Positive electrode composition, positive electrode, and rechargeable lithium battery
By reducing the pH value of the positive electrode composition and using tetravalent metal oxides and organic acids, the problems of lithium elution and lithium compound formation in lithium batteries are solved, the battery capacity and processability are improved, and the battery life is extended.
Patent Information
- Application Number
- CN202410681080.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-05-29
- Publication Date
- 2024-12-03
AI Technical Summary
The existing high-capacity positive electrode active substances are prone to lithium elution and lithium compound formation during the manufacturing process, resulting in increased resistance and deterioration of capacity, and deformation of fluorine-based binders leads to gelation, reducing process yield.
By reducing the pH value of the positive electrode composition, combining tetravalent or higher oxidation number of metal oxides and organic acids, lithium elution and lithium compound formation are inhibited, binder denaturation and gelation are prevented, and capacity stability is improved.
It effectively reduces lithium elution and lithium compound formation, prevents binder denaturation and gelation, improves the capacity maintenance and processability of the positive electrode, and extends the cycle life of the battery.
Smart Images

Figure CN119069638A_ABST
Abstract
Description
Technical Field
[0001] One or more embodiments of the present disclosure relate to a positive electrode composition, a positive electrode, and a rechargeable lithium battery. Background Art
[0002] Portable information devices (such as cellular phones, laptop computers and / or smart phones, etc.) or electric vehicles have used rechargeable lithium batteries with relatively high energy density and easy portability as driving power sources. Recently, research on using rechargeable lithium batteries with high energy density as driving power sources or power storage power sources for hybrid vehicles or electric vehicles has been actively conducted.
[0003] Since low-cost and high-capacity energy storage devices are highly needed and expected, positive electrodes that can achieve relatively high capacity and high energy density are being developed and studied. However, the problem with high-capacity positive electrode active materials may be that lithium is eluted from the inside of the positive electrode active material during the battery manufacturing process and reacts with the atmosphere to additionally form lithium compounds on the surface of the positive electrode active material. If the lithium inside the positive electrode active material is eluted (for example, when the lithium inside the positive electrode active material is eluted), there may be a problem of reducing the available capacity and also increasing the resistance due to the formation of lithium compounds on the surface of the positive electrode active material. In addition, in order to manufacture a positive electrode plate with a relatively high energy density, a fluorine-based binder or the like can be added to increase the adhesion of the particles, but since the fluorine-based binder may be deformed, gelation of the positive electrode composition occurs, resulting in a reduction in process yield. Summary of the invention
[0004] One or more aspects of the embodiments of the present disclosure relate to a positive electrode composition, a positive electrode, and a rechargeable lithium battery including the positive electrode composition, which, by lowering the pH (level) of the positive electrode composition, not only reduces the denaturation of the binder, but also prevents or reduces the elution of lithium inside the positive electrode active material during the electrode plate manufacturing process, and inhibits the formation of additional lithium compounds during the process, thereby preventing or reducing the denaturation of the binder and the gelation of the positive electrode composition, and effectively overcoming or inhibiting the problem of capacity degradation caused by a reduction in reversible lithium (for example, caused by a reduction in the amount of reversible lithium).
[0005] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the presented embodiments.
[0006] According to one or more embodiments of the present disclosure, a positive electrode composition for a rechargeable lithium battery includes a positive electrode active material, a binder, a metal oxide having an oxidation number of 4 or more, and an organic acid.
[0007] According to one or more embodiments of the present disclosure, a positive electrode for a rechargeable lithium battery includes a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, a binder, a metal oxide having an oxidation number of 4 or higher, and an organic acid.
[0008] According to one or more embodiments of the present disclosure, a rechargeable lithium battery includes a positive electrode, a negative electrode, and an electrolyte.
[0009] By lowering the pH of the positive electrode composition, the positive electrode composition not only reduces the denaturation of the binder, but also prevents the elution of lithium inside the positive electrode active material during the electrode plate manufacturing process, and inhibits the formation of additional lithium compounds during the process, thereby preventing or reducing the denaturation of the binder and the gelation of the positive electrode composition, and effectively inhibiting the problem of capacity degradation caused by the reduction of reversible lithium (for example, the reduction in the amount of reversible lithium). BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The above and other aspects, features and advantages of certain embodiments of the present disclosure will become more apparent through the following description in conjunction with the accompanying drawings.
[0011] Figures 1 to 4 Each is a cross-sectional view schematically showing a rechargeable lithium battery according to one or more embodiments of the present disclosure.
[0012] Figure 5 is a graph showing changes in viscosity of positive electrode compositions for Comparative Examples 1 to 3 following storage date according to one or more embodiments of the present disclosure.
[0013] Figure 6 is a graph showing changes in viscosity of positive electrode compositions according to one or more embodiments of the present disclosure for Examples 1 to 5 following storage date.
[0014] Figure 7 is a graph showing the capacity change of rechargeable lithium batteries manufactured according to one or more embodiments of the present disclosure, respectively, immediately after preparing the positive electrode composition of Comparative Example 2 and after leaving it for 3 days, and immediately after preparing the positive electrode composition of Example 1 and after leaving it for 6 days.
[0015] Figure 8 are X-ray diffraction (XRD) analysis graphs of positive electrode active materials of Comparative Example 1 and Example 1 immediately after preparation and 3 days after preparation according to one or more embodiments of the present disclosure.
[0016] Fig. 9is a graph showing pH changes according to adding an organic acid and / or a metal oxide to a positive electrode active material according to one or more embodiments of the present disclosure. DETAILED DESCRIPTION
[0017] Hereinafter, example embodiments will be described in more detail so that those skilled in the art can easily implement them. However, the present disclosure may be implemented in many different forms and is not to be construed as limited to the example embodiments set forth herein.
[0018] The terms used herein are used only to describe embodiments and are not intended to limit the present disclosure. As used herein, the singular forms "a", "an", and "the" are intended to include the plural forms unless the context clearly indicates otherwise. In addition, when describing embodiments of the present disclosure, the use of "may" refers to "one or more embodiments of the present disclosure".
[0019] As utilized herein, "combinations thereof" may refer to mixtures, laminates, composites, copolymers, alloys, blends, and / or reaction products of components, among others.
[0020] Here, it should be understood that terms such as "includes," "comprising," or "having" are intended to indicate the presence of the stated features, quantities, steps, elements, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or any combination thereof.
[0021] In the accompanying drawings, the thickness of layers, films, panels, regions, etc. may be exaggerated for clarity, and throughout the present disclosure, the same reference numerals represent the same elements, and for the sake of brevity, a repeated description thereof may not be provided. It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it may be directly on the other element, or there may be intervening elements. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0022] In some embodiments, the “layer” herein may include not only a shape or layer formed on the entire surface when viewed from a plan view, but also a shape or layer formed on a partial surface.
[0023] In one or more embodiments, the average particle size can be measured by a method that is very suitable for those skilled in the art, for example, it can be measured by a particle size analyzer (e.g., HORIBA, LA-950 laser particle size analyzer), or it can be measured by a transmission electron microscope (TEM) or a scanning electron microscope (SEM). In some embodiments, it can be measured by using a dynamic light scattering method, performing data analysis, counting the number of particles for each particle size range, and obtaining the average particle size value by data calculation. Unless otherwise defined, the average particle size can refer to the diameter (D) of particles having a cumulative volume of 50% by volume in a particle size distribution. 50 ). 50 The average particle diameter refers to the average diameter (or size) of particles whose cumulative volume corresponds to 50% by volume in a particle size distribution (e.g., cumulative distribution), and refers to a value corresponding to 50% of the particle sizes from the smallest particle accumulated in the order of the smallest particle size to the largest particle size in a distribution curve when the total number of particles is 100%. In one or more embodiments, as utilized herein, when no definition is otherwise provided, the average particle diameter refers to the diameter (D) of particles having a cumulative volume of 50% by volume in a particle size distribution obtained by randomly measuring the size (the diameter or length of the major axis) of about 20 particles in a scanning electron microscope image. 50 ). In the present disclosure, when the particle is spherical, the "diameter" means the average particle diameter, and when the particle is non-spherical, the "diameter" means the major axis length.
[0024] Here, "or" will not be interpreted as an exclusive meaning, for example, "A or B" is interpreted as including A, B and / or A+B, etc. In addition, as used herein, the term "and / or" includes any and all combinations of one or more of the relevant listed items. Expressions such as "at least one of...", "one of..." and "selected from" modify the entire list of elements when following a list of elements, without modifying the individual elements of the list. For example, "at least one of a, b and c", "at least one selected from a, b and c", "at least one selected from a to c", etc. can represent only a, only b, only c, both a and b (for example, at the same time), both a and c (for example, at the same time), both b and c (for example, at the same time), all of a, b and c, or their variations. Depending on the circumstances, the " / " used herein can be interpreted as "and" or as "or".
[0025] As utilized herein, the term "metal" is interpreted as a concept including common metals, transition metals, and metalloids (semimetals).
[0026] Positive electrode composition
[0027] In one or more embodiments, a positive electrode composition for a rechargeable lithium battery may include a positive electrode active material, a binder, a metal oxide having an oxidation number of 4 or higher, and an organic acid. The positive electrode composition not only suppresses the denaturation of the binder by lowering the pH due to the organic acid, but also effectively suppresses the problem of lithium elution in the positive electrode active material by including a tetravalent or higher valent metal oxide, thereby preventing or reducing the formation of additional lithium compounds. Therefore, it can also prevent or reduce the denaturation of the binder, effectively prevent or reduce the gelation of the positive electrode composition, and even solve or overcome the problem of capacity degradation caused by the reduction of reversible lithium (e.g., due to the reduction of the amount of reversible lithium).
[0028] Metal oxides
[0029] The metal oxide according to one or more embodiments is not particularly limited as long as it is an oxide including a metal having an oxidation number of 4 or greater (e.g., MoO3, V2O5, WO3, KMnO4, Nb2O5, Sb2O5, As2O5, SiO2, MnO2, SnO2, ZnO2, MoO2, RuO2, TiO2, or any combination thereof).
[0030] For example, in one or more embodiments, the metal oxide may be a metal oxide having an oxidation number of 5 or higher. The metal oxide having an oxidation number of 5 or higher may include, for example, MoO3, V2O5, WO3, KMnO4, Nb2O5, Sb2O5, As2O5, or any combination thereof. The metal oxide having a high oxidation number of 5 or higher may effectively suppress or reduce the elution problem of internal lithium of the positive electrode active material within the positive electrode composition, and effectively prevent or reduce the denaturation of the binder and the subsequent gelation of the positive electrode composition.
[0031] In one or more embodiments, based on the total weight 100wt% of the positive electrode composition, the metal oxide may be included in an amount of about 0.01wt% to about 0.5wt% (e.g., about 0.01wt% to about 0.4wt%, about 0.01wt% to about 0.3wt%, about 0.01wt% to about 0.2wt%, about 0.01wt% to about 0.1wt%, about 0.01wt% to about 0.09wt%, about 0.02wt% to about 0.5wt%, about 0.03wt% to about 0.5wt%, about 0.04wt% to about 0.5wt%, or about 0.05wt% to about 0.5wt%). By including the metal oxide within the above content (e.g., amount) range, gelation and capacity degradation of the positive electrode composition may be effectively suppressed or reduced without reducing capacity or causing side effects.
[0032] Organic Acid
[0033] The organic acid is not particularly limited, but may include, for example, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, nonanoic acid, capric acid, caprylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, fluoroacetic acid, trifluoroacetic acid, chloroacetic acid, dichloroacetic acid, bromoacetic acid, iodoacetic acid, glycolic acid, methoxyacetic acid, cyanoacetic acid, 2-chlorobutyric acid, 3-chlorobutyric acid, 3-butenoic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, or any combination thereof.
[0034] In one or more embodiments, the organic acid may be included in an amount of about 0.01 wt% to about 1 wt% (e.g., about 0.01 wt% to about 0.9 wt%, about 0.01 wt% to about 0.7 wt%, about 0.01 wt% to about 0.5 wt%, about 0.01 wt% to about 0.3 wt%, about 0.01 wt% to about 0.1 wt%, about 0.05 wt% to about 1 wt%, or about 0.1 wt% to about 1 wt%) based on the total weight 100 wt% of the positive electrode composition. If the organic acid is included in the above content (e.g., amount) range (e.g., when the organic acid is included in the above content (e.g., amount) range), the processability can be improved by suppressing deformation / denaturation of the binder and preventing or reducing gelation of the positive electrode composition without adversely affecting the positive electrode composition.
[0035] The weight ratio of the metal oxide to the organic acid may be about 1: 1 to about 1: 10, for example, about 1: 2 to about 1: 10, about 1: 1 to about 1: 8, about 1: 1 to about 1: 6, about 1: 1 to about 1: 4, or about 1: 1 to about 1: 3. If the weight ratio of the metal oxide to the organic acid satisfies the above range (for example, when the weight ratio of the metal oxide to the organic acid satisfies the above range), the elution of lithium inside the positive electrode active material and the formation of lithium compounds on the surface of the positive electrode active material are effectively suppressed or reduced, thereby maximizing or increasing the effect of preventing or reducing the gelation of the positive electrode composition.
[0036] Positive electrode active material
[0037] The positive electrode active material is not particularly limited as long as it is a positive electrode active material used in a rechargeable lithium battery, and may include, for example, lithium nickel oxides, lithium cobalt oxides, lithium manganese oxides, lithium iron phosphate compounds, cobalt-free lithium nickel manganese oxides, over-lithiated layered oxides, or any combination thereof.
[0038] The positive electrode active material according to one or more embodiments may include a lithium nickel oxide, and the lithium nickel oxide has a nickel content (e.g., amount) of about 80 mol% or more or about 90 mol% or more, based on 100 mol% of the total molar number of metals other than lithium included in the lithium nickel oxide. High nickel layered positive electrode active materials have the advantages of achieving high capacity and high energy density. However, the higher the nickel content (e.g., amount), the easier it is for the lithium inside the positive electrode active material to be due to the Ni on the surface of the positive electrode active material. 3+ Reduction to Ni 2+ And eluted, and lithium compounds are formed on the surface, thereby increasing resistance. As a result, the binder is deformed and the positive electrode composition is gelled, reducing processability. On the contrary, if the metal oxide and organic acid according to one or more embodiments are applied while applying a high-nickel positive electrode active material (for example, when the metal oxide and organic acid according to one or more embodiments are applied while applying a high-nickel positive electrode active material), the elution of lithium inside the positive electrode active material is suppressed or reduced, the formation of additional lithium compounds is prevented or reduced, and the deformation of the binder is suppressed or reduced, thereby effectively preventing or reducing the gelation of the positive electrode composition. As a result, high capacity and high energy density can be achieved while preventing or reducing capacity degradation and improving processability.
[0039] In one or more embodiments, the positive electrode active material may include a compound represented by Chemical Formula 1, for example.
[0040] Chemical formula 1
[0041] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1
[0042] In Chemical Formula 1, 0.9≤a1≤1.8, 0.8≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, M 1 and M 2 may be independently selected from one or more elements selected from aluminum (Al), boron (B), barium (Ba), calcium (Ca), cerium (Ce), cobalt (Co), chromium (Cr), copper (Cu), iron (Fe), magnesium (Mg), manganese (Mn), molybdenum (Mo), niobium (Nb), silicon (Si), tin (Sn), strontium (Sr), titanium (Ti), vanadium (V), tungsten (W) and zirconium (Zr), and X may be one or more elements selected from fluorine (F), phosphorus (P) and sulfur (S).
[0043] In some embodiments, in Chemical Formula 1, 0.85 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.15, 0 ≤ z1 ≤ 0.15; 0.9 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.1, 0 ≤ z1 ≤ 0.1; or 0.91 ≤ x1 < 1, 0 < y1 ≤ 0.09, and 0 ≤ z1 ≤ 0.09.
[0044] In some embodiments, the positive electrode active material may include a lithium nickel cobalt composite oxide represented by Chemical Formula 2.
[0045] Chemical Formula 2
[0046] Li a2 Ni x2 Co y2 M 3 z2 O 2-b2 X b2
[0047] In Chemical Formula 2, 0.9 ≤ a2 ≤ 1.8, 0.8 ≤ x2 < 1, 0 < y2 ≤ 0.2, 0 ≤ z2 ≤ 0.2, 0.9 ≤ x2 + y2 + z2 ≤ 1.1, and 0 ≤ b2 ≤ 0.1, M 3 may be one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X may be one or more elements selected from F, P, and S.
[0048] In some embodiments, in Chemical Formula 2, 0.9 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.1, and 0.01 ≤ z2 ≤ 0.1.
[0049] In some embodiments, the positive electrode active material may include a lithium nickel composite oxide represented by Chemical Formula 3. The compound of Chemical Formula 3 may be referred to as lithium nickel-cobalt-aluminum oxide or lithium nickel-cobalt-manganese oxide.
[0050] Chemical Formula 3
[0051] Li a3 Ni x3 Co y3 M 4 z3 M 5 w3 O 2-b3 X b3
[0052] In Chemical Formula 3, 0.9≤a3≤1.8, 0.8≤x3≤0.98, 0.01≤y3≤0.19, 0.01≤z3≤0.19, 0≤w3≤0.19, 0.9≤x3+y3+z3+w3≤1.1, and 0≤b3≤0.1, M 4 It can be one or more elements selected from Al and Mn, M 5 It may be one or more elements selected from B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W and Zr, and X may be one or more elements selected from F, P and S.
[0053] In some embodiments, in Chemical Formula 3, 0.9≤x3≤0.98, 0.01≤y3≤0.09, 0.01≤z3≤0.09, and 0≤w3≤0.09.
[0054] The positive electrode active material may be in the form of particles, for example, it may be in the form of secondary particles in which a plurality of primary particles are aggregated (for example, a plurality of primary particles are aggregated in each of the secondary particles), or it may be in the form of a single particle (for example, each is a whole particle).
[0055] The average particle size (D 50 ) is not particularly limited, but may be, for example, about 1 μm to about 20 μm, about 3 μm to about 18 μm, or about 5 μm to about 15 μm. The average particle size refers to the diameter (D) of particles having a cumulative volume of 50% by volume in a particle size distribution obtained by randomly measuring the size (diameter or length of the major axis) of about 20 particles in a scanning electron microscope image for the positive electrode active material. 50 ).
[0056] Binder
[0057] The binder according to one or more embodiments may be a fluorine binder. Fluorine binders are advantageous for achieving high energy density by firmly adhering to the positive electrode active material. However, due to the residual lithium compound formed on the surface of the positive electrode active material, the fluorine binder is easily deformed, and the modified / deformed fluorine binder has the harmful effect of causing aggregation and gelation of the positive electrode composition. However, if the metal oxide and organic acid according to one or more embodiments are used together with the fluorine binder (for example, when the metal oxide and organic acid according to one or more embodiments are used together with the fluorine binder), the pH (pH level) is adjusted to suppress or reduce the deformation of the binder, and the formation of additional lithium compounds is suppressed or reduced, thereby additionally preventing or reducing the deformation of the binder, and effectively suppressing the gelation of the positive electrode composition.
[0058] The fluorine-based binder may include, for example, polyvinylidene fluoride (PVdF), polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP) copolymer, polyvinylidene fluoride-trichloroethylene (PVdF-TCE) copolymer, polytetrafluoroethylene (PTFE), polytrifluoroethylene (PTrFE), polychlorotrifluoroethylene (CTFE), polyhexafluoropropylene, hexafluoroisobutylene, or any combination thereof.
[0059] In one or more embodiments, based on the total weight 100wt% of the positive electrode composition, the binder may be included in an amount of about 0.1wt% to about 3wt% (e.g., about 0.1wt% to about 2wt% or about 0.5wt% to about 1.5wt%). If the binder content (e.g., amount) satisfies the above range (e.g., when the binder content (e.g., amount) satisfies the above range), the energy density may be increased and the durability may be improved by increasing the binding force of the positive electrode active material without adversely affecting the positive electrode.
[0060] Conductive Materials
[0061] The positive electrode composition according to one or more embodiments may further include a conductive material. The conductive material may include, for example: a carbon material such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber and / or carbon nanotube; a metal material containing copper, nickel, aluminum, silver, etc. in the form of a metal powder or metal fiber; a conductive polymer such as a polyphenylene derivative; or any mixture thereof.
[0062] In one or more embodiments, the conductive material may be included in an amount of about 0.1 wt% to about 2 wt% (e.g., about 0.1 wt% to about 1 wt% or about 0.3 wt% to about 0.8 wt%) based on the total weight 100 wt% of the positive electrode composition. If the content (e.g., amount) of the conductive material satisfies the above range (e.g., when the content (e.g., amount) of the conductive material satisfies the above range), the electronic conductivity may be increased without adversely affecting the positive electrode.
[0063] For example, in one or more embodiments, based on the total weight 100wt% of the positive electrode composition, the positive electrode active material may be included in an amount of about 93.5wt% to about 99.78wt%, the metal oxide may be included in an amount of about 0.01wt% to about 0.5wt%, the organic acid may be included in an amount of about 0.01wt% to about 1wt%, the binder may be included in an amount of about 0.1wt% to about 3wt%, and the conductive material may be included in an amount of about 0.1wt% to about 2wt%. In one or more embodiments, based on the total weight 100wt% of the positive electrode composition, the positive electrode active material may be included in an amount of about 93.5wt% to about 99.88wt%, the metal oxide may be included in an amount of about 0.01wt% to about 0.5wt%, the organic acid may be included in an amount of about 0.01wt% to about 1wt%, and the binder may be included in an amount of about 0.1wt% to about 3wt%.
[0064] Positive electrode
[0065] In one or more embodiments, a positive electrode for a rechargeable lithium battery may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, wherein the positive electrode active material layer may include a positive electrode active material, a binder, a metal oxide having an oxidation number of 4 or higher, and an organic acid. The positive electrode may be formed by the above-mentioned positive electrode composition.
[0066] The positive electrode current collector may be aluminum, stainless steel (SUS), or the like, but the embodiments of the present disclosure are not limited thereto.
[0067] Descriptions of the positive electrode active material, the binder, the metal oxide having an oxidation number of 4 or higher, and the organic acid may each independently be the same as described above, and thus are omitted for the sake of brevity.
[0068] The metal oxide may be included in an amount of about 0.01 wt % to about 0.5 wt % (e.g., about 0.01 wt % to about 0.4 wt %, about 0.01 wt % to about 0.3 wt %, about 0.01 wt % to about 0.2 wt %, about 0.01 wt % to about 0.1 wt %, about 0.01 wt % to about 0.09 wt %, about 0.02 wt % to about 0.5 wt %, about 0.03 wt % to about 0.5 wt %, about 0.04 wt % to about 0.5 wt %, or about 0.05 wt % to about 0.5 wt %) based on the total weight 100 wt % of the positive electrode active material layer.
[0069] The organic acid may be included in an amount of about 0.01 wt % to about 1 wt % (e.g., about 0.01 wt % to about 0.9 wt %, about 0.01 wt % to about 0.7 wt %, about 0.01 wt % to about 0.5 wt %, about 0.01 wt % to about 0.3 wt %, about 0.01 wt % to about 0.1 wt %, about 0.05 wt % to about 1 wt % or about 0.1 wt % to about 1 wt %) based on the total weight 100 wt % of the positive electrode active material layer.
[0070] The binder may be included in an amount of about 0.1 wt % to about 3 wt % (eg, about 0.1 wt % to about 2 wt % or about 0.5 wt % to about 1.5 wt %) based on 100 wt % of the total weight of the positive electrode active material layer.
[0071] In one or more embodiments, the positive electrode active material layer may further include a conductive material, and the conductive material may be included in an amount of about 0.1 wt % to about 2 wt % (e.g., about 0.1 wt % to about 1 wt % or about 0.3 wt % to about 0.8 wt %) based on the total weight of the positive electrode active material layer, 100 wt %.
[0072] Rechargeable lithium battery
[0073] According to one or more embodiments, a rechargeable lithium battery may include the above-described positive electrode, negative electrode, and electrolyte.
[0074] Rechargeable lithium batteries may be classified according to their shapes into cylindrical, prismatic, pouch and / or coin types, etc. Figures 1 to 4 2 are schematic diagrams showing a rechargeable lithium battery according to one or more embodiments. Figure 1 A cylindrical battery is shown, Figure 2 A prismatic cell is shown, Figure 3 and Figure 4 A pouch type or bag type battery is shown. Figures 1 to 4 , the rechargeable lithium battery 100 may include an electrode assembly 40 and a case, the electrode assembly 40 including a positive electrode 10 and a negative electrode 20 and a separator 30 disposed between the positive electrode 10 and the negative electrode 20, and the electrode assembly 40 is included in the case. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution. In some embodiments, as Figure 1 As shown in , the rechargeable lithium battery 100 may include a sealing member 60 that seals the housing 50. In some embodiments, as Figure 2 As shown in , the rechargeable lithium battery 100 may include a positive lead tab 11, a positive terminal 12, a negative lead tab 21, and a negative terminal 22. In some embodiments, as Figure 3 and Figure 4As shown in , the rechargeable lithium battery 100 may include electrode tabs 70 serving as an electrical path for inducing a current formed in the electrode assembly 40 to the outside, that is, a positive electrode tab 71 and a negative electrode tab 72 .
[0075] The rechargeable lithium battery according to one or more embodiments may be capable of being driven at a high voltage, or may be suitable for being driven at a high voltage. For example, the driving voltage of the rechargeable lithium battery may be about 4.3V to about 4.6V or about 4.40V to about 4.55V. By applying the positive electrode active material according to one or more embodiments, the rechargeable lithium battery can significantly reduce the amount of gas generated even when driven at a high voltage, and can achieve high capacity and long cycle life characteristics.
[0076] Negative electrode
[0077] The negative electrode may include a negative electrode current collector and a negative electrode active material layer on the negative electrode current collector, and the negative electrode active material layer may include a negative electrode active material, a binder, a conductive material, or any combination thereof.
[0078] Negative electrode active material
[0079] The negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / dedoping lithium, and / or a transition metal oxide.
[0080] The material that reversibly intercalates / deintercalates lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or any combination thereof. The crystalline carbon may be graphite, such as amorphous, flaky, plate-like, spherical or fibrous natural graphite or artificial graphite, and the amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbonization product, and / or burnt coke, etc.
[0081] The lithium metal alloy may include an alloy of lithium and at least one metal selected from sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), silicon (Si), antimony (Sb), lead (Pb), indium (In), zinc (Zn), barium (Ba), radium (Ra), germanium (Ge), aluminum (Al) and tin (Sn).
[0082] The material capable of being doped / undoped with lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may include silicon, a silicon-carbon composite, SiO x(0 < x ≤ 2), Si-Q alloy (where Q is selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements (excluding Si), Group 15 elements, Group 16 elements, transition metals, rare earth elements, and any combination thereof, for example, magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), rutherfordium (Rf), vanadium (V), niobium (Nb), tantalum (Ta), dubnium (Db), chromium (Cr), molybdenum (Mo), tungsten (W), seaborgium (Sg), technetium (Tc), rhenium (Re), (Bh), iron (Fe), lead (Pb), ruthenium (Ru), osmium (Os), hassium (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), aluminum (Al), gallium (Ga), tin (Sn), indium (In), thallium (Tl), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), and any combination thereof) or any combination of them. The Sn-based negative electrode active material may include Sn, SnO x (0 < x ≤ 2), Sn alloy, or any combination thereof.
[0083] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle size (D 50 ) may be, for example, from about 0.5 μm to about 20 μm. According to one or more embodiments, the silicon-carbon composite may be in the form of silicon particles and an amorphous carbon coating on the surface of the silicon particles. For example, in some embodiments, the silicon-carbon composite may include secondary particles (cores) and an amorphous carbon coating layer (shells) on the surface of the secondary particles, and primary silicon particles are assembled (e.g., aggregated) in the secondary particles (cores). In some embodiments, amorphous carbon may also be between the primary silicon particles, for example, the primary silicon particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.
[0084] In one or more embodiments, the silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core containing crystalline carbon and silicon particles and an amorphous carbon coating layer on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or any combination thereof. The amorphous carbon may be soft carbon or hard carbon, mesophase pitch carbonized product, and / or calcined coke, etc.
[0085] If the silicon-carbon composite includes silicon and amorphous carbon (e.g., when the silicon-carbon composite includes silicon and amorphous carbon), then based on 100 wt% of the total weight of the silicon-carbon composite, the content (e.g., amount) of silicon can be about 10 wt% to about 50 wt%, and the content (e.g., amount) of amorphous carbon can be about 50 wt% to about 90 wt%. In some embodiments, if the silicon-carbon composite includes silicon, amorphous carbon, and crystalline carbon (e.g., when the silicon-carbon composite includes silicon, amorphous carbon, and crystalline carbon), then based on 100 wt% of the total weight of the silicon-carbon composite, the content (e.g., amount) of silicon can be about 10 wt% to about 50 wt%, the content (e.g., amount) of crystalline carbon can be about 10 wt% to about 70 wt%, and the content (e.g., amount) of amorphous carbon can be about 20 wt% to about 40 wt%.
[0086] In one or more embodiments, the thickness of the amorphous carbon coating layer can be about 5 nm to about 100 nm. The average particle size (D 50 ) of the silicon particles (primary particles) can be about 10 nm to about 1 μm or about 10 nm to about 200 nm. The silicon particles can exist alone as silicon, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon can be represented by SiO x (0 < x < 2). In this regard, the atomic content (e.g., amount) ratio of Si:O representing the degree of oxidation can be about 99:1 to about 33:67. As used herein, when no other definition is provided, the average particle size (D 50 ) represents the particles in the particle distribution where the cumulative volume is about 50 volume%.
[0087] Si-based negative electrode active materials or Sn-based negative electrode active materials can be used in combination with carbon-based negative electrode active materials. If Si-based negative electrode active materials or Sn-based negative electrode active materials are mixed and used with carbon-based negative electrode active materials (e.g., when Si-based negative electrode active materials or Sn-based negative electrode active materials are mixed and used with carbon-based negative electrode active materials), then the mixing ratio can be a weight ratio of about 1:99 to about 90:10.
[0088] Binder
[0089] The binder is used to appropriately and / or well attach the negative electrode active material particles to each other and is also used to appropriately and / or well attach the negative electrode active material to the negative electrode current collector. The binder can include a non-aqueous binder, an aqueous binder (e.g., a water-soluble binder), a dry binder, or any combination thereof.
[0090] The non-aqueous binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or any combination thereof.
[0091] The aqueous binder can be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and any combination thereof.
[0092] If an aqueous binder is used as a negative electrode binder (e.g., when an aqueous binder is used as a negative electrode binder), a cellulose compound capable of imparting viscosity may also be included. The cellulose compound may include at least one of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and alkali metal salts thereof. The alkali metal may include Na, K, or Li.
[0093] The dry binder may be a polymer material that can be fibrous, and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or any combination thereof.
[0094] Conductive Materials
[0095] Conductive materials can be used to impart conductivity to electrodes, and any material that does not cause chemical changes and conducts electrons can be used in batteries. Non-limiting examples thereof may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and / or carbon nanotubes; metal-based materials including copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fibers; conductive polymers such as polyphenylene derivatives; or any mixture thereof.
[0096] In one or more embodiments, the content (e.g., amount) of the negative electrode active material may be about 95 wt% to about 99.5 wt% based on the total weight 100 wt% of the negative electrode active material layer, and the content (e.g., amount) of the binder may be about 0.5 wt% to about 5 wt% based on the total weight 100 wt% of the negative electrode active material layer. For example, in some embodiments, the negative electrode active material layer may include about 90 wt% to about 99 wt% of the negative electrode active material, about 0.5 wt% to about 5 wt% of the binder, and about 0.5 wt% to about 5 wt% of the conductive material.
[0097] Negative electrode current collector
[0098] The negative electrode current collector may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or alloys thereof, and may be in the form of foil, sheet or foam. The thickness of the negative electrode current collector may be, for example, about 1 μm to about 20 μm, about 5 μm to about 15 μm or about 7 μm to about 10 μm.
[0099] Electrolytes
[0100] In one or more embodiments, the electrolyte for a rechargeable lithium battery may be an electrolyte that may include a non-aqueous organic solvent and a lithium salt.
[0101] The non-aqueous organic solvent is used as a medium for transporting ions participating in the electrochemical reaction of the battery. The non-aqueous organic solvent may be a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent or an alcohol solvent, an aprotic solvent, or any combination thereof.
[0102] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC) and / or butylene carbonate (BC), etc. Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, decanoic acid lactone, mevalonolactone, valerolactone and / or caprolactone, etc.
[0103] Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran and / or tetrahydrofuran, etc. In some embodiments, ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol and / or isopropanol, etc., and aprotic solvents may include: nitrile, such as R-CN (wherein R is a C2 to C20 straight chain, branched or cyclic hydrocarbon group, and may include a double bond, an aromatic ring or an ether bond), etc.; amides, such as dimethylformamide; dioxolanes, such as 1,3-dioxolanes and / or 1,4-dioxolanes, etc.; and / or sulfolane, etc.
[0104] The non-aqueous organic solvent can be used alone or as a mixture of two or more types (kinds). If two or more types (kinds) are used as a mixture (for example, when two or more types (kinds) are used as a mixture), the mixing ratio can be appropriately adjusted according to the desired or suitable battery performance, which is widely applicable to those skilled in the art.
[0105] If a carbonate-based solvent is used (eg, when a carbonate-based solvent is used), a cyclic carbonate and a chain carbonate may be mixed and used, and the cyclic carbonate and the chain carbonate may be mixed in a volume ratio of about 1:1 to about 1:9.
[0106] In one or more embodiments, the non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent. For example, in some embodiments, a carbonate-based solvent and an aromatic hydrocarbon organic solvent may be mixed and utilized in a volume ratio of about 1:1 to about 30:1.
[0107] In one or more embodiments, the electrolyte may further include ethylene ethyl carbonate, vinylene carbonate, or ethylene carbonate-based compounds to improve battery cycle life.
[0108] Non-limiting examples of the ethylene carbonate-based compound may include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.
[0109] The lithium salt dissolved in the non-aqueous organic solvent supplies lithium ions in the rechargeable lithium battery, realizes the basic operation of the rechargeable lithium battery, and improves the transmission of lithium ions between the positive electrode and the negative electrode. Non-limiting examples of lithium salts may include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (x and y are both integers of 1 to 20), at least one of lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalato)borate (LiDFOB) and lithium bis(oxalato)borate (LiBOB).
[0110] The concentration of the lithium salt may be in the range of about 0.1 M to about 2.0 M. If the concentration of the lithium salt is within the above range (e.g., when the concentration of the lithium salt is within the above range), the electrolyte has suitable or appropriate ion conductivity and viscosity, so excellent or appropriate performance can be achieved, and lithium ions can be efficiently moved.
[0111] Diaphragm
[0112] Depending on the type or kind of the rechargeable lithium battery, the separator may be present between the positive electrode and the negative electrode. The separator may include polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof or a mixed multilayer film (such as a polyethylene / polypropylene double-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and / or a polypropylene / polyethylene / polypropylene three-layer separator, etc.).
[0113] The separator may include a porous substrate and a coating layer including an organic material, an inorganic material, or any combination thereof on one or both (eg, simultaneously) surfaces of the porous substrate.
[0114] The porous substrate can be a polymer film formed by any one selected from the group consisting of polymers polyolefins (such as polyethylene and / or polypropylene), polyesters (such as polyethylene terephthalate and / or polybutylene terephthalate), polyacetals, polyamides, polyimides, polycarbonates, polyether ketones, polyarylether ketones, polyetherimides, polyamideimides, polybenzimidazoles, polyethersulfones, polyphenylene oxides, cyclic olefin copolymers, polyphenylene sulfide, polyethylene naphthalate, fiberglass, Teflon and polytetrafluoroethylene, or any copolymers or mixtures of two or more thereof.
[0115] The porous substrate may have a thickness of about 1 μm to about 40 μm (eg, about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm).
[0116] The organic material may include a (meth)acrylic copolymer including a first structural unit derived from (meth)acrylamide and a second structural unit, the second structural unit including at least one of a structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.
[0117] The inorganic material may include inorganic particles selected from Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, SrTiO3, BaTiO3, Mg(OH)2, boehmite, and any combination thereof, but the embodiments of the present disclosure are not limited thereto. The average particle size (D 50 ) can be about 1 nm to about 2000 nm, for example, about 100 nm to about 1000 nm or about 100 nm to about 700 nm.
[0118] An organic material and an inorganic material may be mixed in one coating layer, or a coating layer including an organic material and a coating layer including an inorganic material may be stacked.
[0119] The coating layer may have a thickness of about 0.5 μm to about 20 μm, for example, about 1 μm to about 10 μm or about 1 μm to about 5 μm.
[0120] Examples and comparative examples of the present disclosure are described in more detail herein.However, the following examples are merely examples of the present disclosure, and the present disclosure is not limited to the following examples.
[0121] Example 1
[0122] 1. Manufacturing of positive electrode
[0123] By adding 98.15 wt% of the positive electrode active material (LiNi 0.915 Co 0.07 Al 0.015 O2), 0.5wt% of carbon nanotube conductive material, 1.2wt% of polyvinylidene fluoride binder, 0.1wt% of oxalic acid and 0.05wt% of WO3 are mixed in N-methyl-2-pyrrolidone (NMP) solvent to prepare a positive electrode composition. The solid content (e.g., amount) of the positive electrode composition is about 75.5%. The prepared positive electrode composition is coated on an aluminum foil current collector, and then dried and pressed to make a positive electrode.
[0124] 2. Manufacturing of rechargeable lithium battery cells
[0125] 97.5 wt% of graphite negative electrode active material, 1.5 wt% of carboxymethyl cellulose and 1 wt% of styrene butadiene rubber in water solvent were used to prepare negative electrode active material layer slurry. The negative electrode active material layer slurry was coated on a copper foil current collector, then dried and compressed to make a negative electrode.
[0126] A rechargeable lithium battery cell was manufactured in a conventional method using a polytetrafluoroethylene separator and using an electrolyte prepared by dissolving 1M LiPF6 in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 3:7.
[0127] Example 2
[0128] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by using MoO 3 instead of WO 3 .
[0129] Example 3
[0130] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by using V2O5 instead of WO3.
[0131] Example 4
[0132] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by using KMnO 4 instead of WO 3 .
[0133] Example 5
[0134] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by using SiO 2 instead of WO 3 .
[0135] Comparative Example 1
[0136] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by using 98.2 wt % of a positive electrode active material, 0.5 wt % of a conductive material, 1.2 wt % of a binder and 0.1 wt % of oxalic acid without adding WO 3 .
[0137] Comparative Example 2
[0138] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by mixing 98.15 wt % of a positive electrode active material, 0.5 wt % of a conductive material, 1.2 wt % of a binder and 0.15 wt % of oxalic acid without adding WO 3 .
[0139] Comparison Example 3
[0140] A positive electrode and a rechargeable lithium battery cell were manufactured in substantially the same manner as in Example 1, except that the positive electrode composition was prepared by mixing 98.25 wt % of a positive electrode active material, 0.5 wt % of a conductive material, 1.2 wt % of a binder and 0.05 wt % of WO 3 without adding oxalic acid.
[0141] For ease of understanding, designs of positive electrode compositions according to Examples and Comparative Examples are briefly shown in Table 1.
[0142] (Table 1)
[0143]
[0144] Evaluation Example 1: Evaluation of Viscosity Change of Positive Electrode Composition During Atmospheric Storage
[0145] When stored in air for 3 days, the viscosity changes of the positive electrode compositions according to Examples 1 to 5 and Comparative Examples 1 to 3 were each measured, and the results are shown in Tables 2, Figure 5 and Figure 6The viscosity at 25° C. was measured by using a viscometer (Anton Paar, MCR 302e). In Table 2, the unit of viscosity is mPa·s.
[0146] (Table 2)
[0147]
[0148] Refer to Table 2 and Figure 5 and Figure 6 , because each of the positive electrode compositions begins to gel due to binder denaturation while being placed, each of Comparative Examples 1 and Comparative Example 2 to which an organic acid is added alone without adding a metal oxide, and Comparative Example 3 to which a metal oxide is added alone without adding an organic acid, exhibits greatly increased viscosity. Comparative Example 1 exhibits a sharp increase in viscosity after 2 days, and is therefore unmeasurable on the 3rd day, and Comparative Example 2 exhibits a sharp increase in viscosity after 3 days. In Comparative Example 3, shear thickening occurs after 2 days. On the other hand, Examples 1 to 5 to which metal oxides and organic acids are added simultaneously (e.g., concurrently) do not exhibit an increase in viscosity even after being placed for 3 days, thereby effectively suppressing or reducing the gelation of the slurry. Specifically, Examples 1 to 4 to which a high-valence metal oxide of 5 or more is added exhibit a much greater slurry gelation inhibition effect.
[0149] Evaluation Example 2: Evaluation of Capacity Degradation
[0150] A battery cell was manufactured immediately after each of the positive electrode compositions of Example 1 and Comparative Example 2 was prepared, a battery cell was manufactured after the positive electrode composition of Comparative Example 2 was left for 3 days, and a battery cell was manufactured after the positive electrode composition of Example 1 was left for 6 days, and then the capacities were respectively checked, and the resulting capacity according to the voltage change curve is shown in FIG. Figure 7 middle.
[0151] Reference Figure 7 When the positive electrode composition was left for 3 days, the discharge capacity of Comparative Example 2 decreased by about 4.7% (from 187.4 mAh / g to 178.6 mAh / g) compared to immediately after the positive electrode composition was prepared. In contrast, when the positive electrode composition was left for 6 days, the discharge capacity of Example 1 decreased by about 0.6% (from 191.6 mAh / g to 190.5 mAh / g) compared to immediately after the positive electrode composition was prepared.
[0152] Evaluation Example 3: XRD peak comparison and pH change comparison
[0153] Each of the positive electrode compositions according to Example 1 and Comparative Example 1 was compared with respect to the change of the (003) phase peak by X-ray diffraction analysis immediately after preparing the compositions and after leaving them for 3 days, and the results are shown in Figure 8 In. Reference Figure 8 , unlike Example 1, Comparative Example 1 showed that the (003) phase peak shifted to the left after it was left for 3 days, which confirmed the lithium elution inside the positive electrode active material, but when the organic acid was applied alone, there was no internal lithium elution inhibition effect from the positive electrode active material.
[0154] In addition, the pH change according to the addition of an organic acid or a metal oxide to the positive electrode active material during the manufacturing process of the positive electrode composition was measured, and the results are shown in Fig. 9 middle. Fig. 9 The pH measured when the positive electrode active material was added alone and then when 0.1 wt % of oxalic acid (OA) was added alone in Comparative Example 1 is shown. Fig. 9 The pH measured when 0.05 wt% of MoO3 was added alone without adding an organic acid and the pH measured when 0.1 wt% of oxalic acid and 0.05 wt% of MoO3 were added as in Example 2 are shown. Fig. 9 , when the metal oxide is added alone, there is an insignificant pH lowering effect, which confirms that the metal oxide alone has no effect of removing the residual lithium compound on the surface of the positive electrode active material. Therefore, in order to improve processability and reliability, an organic acid capable of removing the residual lithium compound on the surface of the positive electrode active material to lower the pH and a metal oxide capable of preventing or reducing the elution of internal lithium from the positive electrode active material should be used simultaneously (e.g., concurrently).
[0155] As used herein, the terms "substantially", "about", and similar terms are used as approximate terms rather than as terms of degree, and are intended to account for the inherent deviations in measured or calculated values that one of ordinary skill in the art will recognize. Taking into account the measurement in question and the errors associated with the measurement of a particular quantity (i.e., the limitations of the measurement system), as used herein, "about" or "approximately" also includes the stated value and means within an acceptable deviation range for a particular value as determined by one of ordinary skill in the art. For example, "about" can mean within one or more standard deviations, or within ±30%, ±20%, ±10%, ±5% of the stated value.
[0156] Any numerical range described herein is intended to include all subranges of the same numerical precision contained within the described range. For example, the range of "1.0 to 10.0" is intended to include all subranges between the described minimum value 1.0 and the described maximum value 10.0 (and including the described minimum value 1.0 and the described maximum value 10.0), that is, having a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as 2.4 to 7.6. Any maximum numerical limit described herein is intended to include all lower numerical limits contained therein, and any minimum numerical limit described in this specification is intended to include all higher numerical limits contained therein. Therefore, the applicant reserves the right to amend this specification and claims to explicitly describe any subranges contained within the range explicitly described herein.
[0157] The battery management system (BMS) device and / or any other related device or component according to the embodiments of the present invention described herein can be implemented using any suitable hardware, firmware (e.g., a dedicated integrated circuit), software, or a combination of software, firmware, and hardware. For example, the various components of the device can be formed on an integrated circuit (IC) chip or on a separate IC chip. In addition, the various components of the device can be implemented on a flexible printed circuit film, a tape carrier package (TCP), a printed circuit board (PCB), or formed on a substrate. In addition, the various components of the device can be processes or threads that run on one or more processors in one or more computing devices, execute computer program instructions, and interact with other system components to perform the various functions described herein. The computer program instructions are stored in a memory, which can be implemented in a computing device using a standard memory device (such as a random access memory (RAM) as an example). The computer program instructions can also be stored in other non-temporary computer-readable media (such as a CD-ROM, a flash drive, etc. as an example). In addition, it should be recognized by those skilled in the art that the functions of various computing devices can be combined or integrated into a single computing device without departing from the scope of the present disclosure, or the functions of a particular computing device can be distributed across one or more other computing devices.
[0158] Although the present disclosure has been described in conjunction with what are presently considered to be practical example embodiments, it will be understood that the present disclosure is not limited to the disclosed embodiments. Instead, it is intended to cover one or more suitable modifications and equivalent arrangements included within the spirit and scope of the appended claims and their equivalents.
[0159] Reference numerals
[0160] 100: Rechargeable lithium battery 10: Positive electrode
[0161] 11: Positive lead lug 12: Positive terminal
[0162] 20: Negative electrode 21: Negative lead lug
[0163] 22: Negative terminal 30: Separator
[0164] 40: electrode assembly 50: shell
[0165] 60: Sealing member 70: Electrode terminal piece
[0166] 71: Positive electrode terminal tab 72: Negative electrode terminal tab
Claims
1. A positive electrode composition for a rechargeable lithium battery, the positive electrode composition comprising: a positive electrode active material; a binder; a metal oxide having an oxidation number of 4 or higher; and an organic acid.
2. The positive electrode composition according to claim 1, wherein, The metal oxide includes MoO 3 、V 2 O 5 , WO 3 、KMnO 4 , Nb 2 O 5 , Sb 2 O 5 、As 2 O 5 、SiO 2 、MnO 2 SnO 2 、ZnO 2 、MoO 2 、RuO 2 、TiO 2 or any combination thereof.
3. The positive electrode composition according to claim 1, wherein, the metal oxide is a metal oxide having an oxidation number of 5 or higher.
4. The positive electrode composition according to claim 1, wherein, based on 100 wt% of the total weight of the positive electrode composition, the amount of the metal oxide is 0.01 wt% to 0.5 wt%.
5. The positive electrode composition according to claim 1, wherein, the organic acid includes formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, pelargonic acid, capric acid, octanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, fluoroacetic acid, trifluoroacetic acid, chloroacetic acid, dichloroacetic acid, bromoacetic acid, iodoacetic acid, glycolic acid, methoxyacetic acid, cyanoacetic acid, 2-chlorobutyric acid, 3-chlorobutyric acid, 3-butenoic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid or any combination thereof.
6. The positive electrode composition according to claim 1, wherein, based on 100 wt% of the total weight of the positive electrode composition, the amount of the organic acid is 0.01 wt% to 1 wt%.
7. The positive electrode composition according to claim 1, wherein, the weight ratio of the metal oxide to the organic acid is 1:1 to 1:
10.
8. The positive electrode composition according to claim 1, wherein, the positive electrode active material includes lithium nickel-based oxides, lithium cobalt-based oxides, lithium manganese-based oxides, lithium iron phosphate compounds, cobalt-free lithium nickel manganese oxides, over-lithiated layered oxides or any combination thereof.
9. The positive electrode composition according to claim 1, wherein, based on 100 mol% of the total moles of metals other than lithium in the lithium nickel-based oxide, the positive electrode active material includes a lithium nickel-based oxide having a nickel amount of 80 mol% or greater.
10. The positive electrode composition according to claim 1, wherein, the positive electrode active material includes a compound represented by Chemical Formula 1: Chemical Formula 1 Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 Wherein, in Chemical Formula 1, 0.9≤a1≤1.8, 0.8≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, M 1 and M 2 are independently one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W and Zr, and X is one or more elements selected from F, P and S.
11. The positive electrode composition according to claim 10, wherein, 0.91 ≤ x1 < 1, 0 < y1 ≤ 0.09, and 0 ≤ z1 ≤ 0.
09.
12. The positive electrode composition according to claim 1, wherein, the binder includes a fluorine-based binder.
13. The positive electrode composition according to claim 1, wherein, based on 100 wt% of the total weight of the positive electrode composition, the amount of the positive electrode active material is 93.5 wt% to 99.88 wt%, the amount of the metal oxide is 0.01 wt% to 0.5 wt%, the amount of the organic acid is 0.01 wt% to 1 wt%, and the amount of the binder is 0.1 wt% to 3 wt%.
14. A positive electrode for a rechargeable lithium battery, the positive electrode comprising: a positive electrode current collector; and A positive electrode active material layer is on the positive electrode current collector and includes the positive electrode composition according to any one of claims 1 to 13.
15. A rechargeable lithium battery, the rechargeable lithium battery include: The positive electrode according to claim 14; Negative electrode; as well as Electrolytes.