate 110, light loss can be minimized in the solar cell 110 having a double-sided light receiving structure. However, the present disclosure is not limited thereto, and it is also possible that the first uneven portions 112a and 114a are formed on one of the front surface, the rear surface, and the side surface of the semiconductor substrate 110. Alternatively, the first uneven portions 112a and 114a may not be formed on the front surface, the rear surface, and the side surface of the semiconductor substrate 110.

[0116] Then, if Fig.10bAs shown, in the tunneling layer forming step S12, the tunneling layer 52 is completely formed on the surface of the semiconductor substrate 110. More specifically, the tunneling layer 52 may be formed on the front and rear surfaces, and optionally on the side surface of the semiconductor substrate 110. Although the drawings illustrate that the tunneling layer 52 located on the front surface of the semiconductor substrate 110 and the tunneling layer 52 located on the rear surface of the semiconductor substrate are formed separately from each other, the tunneling layer 52 may be completely formed on the surface of the semiconductor substrate 110 by being formed not only on the front and rear surfaces of the semiconductor substrate 110 but also on the side surface. In this case, the tunneling layer 52 formed on the front, side, and rear surfaces of the semiconductor substrate 110 may have a shape that is continuously connected to each other.

[0117] The tunnel layer 52 may be formed by, for example, a thermal growth method, a vapor deposition method (eg, plasma enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD)), etc. However, the present disclosure is not limited thereto, and the tunnel layer 52 may be formed by various methods.

[0118] Then, if Fig.10c As shown, in the semiconductor layer forming step S14, the semiconductor layer 202 may be formed on the tunneling layer 52. More specifically, the semiconductor layer 202 is formed on the tunneling layer 52 formed on the front and rear surfaces of the semiconductor substrate 110 and optionally on the side surface of the semiconductor substrate 110. Although the drawings illustrate that the semiconductor layer 202 located on the front surface of the semiconductor substrate 110 and the semiconductor layer 202 located on the rear surface of the semiconductor substrate 110 are formed separately from each other, the semiconductor layer 202 may be completely formed on the surface of the semiconductor substrate 110 by being formed not only on the front and rear surfaces of the semiconductor substrate 110 but also on the side surface of the semiconductor substrate 110 on the tunneling layer 52. In this case, the semiconductor layer 202 formed on the front, side, and rear surfaces of the semiconductor substrate 110 may have a shape that is continuously connected to each other.

[0119] The semiconductor layer 202 may be formed by, for example, a deposition method (e.g., plasma enhanced chemical vapor deposition (PECVD)). The semiconductor layer 202 may not include a first conductive type dopant, and may include a first conductive type dopant in at least a portion of the layer or a portion thereof. In addition, the semiconductor layer 202 may be formed by a semiconductor layer (e.g., an amorphous semiconductor layer, a microcrystalline semiconductor layer, a polycrystalline semiconductor layer, e.g., an amorphous silicon layer, a microcrystalline silicon layer, or a polycrystalline silicon layer) having a crystal structure different from that of the semiconductor substrate 110. In particular, the semiconductor layer 202I may be formed by a polycrystalline semiconductor layer (e.g., a polycrystalline silicon layer) to have excellent electrical characteristics. In this case, the semiconductor layer 202 may be deposited in the form of a polycrystalline semiconductor layer, or after being deposited in the form of an amorphous semiconductor or a microcrystalline semiconductor layer, a recrystallization process may be performed to form a polycrystalline semiconductor layer.

[0120] When the semiconductor layer 202 is formed of a polycrystalline semiconductor layer including a first conductive type dopant, the semiconductor layer 202 may be regarded as a first conductive type region ( Fig.10f Therefore, in this case, it can be considered that the first conductive type region 20 is formed by the process of forming the semiconductor layer 202.

[0121] Then, if Fig.10d As shown, a first etching step S16 is performed to remove the tunneling layer 52 and the semiconductor layer 202 located on the front surface of the semiconductor substrate 110 by cross-sectional etching. When the tunneling layer 52 and the semiconductor layer 202 are also located on the side of the semiconductor substrate 110, the tunneling layer 52 and the portion of the semiconductor layer 202 located on the side surface of the semiconductor substrate 110 may be etched together in the first etching step S16. In addition, in the accompanying drawings, it is illustrated that the tunneling layer 52 is etched together with the semiconductor layer 202 in the first etching step S16. However, the present disclosure is not limited thereto, and all or part of the tunneling layer 52 may be retained without being etched in the first etching step S16.

[0122] When described in Fig.10e When the second etching step S18 is performed in the illustrated process, the first etching step S16 will be described in more detail.

[0123] Next, if Fig.10e As shown, a second etching step S18 of forming a second uneven portion 112 b on the front surface of the semiconductor substrate 110 is performed.

[0124] In the present embodiment, the first etching step S16 and the second etching step S18 can be performed by an in-situ process consisting of a continuous process in the same device. Therefore, the first etching step S16 and the second etching step S18 can be performed using an etching method that can form the second uneven portion 112b in the second etching step S18 while being able to perform lateral etching in the first etching step S16 according to process conditions.

[0125] For example, in the present embodiment, the first etching step S16 and the second etching step S18 are performed by reactive ion etching (RIE), but the process conditions may be different from each other. Reactive ion etching is a dry etching method for etching by generating plasma after supplying an etching gas (e.g., Cl2, SF6, NF3, HBr, etc.). Reactive ion etching can be applied to lateral etching. In addition, the material can be etched substantially isotropically without considering the crystal direction of the grains, etc. Therefore, according to the process conditions such as the etching gas to be used, the semiconductor layer 202 and / or the tunneling layer 52 located on the front surface of the semiconductor substrate 110 can be completely removed, and the second uneven portion 112b can be formed by etching a surface of the semiconductor substrate 110.

[0126] In the present embodiment, desired etching is achieved by adjusting process conditions such as the type, partial pressure and pressure of etching gas in the first etching step S16 and the second etching step S18. Since various known process conditions can be applied thereto, a detailed description thereof will be omitted.

[0127] The second uneven portion 112b of the first uneven portion 112 formed by the second etching step S18 is formed on the outer surface of the first uneven portion 112a, and the average size of the second uneven portion 112b is smaller than the average size of the uneven portion 112a of the first uneven portion 112. Reactive ion etching can form a fine and uniform second uneven portion 112b on the surface of the semiconductor substrate 110 regardless of the crystal orientation of the grains. In this case, the second uneven portion 112b can be formed to have a sharp upper end, can have an average size of the nanometer level, and can have a second deviation whose size deviation is smaller than the first deviation.

[0128] As described above, in the present embodiment, on the first uneven portion 112 a of the first uneven part 112 , the second uneven portion 112 b having a smaller average size than the first uneven portion 112 is formed, so that reflectivity that may occur on the surface of the semiconductor substrate 110 may be minimized.

[0129] In the present embodiment, only the first uneven portion 112 includes the first uneven portion 112a and the second uneven portion 112b, and the second uneven portion 114 includes the first uneven portion 114a and does not include the second uneven portion 112b. Since the second etching step S18 for forming the second uneven portion 112b is performed after the first etching step S16 for etching the semiconductor layer 202, the rear surface of the semiconductor substrate 110 is covered by the semiconductor layer 202, and the second etching step S18 is performed by lateral etching. Therefore, the second uneven portion 112b is formed on the front surface of the semiconductor substrate 110, and the second uneven portion 112b is not formed on the rear surface of the semiconductor substrate 110. Therefore, the passivation characteristics can be improved and the damage caused by reactive ion etching can be minimized by minimizing the surface area of ​​the rear surface of the semiconductor substrate 110 (whose incident light is relatively small).

[0130] However, the present disclosure is not limited thereto, and the first etching step S16 and the second etching step S18 may be performed by separate devices or processes, and the second etching step S18 may not be performed. Various other modifications are possible.

[0131] Then, if Fig.10f As shown, in the doping step S20, the second conductive type region 30 is formed by doping or diffusing the second conductive type dopant. In the doping step S20, the first conductive type dopant of the semiconductor layer 202 or the first conductive type region 20 can be doped, diffused or activated together. The method of forming the first conductive type region 20 and the second conductive type region 30 can use various known methods.

[0132] The first conductive type region 20 may be formed based on the semiconductor layer 202 .

[0133] For example, when the semiconductor layer 202 does not include the first conductive type dopant, the first conductive type region 20 is formed by doping or diffusing the first conductive type dopant. Various methods may be used as a method of doping or diffusing the first conductive type dopant into the semiconductor layer 202. For example, the first conductive type region 20 may be formed by doping or diffusing the first conductive type dopant by a method such as an ion implantation method, a thermal diffusion method, or a laser doping method. In this case, a heat treatment process for activation of the first conductive type dopant may be additionally performed. The heat treatment process for activation is not necessary and may be omitted according to the doping method, etc. Alternatively, after the first conductive type region 20 is formed by diffusing the first conductive type dopant by performing a heat treatment process while forming a first dopant film (e.g., a phosphosilicate glass (PSG) film) including the first conductive type dopant on the semiconductor layer 202, the first dopant film may be removed. The first dopant film may be formed by various methods such as atmospheric pressure chemical vapor deposition (APCVD), plasma enhanced chemical vapor deposition (PECVD), etc. In particular, the ion implantation method or the method of forming the first dopant film may be advantageous for cross-sectional doping.

[0134] If the first conductive type dopant is doped after the intrinsic semiconductor layer 202 is formed as described above, the intrinsic semiconductor layer 202 and the like can be more easily etched in the first etching step S16 and the like.

[0135] As another example, when at least a portion of the layer or at least a portion of the semiconductor layer 202 includes a first conductive type dopant, the first conductive type region 20 may be formed or activated by doping, diffusing or activating the first conductive type dopant included in the semiconductor layer 202 via a heat treatment process. For example, the semiconductor layer 202 may include a doped layer including a first conductive type dopant and an undoped layer not including the first conductive type dopant, and the first conductive type region 20 may be formed by doping and diffusing the first conductive type dopant of the doped layer into the undoped layer in a heat treatment process. As another example, when the semiconductor layer 202 is formed, a gas (e.g., PH3 gas) including a first conductive type dopant may be used to form the semiconductor layer 202 to have a first conductive type. Then, since the semiconductor layer 202 forms the first conductive type region 20 as it is without a separate doping process, the manufacturing process may be simplified by omitting the process for doping the semiconductor layer 202. Even in this case, a heat treatment process for activating the first conductive type dopant may be performed additionally. The heat treatment process for activation may not be necessary and may be omitted according to the doping method, etc. In addition, various modifications are possible.

[0136] The second conductive type region 30 may be formed by doping or diffusing the second conductive type dopant from the front surface of the semiconductor substrate 110 to the inside of the semiconductor substrate 110. Various methods may be used as a method of doping or diffusing the second conductive type dopant on the front surface side of the semiconductor substrate 110. For example, the second conductive type region 30 may be formed by doping or diffusing the second conductive type dopant to a partial thickness on the front surface of the semiconductor substrate 110 via a method such as an ion implantation method, a thermal diffusion method, or a laser doping method. In this case, a heat treatment process for activating the second conductive type dopant may be additionally performed. The heat treatment process for activation may not be necessary and may be omitted according to the doping method, etc. Alternatively, after the second conductive type region 30 is formed by diffusing the second conductive type dopant by performing a heat treatment process while forming a second dopant film (e.g., a borosilicate glass (BSG) film) including the second conductive type dopant on the semiconductor substrate 110, the second dopant film may be removed. The second dopant film may be formed by various methods such as atmospheric pressure chemical vapor deposition (APCVD), plasma enhanced chemical vapor deposition (PECVD), etc. In particular, an ion implantation method or a method of forming a second dopant film may be advantageous for lateral doping.

[0137] The heat treatment process for doping, diffusion or activation to form the first conductive type region 20 and the heat treatment process for doping, diffusion or activation to form the second conductive type region 30 can be performed simultaneously or separately from each other. Alternatively, after forming the first conductive type region 20 and the second conductive type region 30, the first conductive type dopant of the first conductive type region 20 and the second conductive type dopant of the second conductive type region 30 can be activated together by a co-activation heat treatment. For example, the co-activation heat treatment can be performed at various temperatures that can activate the first conductive type dopant and the second conductive type dopant together. However, the present disclosure is not limited to this. Therefore, the activation heat treatment is performed after the second conductive type region 30 is formed, and then the activation heat treatment is performed after the first conductive type region 20 is formed, and the activation heat treatment of the first conductive type region 20 and the second conductive type region 30 can also be performed separately. Various other modifications are possible.

[0138] In addition, the second conductive type dopant may be doped first, and the first conductive type dopant may be doped later, or the first conductive type dopant may be doped first, and the second conductive type dopant may be doped later. When the first conductive type region 20 and the second conductive type region 30 are formed by the first dopant film and the second dopant film, respectively, the first conductive type region 20 and the second conductive type region 30 may be formed together by heat treatment in a state where the first dopant film for forming the first conductive type region 20 and the second dopant film for forming the second conductive type region 30 are formed together, and then the first dopant film and the second dopant film may be removed. Various other modifications are possible.

[0139] After the process of forming the conductive type regions 20 and 30 including the first conductive type region 20 and the second conductive type region 30 , a cleaning process may be performed to remove byproducts, etc. remaining in the doping, diffusion, or activation heat treatment process.

[0140] Then, if Figure 10g to Figure 10i As shown, a passivation layer forming step is performed, which includes forming a first passivation layer 22 on the rear surface of the semiconductor substrate 110 and forming a second passivation layer 32 on the front surface of the semiconductor substrate 110. In this case, the step of forming the first passivation layer 22 may include a process of forming a first aluminum oxide layer 22a having hydrogen on the first conductive type region 20, and a process of forming a first dielectric layer 22b located on the first aluminum oxide layer 22a and including a material different from the first aluminum oxide layer 22a. In addition, the step of forming the second passivation layer 32 may include a process of forming a second aluminum oxide layer 32a on the second conductive type region 30, and a process of forming a second dielectric layer 32b located on the second aluminum oxide layer 32a and including a material different from the aluminum oxide layer 32a. In addition, the hydrogen included in the first aluminum oxide layer 22a may be injected into the first conductive type region 20 and / or the semiconductor substrate 110 through an annealing process performed in the passivation layer forming step and / or the electrode forming step, which will be described in more detail.

[0141] More specifically, if Figure 10gAs shown, in the aluminum oxide layer forming step S22, a process of forming the first aluminum oxide layer 22a and a process of forming the second aluminum oxide layer 32a may be performed to form the first aluminum oxide layer 22a and the second aluminum oxide layer 32a. In this case, the process of forming the first aluminum oxide layer 22a and the process of forming the second aluminum oxide layer 32a may be performed together by the same process, so that the first aluminum oxide layer 22a and the second aluminum oxide layer 32a may be formed together in the same process. Then, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a may be composed of the same layer having the same material, composition and thickness. As described above, when the first aluminum oxide layer 22a and the second aluminum oxide layer 32a are formed together in the same process, the process may be simplified.

[0142] Although the drawings illustrate that the first aluminum oxide layer 22a and the second aluminum oxide layer 32a are formed separately from each other, the first aluminum oxide layer 22a and / or the second aluminum oxide layer 32a may be completely formed on the surface of the semiconductor substrate 110 by being formed not only on the front and rear surfaces but also on the side surfaces of the semiconductor substrate 110. In this case, the first aluminum oxide layer 22a formed on the rear surface of the semiconductor substrate 110 and the second aluminum oxide layer 32a formed on the front surface of the semiconductor substrate 110 may be connected to each other from the side surfaces so that the aluminum oxide layers formed on the front surface, the side surface, and the rear surface may have a shape that is continuously connected to each other.

[0143] The present disclosure is not limited thereto. Therefore, the process of forming the first aluminum oxide layer 22a and the process of forming the second aluminum oxide layer 32a may be performed separately to form the first aluminum oxide layer 22a and the second aluminum oxide layer 32a in separate processes. In this case, the first aluminum oxide layer 22a and the second aluminum oxide layer 32a may be the same layer having the same material, composition, and thickness, or may be different layers having different materials, compositions, or thicknesses.

[0144] The first aluminum oxide layer 22a and / or the second aluminum oxide layer 32a may be formed by various methods, for example, they may be formed by an atomic layer deposition method (ALD), a plasma induced chemical vapor deposition method, etc. For example, the first aluminum oxide layer 22a and / or the second aluminum oxide layer 32a may be formed by an atomic layer deposition method using H2O, trimethylamine (TMA), etc. as a raw material.

[0145] Then, if Fig.10h As shown, in the second dielectric layer forming step S24, a second dielectric layer 32b is formed. Here, the second dielectric layer 32b may be made of silicon nitride, silicon oxide, or silicon oxynitride, and may be, for example, a silicon nitride layer made of silicon nitride.

[0146] In this embodiment, the second dielectric layer forming step S24 may include a first annealing process and a deposition process performed after the first annealing process. That is, in the second dielectric layer forming step S24, the first annealing process may be performed before the deposition process. The first annealing process and the deposition process may be performed by an in-situ process that is performed continuously in the same device.

[0147] The first annealing process may be a process in which hydrogen included in the first aluminum oxide layer 22a is implanted into the first conductive type region 20 and / or the semiconductor substrate 110, and may be performed under conditions suitable for hydrogen implantation, such as temperature, gas atmosphere, etc. For example, the first annealing process may be performed at a temperature of 300° C. to 600° C. in a nitrogen (N2) atmosphere.

[0148] The deposition process may be performed under temperature, gas atmosphere, etc., which can form the second dielectric layer 32b. For example, the deposition process may be performed by atmospheric pressure chemical vapor deposition or plasma induced chemical vapor deposition in a gas atmosphere of silane (SiH4) or ammonia (NH3).

[0149] Then, if Fig.10i As shown, in the first dielectric layer forming step S26, a first dielectric layer 22b is formed. Here, the first dielectric layer 22b may be made of silicon nitride, silicon oxide, or silicon oxynitride, and may be, for example, a silicon nitride layer made of silicon nitride.

[0150] In the present embodiment, the first dielectric layer forming step S26 may include a deposition process. The deposition process may be performed under conditions such as a temperature and a gas atmosphere at which the first dielectric layer 22 b may be formed. For example, the deposition process may be performed by atmospheric pressure chemical vapor deposition or plasma induced chemical vapor deposition performed in a gas atmosphere of silane (SiH 4 ) or ammonia (NH 3 ).

[0151] Next, if Fig.10j As shown, a first electrode 42 and a second electrode 44 connected to the first conductive type region 20 and the second conductive type region 30 , respectively, are formed in the electrode forming step S28 .

[0152] In the present embodiment, after a paste for forming the first electrode and a paste for forming the second electrode are applied on the first passivation layer 22 and the second passivation layer 32 by screen printing, etc., the first electrode 42 and the second electrode 44 may be formed while the openings 102 and 104 are formed by burning through or laser burning through the contact, etc. In this case, since the openings 102 and 104 are formed when the first electrode 42 and the second electrode 44 are fired, there is no need to add a separate process for forming the openings 102 and 104.

[0153] In this case, the second annealing process of injecting hydrogen included in the first aluminum oxide layer 22a into the first conductive type region 20 and / or the semiconductor substrate 110 can be performed by a process of firing the first electrode 42 and the second electrode 44. That is, when a firing process performed at a relatively high temperature (e.g., a temperature higher than the first annealing process) is performed in the step of forming the first electrode 42 and the second electrode 44, the hydrogen included in the first aluminum oxide layer 22a can be effectively injected into the first conductive type region 20 and / or the semiconductor substrate 110 due to the high temperature of the firing process. In this case, the first dielectric layer 22b serves as a capping layer to prevent outward diffusion of hydrogen included in the first aluminum oxide layer 22a. Due to the high temperature of the firing process and the first aluminum oxide layer 22a serving as a capping layer, hydrogen can be effectively injected into the first conductive type region 20 and / or the semiconductor substrate 110.

[0154] As another example, the openings 102 and 104 may be formed in the first passivation layer 22 and the second passivation layer 32 , respectively, and the first electrode 42 and the second electrode 44 may be formed in the openings 102 and 104 using various methods such as an electroplating method and a vapor deposition method.

[0155] As described above, in the present embodiment, the semiconductor layer 202 and / or the tunneling layer 52 located on the front surface of the semiconductor substrate 110 are removed by the first etching step S16. Therefore, the second conductive type region 30 is configured as a doped region formed by doping (or diffusing) a second conductive type dopant into the semiconductor substrate 110. The first conductive type region 20 is formed based on the semiconductor layer 202 formed on the tunneling layer 52, and the first conductive type region 20 is formed by a semiconductor layer having a crystal structure different from that of the semiconductor substrate 110. Therefore, the incident interference of light from the front surface of the semiconductor substrate 110 can be minimized, and the degradation of the composite characteristics caused by the first conductive type region 20 located on the rear surface of the semiconductor substrate 110 can be minimized. Therefore, the characteristics of the solar cell 100 can be greatly improved.

[0156] In addition, hydrogen passivation can be generated by injecting hydrogen included in the first aluminum oxide layer 22a into the first conductive type region 20 and / or the semiconductor substrate 110 through the first annealing process and / or the second annealing process, thereby improving the passivation characteristics in the solar cell 100 having the first conductive type region 20 formed of a semiconductor layer (specifically, an n-type semiconductor layer). Therefore, the efficiency of the solar cell 100 can be improved through a simple process.

[0157] In the above drawings and descriptions, it has been exemplified that the first aluminum oxide layer 22a and the first dielectric layer 22b are sequentially formed in contact with each other on the first conductive type region 20, and the second aluminum oxide layer 32a and the second dielectric layer 32b are sequentially formed in contact with each other on the second conductive type region 30. However, as Fig.11 As shown, in the heat treatment process such as the doping step S20 and the first annealing process and / or the second annealing process, the silicon oxide layers 20a and 30a may be formed and positioned between the first conductive type region 20 and the first aluminum oxide layer 22a and / or between the second conductive type region 30 and the second aluminum oxide layer 32b. The silicon oxide layers 20a and 30a may be provided together with the first passivation layer 20 and / or the second passivation layer 30 to further improve the passivation characteristics. However, the present disclosure is not limited thereto.

[0158] Hereinafter, the present disclosure will be described in more detail according to the experimental examples of the present disclosure. However, the experimental examples of the present disclosure are only for illustrating the present disclosure, and the present disclosure is not limited thereto.

[0159] Implementation Method 1

[0160] Manufacturing with Figure 1 A plurality of solar cells of the structure shown are provided. More specifically, by preparing a single crystal silicon substrate having phosphorus as a base dopant, a first conductive type region consisting of a tunneling layer consisting of a silicon oxide layer and a polycrystalline silicon layer including phosphorus (P) as a first conductive type dopant is formed, and a second conductive type region consisting of a doped region including boron as a second conductive type dopant is formed. A first aluminum oxide layer and a second aluminum oxide layer are simultaneously formed on the first conductive type region and the second conductive type region by using an atomic layer deposition method. A second dielectric layer consisting of a silicon nitride layer is formed on the second aluminum oxide layer. In the process of forming the second dielectric layer, a deposition process for forming a silicon nitride layer after performing a first annealing process can be performed at a temperature of 550° C. and under a nitrogen atmosphere. Then, a deposition process is performed on the first aluminum oxide layer to form a first dielectric layer consisting of a silicon nitride layer. Then, after the paste for forming the first electrode and the paste for forming the second electrode are applied to the first passivation layer and the second passivation layer by screen printing, they are fired, and while performing a second annealing process, the first electrode and the second electrode connected to the first conductive type region and the second conductive type region are formed by burning through.

[0161] Comparative Example 1

[0162] A plurality of solar cells were manufactured in the same manner as in Embodiment 1, except that the process of forming the first and second aluminum oxide layers and the first annealing process were not performed so that the first and second passivation layers were each made of only the silicon nitride layer.

[0163] Comparative Example 2

[0164] A plurality of solar cells were manufactured in the same manner as in Embodiment 1, except that the process of forming the first dielectric layer and the second dielectric layer was not performed so that the first passivation layer and the second passivation layer were each made of only the aluminum oxide layer.

[0165] The implicit open circuit voltage of the solar cells according to Embodiment 1 and Comparative Examples 1 and 2 was measured, and the results were Fig.12 Here, the implicit open circuit voltage is measured in a plurality of solar cells before the passivation layer is formed, after the passivation layer is formed, and after the electrode is fired, and Fig.12 The average values ​​are shown together.

[0166] Reference Fig.12 It can be seen that the implicit open circuit voltage of the solar cell according to Embodiment 1 is greatly increased after forming the passivation layer and after electrode firing, compared with the solar cells according to Comparative Examples 1 and 2. This is expected because the passivation characteristics are improved by the first passivation layer including the first aluminum oxide layer and the first dielectric layer and the second passivation layer including the second aluminum oxide layer and the second dielectric layer.

[0167] Photoluminescence (PL) photographs were taken by selecting a solar cell using a semiconductor substrate manufactured in the same or similar portion of an ingot from among a plurality of solar cells manufactured according to Embodiment 1 and Comparative Example 1, and the results were Fig.13 and Fig.14 Here, Fig.13 (a) shows a photoluminescence photograph after the first conductive type region and the second conductive type region are formed in Embodiment 1, Fig.13 (b) shows a photoluminescence photograph after the first passivation layer and the second passivation layer are formed in Embodiment 1. Fig.14 (a) shows a photoluminescence photograph after the first conductive type region and the second conductive type region are formed in Comparative Example 1, and Fig.14 (b) shows a photoluminescence photograph after the first passivation layer and the second passivation layer are formed in Comparative Example 1.

[0168] Even if Fig.13 When a ring pattern is provided in the photoluminescence photograph before forming the passivation layer in Embodiment 1, as shown in (a) of Fig.13As shown in (b), it can be seen that after the passivation layer is formed, many ring patterns disappear from the photoluminescence photograph. In the photoluminescence photograph, the ring patterns are caused by oxidation induced stacking failure (OISF, which is a defect type), and in Embodiment 1, it can be seen that the ring patterns are greatly reduced after the passivation layer is formed. Therefore, it can be seen that the passivation characteristics can be improved by forming the passivation layer according to Embodiment 1. This is expected because the hydrogen injection effect of the first aluminum oxide layer is maximized by the stacked structure of the first aluminum oxide layer and the first dielectric layer. On the other hand, as Fig.14 As shown in (a) and (b), in Comparative Example 1, it can be seen that the ring pattern still exists even after the passivation layer is formed.

[0169] The features, structures, effects, etc. according to the above-mentioned embodiments are included in at least one embodiment of the present disclosure, and are not necessarily limited to one embodiment. In addition, the features, structures, effects, etc. illustrated in the embodiments can be combined or modified in other embodiments by a person skilled in the art to which the embodiments belong. Therefore, the contents related to these combinations and modifications should be interpreted as being included in the scope of the present disclosure.

Claims

1. A solar cell, the solar cell include: Semiconductor substrates; a first conductive type region, the first conductive type region being formed on the first surface of the semiconductor substrate and consisting of a polysilicon layer having n-type conductivity; a first passivation layer including a first aluminum oxide layer located on the first conductive type region and having hydrogen, and a first dielectric layer located on the first aluminum oxide layer and including a material different from that of the first aluminum oxide layer; a second conductive type region formed at or on a second surface of the semiconductor substrate and having p-type conductivity; a second passivation layer, the second passivation layer comprising a second aluminum oxide layer located on the second conductive type region and a second dielectric layer located on the second aluminum oxide layer and comprising a material different from that of the second aluminum oxide layer; the second aluminum oxide layer is prepared by a hydrogen injection process; as well as a first electrode, the first electrode passing through the first passivation layer and electrically connected to the first conductive type region; A second electrode is provided, the second electrode passing through the second passivation layer and being electrically connected to the second conductive type region.

2. The solar cell according to claim 1, in, The second aluminum oxide layer serves as a fixed charge passivation layer.

3. The solar cell according to claim 2, in, The second aluminum oxide layer realizes fixed charge passivation through negative fixed charges.

4. The solar cell according to claim 1, in, The first dielectric layer includes silicon nitride, silicon oxide or silicon oxynitride.

5. The solar cell according to claim 1, in, The thickness of the first aluminum oxide layer is smaller than the thickness of the first dielectric layer.

6. The solar cell according to claim 1, in, A hydrogen content per unit volume in the first aluminum oxide layer is greater than a hydrogen content per unit volume in the first dielectric layer.

7. The solar cell according to claim 1, further comprising: include: A silicon oxide layer is located between the first conductive type region and the first passivation layer.

8. The solar cell according to claim 1, in, The first surface of the semiconductor substrate is a rear surface of the semiconductor substrate, the first electrode includes a plurality of finger electrodes extending in one direction, and the first dielectric layer functions as an anti-reflection film.

9. The solar cell according to claim 8, in, The second conductive type region is composed of a doped region constituting a portion of the semiconductor substrate, and The first aluminum oxide layer and the second aluminum oxide layer have the same material, composition and thickness.

10. A solar cell, the solar cell include: Semiconductor substrates; a first conductivity type region, the first conductivity type region being formed on the first surface of the semiconductor substrate and consisting of a polysilicon layer having a first conductivity type; a second conductive type region, the second conductive type region being formed on the second surface of the semiconductor substrate and consisting of a doped region having a second conductive type; a first passivation layer, wherein the first passivation layer is located on the first conductive type region; a second passivation layer, wherein the second passivation layer is located on the second conductive type region; a first electrode, the first electrode passing through the first passivation layer and electrically connected to the first conductive type region; as well as a second electrode, the second electrode passing through the second passivation layer and electrically connected to the second conductive type region, wherein the first passivation layer and the second passivation layer each include an aluminum oxide layer located on the first conductive type region or the second conductive type region and a dielectric layer located on the aluminum oxide layer and including a material different from the aluminum oxide layer; The aluminum oxide layer is prepared by a hydrogen injection process.

11. The solar cell according to claim 10, in, The dielectric layer includes silicon nitride, silicon oxide or silicon oxynitride.

12. The solar cell according to claim 10, in, The thickness of the aluminum oxide layer is smaller than the thickness of the dielectric layer.