High-efficiency sodium ion battery hard carbon negative electrode and preparation method and application thereof
By using phosphorus bromine doped multi-walled carbon nanotubes as conductive agents in sodium ion batteries, the conductivity of the hard carbon negative electrode is improved, and the problem of low charging and discharge efficiency of the negative electrode material of sodium ion batteries is solved, and the discharge specific capacity of the battery is significantly improved and cycle efficiency.
Patent Information
- Application Number
- CN202411230533.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sodium ion battery anode materials have poor performance in charging and discharging efficiency, especially in terms of charging and discharging efficiency.
Using phosphorus bromine doped multi-wall carbon nanotubes as conductive agents, the hard carbon negative electrode of high-efficiency sodium ion battery is prepared by mixing it uniformly with hard carbon negative electrode materials and binder, which improves the conductivity and reduces internal resistance, thereby improving battery charging. Discharge efficiency.
The discharge specific capacity and battery circulation efficiency of sodium ion batteries have been effectively improved. The discharge specific capacity of 0.1C has been increased by up to 19%, and the specific capacity retention rate has been increased by up to 5.38% after 100 weeks, significantly improving the charging and discharging efficiency of the battery.
Smart Images

Figure BDA0005025981530000091
Abstract
Description
Technical Field
[0001] The present invention relates to the field of negative electrode materials for sodium ion batteries, and in particular to a high-efficiency hard carbon negative electrode for sodium ion batteries and a preparation method and application thereof. Background Art
[0002] In recent years, with the continuous improvement of environmental awareness and the increasingly serious energy crisis, the development of new energy vehicles and renewable energy has received more and more attention. Among them, sodium batteries, as a new type of energy storage technology, have the advantages of high energy storage density, good safety, and long service life. They are widely used in new energy vehicles, smart grids, energy storage systems and other fields. As one of the core components of sodium-ion batteries, the negative electrode has an important influence on the battery's energy density, rate performance, cycle performance, and first coulombic efficiency.
[0003] The patent application with publication number CN112086640A discloses a lithium / sodium ion battery electrode material and a preparation method thereof. The electrode material provided by the material is a nanosheet structure having an outer layer and a porous structure coated in the outer layer; the outer layer is a carbon layer, and the surface of the carbon layer has a concave-convex structure; the porous structure is a sulfide. The lithium / sodium ion battery electrode material provided by the invention has a concave-convex structure distributed on the surface of the material, which is conducive to the shuttling of ions and electrons, full contact with the electrolyte, and improved conductivity. The lithium / sodium ion battery electrode material provided by the invention has an outer layer of a carbon layer, and the carbon layer can effectively alleviate the problem of volume expansion of the electrode material during charging and discharging, and has better stability. In addition, it also has excellent performance and can be used as an electrode material in the fields of lithium ion batteries and sodium ion batteries.
[0004] The patent application with publication number CN117049505A discloses a method for preparing a hard carbon negative electrode material, a hard carbon negative electrode material, and a sodium ion battery, including: subjecting a biomass material and deionized water to a hydrothermal reaction at 180-200°C for 12 to 24 hours, washing and drying to obtain a pre-carbonized intermediate; subjecting the pre-carbonized intermediate to sintering and carbonization treatment and then to an alkali treatment for 12 to 36 hours, washing and drying to obtain a hard carbon negative electrode material. This application forms a porous spherical hard carbon negative electrode material with uniformly dispersed pores by subjecting the biomass material to specific hydrothermal treatment conditions, and then to high-temperature carbonization and alkali treatment.
[0005] The patent application with publication number CN116190638A discloses a hard carbon negative electrode material and a preparation method thereof, a mixed negative electrode material, and a secondary battery, including: a hard carbon precursor is passivated to obtain a hard carbon negative electrode material; wherein the hard carbon precursor includes at least one of a pre-lithiation hard carbon precursor and a pre-sodium hard carbon precursor; the passivation treatment includes: under a protective atmosphere, the sodium and / or lithium in the hard carbon precursor reacts with a passivating substance to form a passivation layer to reduce the activity of sodium and / or lithium.
[0006] In sodium-ion batteries, the negative electrode material has a crucial impact on the overall performance of the battery, especially the charge and discharge efficiency of the battery. However, the negative electrode materials in the above-mentioned public information and prior art perform poorly in practical applications, especially in terms of charge and discharge efficiency. Summary of the invention
[0007] Based on the deficiencies in the prior art, the main purpose of the present invention is to provide a high-efficiency sodium ion battery hard carbon negative electrode and its preparation method and application. By modifying the conductive agent, the conductive performance of the hard carbon negative electrode can be effectively improved, the internal resistance can be reduced, and the charge and discharge efficiency of the battery can be improved.
[0008] The specific technical solutions of the present invention are as follows:
[0009] The present invention provides a method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery, comprising the following steps:
[0010] The hard carbon negative electrode material, the conductive agent and the binder are evenly ground, water is added, and the electrode slurry is obtained after mixing, and the electrode slurry is evenly coated on the metal foil, and the hard carbon negative electrode is prepared after drying in a vacuum oven;
[0011] The conductive agent is a phosphorus-bromine doped multi-walled carbon nanotube, and the preparation method includes:
[0012] Under alkaline conditions, the aminated multi-walled carbon nanotubes undergo amino-alkenyl addition reactions with allyl diethyl phosphate and 1-allyl-3-methylimidazolium bromide to obtain the phosphorus-bromine doped multi-walled carbon nanotubes.
[0013] Specifically, the preparation method of the phosphorus-bromine doped multi-walled carbon nanotubes is:
[0014] According to weight, 100-200 parts of amino multi-walled carbon nanotubes, 10-20 parts of allyl diethyl phosphate, 0.005-0.05 parts of 1-allyl-3-methylimidazolium bromide, 3-6 parts of sodium tert-butoxide and 1000-1400 parts of anhydrous ethanol are mixed, stirred and reacted at 60-70° C. for 30-70 minutes, and the anhydrous ethanol is removed to obtain the phosphorus-bromine doped multi-walled carbon nanotubes.
[0015] The hard carbon negative electrode prepared by the present invention effectively improves the discharge specific capacity and battery cycle efficiency of the sodium ion battery, especially the discharge specific capacity at 0.1C is increased by up to 19%, and the specific capacity retention rate after 100 weeks is increased by up to 5.38%, thereby improving the battery charge and discharge efficiency.
[0016] In some technical solutions of the present invention, the preparation method of the hard carbon negative electrode material may be selected from the following methods:
[0017] S1: crushing the carbon-based material into powder, washing it with a mixed solution of hydrochloric acid solution and anhydrous ethanol, then washing it with water until it is neutral, and drying it to obtain a precursor material;
[0018] S2: placing the precursor material into a tubular furnace, heating it to 1250-1650°C at a heating rate of 1-5°C / min under the protection of an inert gas, carbonizing it at high temperature for 1-3h, and then slowly cooling it to room temperature at a cooling rate of 3-5°C / min after carbonization to obtain the hard carbon negative electrode material.
[0019] Preferably, in step S1, the carbon-based material is at least one of lignite, anthracite, and sub-bituminous coal.
[0020] The carbon-based material can be crushed by a jaw crusher and then crushed again by a jet mill, which can make the carbon-based material and the acid fully contact and better implement pre-treatment.
[0021] Furthermore, in step S1, the concentration of the hydrochloric acid solution is 0.8-1.6 M, and the mass ratio of the hydrochloric acid solution to anhydrous ethanol is 1:0.8-1.2.
[0022] Furthermore, in step S1, the mass ratio of the powder to the mixed solution of hydrochloric acid and anhydrous ethanol is 1:1.6-3.2.
[0023] Optionally, in step S2, the inert gas is at least one of nitrogen, argon and helium, and the gas flow rate of the inert gas is 15-45 cc / min.
[0024] In the method for preparing a high-efficiency sodium ion battery hard carbon negative electrode of the present invention, the binder can be selected from at least one of sodium polyacrylate, sodium carboxymethyl cellulose, and polyvinylidene fluoride.
[0025] The present invention also provides a high-efficiency sodium ion battery hard carbon negative electrode prepared by the preparation method.
[0026] The present invention also provides a sodium ion battery, which comprises the high-efficiency sodium ion battery hard carbon negative electrode.
[0027] Beneficial effects of the present invention:
[0028] 1. In the preparation method of the present invention, the aminated multi-walled carbon nanotubes undergo an amino-alkenyl addition reaction with diethyl allyl phosphate and an amino-alkenyl addition reaction with 1-allyl-3-methylimidazolium bromide to obtain multi-walled carbon nanotubes containing diethyl phosphate and imidazole bromide. The multi-walled carbon nanotubes are used as conductive agents and can be used as channels for electron transmission, thereby effectively improving the conductive properties of the hard carbon negative electrode, thereby improving the charge and discharge efficiency of the battery.
[0029] 2. The conductive agent used in the present invention can form a stable network structure in the hard carbon negative electrode, effectively preventing the volume expansion and contraction of the hard carbon during the charge and discharge process, thereby improving the structural stability of the hard carbon negative electrode.
[0030] 3. The additives such as diethyl phosphate and imidazole bromide in the present invention are helpful to improve the surface properties of hard carbon and increase the diffusion rate of sodium ions in hard carbon. DETAILED DESCRIPTION
[0031] Example 1
[0032] The preparation method of the hard carbon negative electrode material used in the present invention is as follows:
[0033] S1: Weigh 10g of blue carbon and crush it with a jaw crusher, and then crush it again with a jet mill;
[0034] S2: The powder after the pulverization treatment is washed with a mixed solution of 0.8M dilute hydrochloric acid solution and anhydrous ethanol for 6 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0035] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:0.8, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:1.6;
[0036] S3: Place the precursor material into a tubular furnace, introduce high-purity nitrogen at a gas flow rate of 15cc / min, heat up to 1250℃ at a heating rate of 5℃ / min, and carbonize at high temperature for 1h. After carbonization, slowly cool down to room temperature at a cooling rate of 5℃ / min to obtain a hard carbon negative electrode material.
[0037] The conductive agent used in the present invention is phosphorus-bromine doped multi-walled carbon nanotubes, and the preparation method thereof is as follows:
[0038] 100 g of amino-modified multi-walled carbon nanotubes (CNT903: NH 2 : 0.45wt%; CAS number: 308068-56-6), 10g of diethyl allyl phosphate, 0.01g of 1-allyl-3-methylimidazolium bromide, 3g of sodium tert-butoxide and 1000g of anhydrous ethanol were mixed, stirred and reacted at 60°C for 30 minutes, and the anhydrous ethanol was distilled off to obtain phosphorus-bromine-doped multi-walled carbon nanotubes.
[0039] The method for preparing a high-efficiency sodium ion battery hard carbon negative electrode of the present invention comprises the following steps:
[0040] Weigh 6g of hard carbon negative electrode material, 0.6g of conductive agent, and 0.8g of sodium polyacrylate and grind them evenly. Add 8g of deionized water and stir magnetically for 3h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 150μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard was prepared.
[0041] Example 2
[0042] The preparation method of the hard carbon negative electrode material used in the present invention is as follows:
[0043] S1: Weigh 13g of blue carbon and crush it with a jaw crusher, and then crush it again with a jet mill;
[0044] S2: The powder after the pulverization treatment is washed with a mixed solution of 1.2M dilute hydrochloric acid solution and anhydrous ethanol for 8 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0045] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:1, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:2.2;
[0046] S3: Place the precursor material into a tubular furnace, introduce high-purity nitrogen at a gas flow rate of 25cc / min, heat up to 1350℃ at a heating rate of 3℃ / min, and carbonize at high temperature for 2h. After carbonization, slowly cool to room temperature at a cooling rate of 4℃ / min to obtain a hard carbon negative electrode material.
[0047] The conductive agent used in the present invention is phosphorus-bromine doped multi-walled carbon nanotubes, and the preparation method thereof is as follows:
[0048] 135 g of amino-modified multi-walled carbon nanotubes (Turing brand amino-modified multi-walled carbon nanotubes, CAS number: 308068-56-6), 13 g of diethyl allyl phosphate, 0.02 g of 1-allyl-3-methylimidazolium bromide, 4 g of sodium tert-butoxide and 1150 g of anhydrous ethanol were mixed, stirred and reacted at 65° C. for 45 minutes, and the anhydrous ethanol was distilled off to obtain phosphorus-bromine-doped multi-walled carbon nanotubes.
[0049] The method for preparing a high-efficiency sodium ion battery hard carbon negative electrode of the present invention comprises the following steps:
[0050] Weigh 8g of hard carbon negative electrode material, 0.8g of conductive agent, and 1.2g of sodium carboxymethyl cellulose and grind them evenly. Add 12g of deionized water and stir magnetically for 4h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 160μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard was prepared.
[0051] Example 3
[0052] The preparation method of the hard carbon negative electrode material used in the present invention is as follows:
[0053] S1: Weigh 18g of anthracite and crush it with a jaw crusher, and then crush it again with a jet mill;
[0054] S2: The powder after the pulverization treatment is washed with a mixed solution of 1.4M dilute hydrochloric acid solution and anhydrous ethanol for 8 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0055] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:1, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:2.8;
[0056] S3: Place the precursor material into a tubular furnace, introduce argon gas at a gas flow rate of 35cc / min, heat up to 1500℃ at a heating rate of 2℃ / min, and carbonize at high temperature for 2h. After carbonization, slowly cool to room temperature at a cooling rate of 4℃ / min to obtain a hard carbon negative electrode material.
[0057] The conductive agent used in the present invention is phosphorus-bromine doped multi-walled carbon nanotubes, and the preparation method thereof is as follows:
[0058] 175 g of amino-modified multi-walled carbon nanotubes (CNT903: NH 2 : 0.45wt%; CAS No.: 308068-56-6), 17g of diethyl allyl phosphate, 0.04g of 1-allyl-3-methylimidazolium bromide, 5g of sodium tert-butoxide and 1300g of anhydrous ethanol were mixed, stirred and reacted at 65°C for 60 minutes, and the anhydrous ethanol was distilled off to obtain phosphorus-bromine-doped multi-walled carbon nanotubes.
[0059] The method for preparing a high-efficiency sodium ion battery hard carbon negative electrode of the present invention comprises the following steps:
[0060] Weigh 8g of hard carbon negative electrode material, 1.0g of conductive agent, and 1.6g of sodium carboxymethyl cellulose and grind them evenly. Add 12g of deionized water and stir magnetically for 4h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 170μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard was prepared.
[0061] Example 4
[0062] The preparation method of the hard carbon negative electrode material used in the present invention is as follows:
[0063] S1: Weigh 20g of sub-bituminous coal and crush it with a jaw crusher, and then crush it again with a jet mill;
[0064] S2: The powder after the pulverization treatment is washed with a mixed solution of 1.6M dilute hydrochloric acid solution and anhydrous ethanol for 10 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0065] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:1.2, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:3.2;
[0066] S3: Place the precursor material into a tubular furnace, introduce helium at a gas flow rate of 45cc / min, heat up to 1650℃ at a heating rate of 1℃ / min, and carbonize at high temperature for 3h. After carbonization, slowly cool to room temperature at a cooling rate of 3℃ / min to obtain a hard carbon negative electrode material.
[0067] The conductive agent used in the present invention is phosphorus-bromine doped multi-walled carbon nanotubes, and the preparation method thereof is as follows:
[0068] 200 g of amino-modified multi-walled carbon nanotubes (CNT903: NH 2 : 0.45wt%; CAS No.: 308068-56-6), 20g of diethyl allyl phosphate, 0.05g of 1-allyl-3-methylimidazolium bromide, 6g of sodium tert-butoxide and 1400g of anhydrous ethanol were mixed, stirred and reacted at 70°C for 70 minutes, and the anhydrous ethanol was distilled off to obtain phosphorus-bromine-doped multi-walled carbon nanotubes.
[0069] The method for preparing a high-efficiency sodium ion battery hard carbon negative electrode of the present invention comprises the following steps:
[0070] Weigh 10g of hard carbon negative electrode material, 1.2g of conductive agent, and 2g of polyvinylidene fluoride and grind them evenly. Add 18g of deionized water and stir magnetically for 6h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 180μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard is prepared.
[0071] Comparative Example 1
[0072] The preparation method of the hard carbon negative electrode material used in Comparative Example 1 is as follows:
[0073] S1: Weigh 10g of blue carbon and crush it with a jaw crusher, and then crush it again with a jet mill;
[0074] S2: The powder after the pulverization treatment is washed with a mixed solution of 0.8M dilute hydrochloric acid solution and anhydrous ethanol for 6 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0075] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:0.8, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:1.6;
[0076] S3: Place the precursor material into a tubular furnace, introduce high-purity nitrogen at a gas flow rate of 15cc / min, heat up to 1250℃ at a heating rate of 5℃ / min, and carbonize at high temperature for 1h. After carbonization, slowly cool down to room temperature at a cooling rate of 5℃ / min to obtain a hard carbon negative electrode material.
[0077] A method for preparing a hard carbon negative electrode for a sodium ion battery, the operating steps of which are:
[0078] Weigh 6g of hard carbon negative electrode material, 0.6g of amino-modified multi-walled carbon nanotubes, and 0.8g of sodium polyacrylate and grind them evenly. Add 8g of deionized water and stir magnetically for 3h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 150μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard was prepared.
[0079] Comparative Example 2
[0080] The preparation method of the hard carbon negative electrode material used in Comparative Example 2 is as follows:
[0081] S1: Weigh 10g of blue carbon and crush it with a jaw crusher, and then crush it again with a jet mill;
[0082] S2: The powder after the pulverization treatment is washed with a mixed solution of 0.8M dilute hydrochloric acid solution and anhydrous ethanol for 6 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0083] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:0.8, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:1.6;
[0084] S3: Place the precursor material into a tubular furnace, introduce high-purity nitrogen at a gas flow rate of 15cc / min, heat up to 1250℃ at a heating rate of 5℃ / min, and carbonize at high temperature for 1h. After carbonization, slowly cool down to room temperature at a cooling rate of 5℃ / min to obtain a hard carbon negative electrode material.
[0085] The conductive agent used is phosphorus-doped multi-walled carbon nanotubes, and the preparation method thereof is as follows:
[0086] 100 g of amino-modified multi-walled carbon nanotubes (CNT903: NH 2 : 0.45wt%; CAS number: 308068-56-6), 10g of diethyl allyl phosphate, 3g of sodium tert-butoxide and 1000g of anhydrous ethanol were mixed, stirred and reacted at 60°C for 30 minutes, and the anhydrous ethanol was distilled off to obtain phosphorus-doped multi-walled carbon nanotubes.
[0087] A method for preparing a hard carbon negative electrode for a sodium ion battery, the operating steps of which are:
[0088] Weigh 6g of hard carbon negative electrode material, 0.6g of conductive agent, and 0.8g of sodium polyacrylate and grind them evenly. Add 8g of deionized water and stir magnetically for 3h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 150μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard was prepared.
[0089] Comparative Example 3
[0090] The preparation method of the hard carbon negative electrode material used in Comparative Example 3 is as follows:
[0091] S1: Weigh 10g of blue carbon and crush it with a jaw crusher, and then crush it again with a jet mill;
[0092] S2: The powder after the pulverization treatment is washed with a mixed solution of 0.8M dilute hydrochloric acid solution and anhydrous ethanol for 6 hours by stirring, and then washed with deionized water until neutral, and dried to obtain a precursor material;
[0093] The mass ratio of the dilute hydrochloric acid solution to anhydrous ethanol is 1:0.8, and the mass ratio of the crushed powder to the mixed solution of dilute hydrochloric acid and anhydrous ethanol is 1:1.6;
[0094] S3: Place the precursor material into a tubular furnace, introduce high-purity nitrogen at a gas flow rate of 15cc / min, heat up to 1250℃ at a heating rate of 5℃ / min, and carbonize at high temperature for 1h. After carbonization, slowly cool down to room temperature at a cooling rate of 5℃ / min to obtain a hard carbon negative electrode material.
[0095] The conductive agent used is bromine-doped multi-walled carbon nanotubes, and the preparation method thereof is as follows:
[0096] 100 g of amino-modified multi-walled carbon nanotubes (CNT903: NH 2 : 0.45wt%; CAS No.: 308068-56-6), 0.01g 1-allyl-3-methylimidazolium bromide, 3g sodium tert-butoxide and 1000g anhydrous ethanol were mixed, stirred and reacted at 60°C for 30 minutes, and the anhydrous ethanol was distilled off to obtain bromine-doped multi-walled carbon nanotubes.
[0097] A method for preparing a hard carbon negative electrode for a sodium ion battery, the operating steps of which are:
[0098] Weigh 6g of hard carbon negative electrode material, 0.6g of conductive agent, and 0.8g of sodium polyacrylate and grind them evenly. Add 8g of deionized water and stir magnetically for 3h to obtain electrode slurry. Use a coater to evenly coat the slurry on copper foil with a coating thickness of 150μm. After drying in a vacuum oven, a hard carbon negative electrode sheet of standard was prepared.
[0099] Test Example 1
[0100] Electrochemical performance test.
[0101] Battery assembly: The hard carbon negative electrode sheet obtained in the above examples and comparative examples and the metal sodium sheet were used as the positive electrode, GF / C glass fiber film (brand: Waterman) was used as the separator, and 1 mol / L NaPF 6 (the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) as the electrolyte, and 2032 button-type sodium-ion batteries were assembled in an Ar protection glove box.
[0102] The battery was tested in the voltage range of 0 to 2.5 V, activated at 0.1C for three weeks, and cycled at 1C for 100 weeks. The discharge capacity at 0.1C in the first week and the discharge capacity retention rate after 100 cycles at 1C were recorded. The results are shown in Table 1.
[0103] Table 1
[0104]
[0105] From the electrochemical performance test results of the embodiments and comparative examples in Table 1 above, it can be seen that the negative electrode material prepared by the present invention effectively improves the discharge specific capacity and battery cycle efficiency of the sodium ion battery, especially the discharge specific capacity at 0.1C is increased by up to 19%, and the specific capacity retention rate after 100 weeks is increased by up to 5.38%, thereby improving the battery charge and discharge efficiency.
[0106] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery, characterized in that: The following steps are involved: The hard carbon negative electrode material, the conductive agent and the binder are evenly ground, water is added, and the electrode slurry is obtained after mixing, and the electrode slurry is evenly coated on the metal foil, and the hard carbon negative electrode is prepared after drying in a vacuum oven; The conductive agent is a phosphorus-bromine doped multi-walled carbon nanotube, and the preparation method includes: Under alkaline conditions, the aminated multi-walled carbon nanotubes undergo amino-alkenyl addition reactions with allyl diethyl phosphate and 1-allyl-3-methylimidazolium bromide to obtain the phosphorus-bromine doped multi-walled carbon nanotubes.
2. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 1, characterized in that: The preparation method of the phosphorus-bromine doped multi-walled carbon nanotubes is as follows: According to weight, 100-200 parts of amino multi-walled carbon nanotubes, 10-20 parts of allyl diethyl phosphate, 0.005-0.05 parts of 1-allyl-3-methylimidazolium bromide, 3-6 parts of sodium tert-butoxide and 1000-1400 parts of anhydrous ethanol are mixed, stirred and reacted at 60-70° C. for 30-70 minutes, and the anhydrous ethanol is removed to obtain the phosphorus-bromine doped multi-walled carbon nanotubes.
3. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 1, characterized in that: The preparation method of the hard carbon negative electrode material is as follows: S1: crushing the carbon-based material into powder, washing it with a mixed solution of hydrochloric acid solution and anhydrous ethanol, then washing it with water until it is neutral, and drying it to obtain a precursor material; S2: placing the precursor material into a tubular furnace, heating it to 1250-1650°C at a heating rate of 1-5°C / min under the protection of an inert gas, carbonizing it at high temperature for 1-3h, and then slowly cooling it to room temperature at a cooling rate of 3-5°C / min after carbonization to obtain the hard carbon negative electrode material.
4. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 3, characterized in that: In step S1, the carbon-based material is at least one of lignite, anthracite, and sub-bituminous coal.
5. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 3, characterized in that: In step S1, the concentration of the hydrochloric acid solution is 0.8-1.6M, and the mass ratio of the hydrochloric acid solution to anhydrous ethanol is 1:0.8-1.
2.
6. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 5, characterized in that: In step S1, the mass ratio of the powder to the mixed solution of hydrochloric acid and anhydrous ethanol is 1:1.6-3.
2.
7. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 3, characterized in that: In step S2, the inert gas is at least one of nitrogen, argon and helium, and the gas flow rate of the inert gas is 15-45cc / min.
8. The method for preparing a high-efficiency hard carbon negative electrode for a sodium ion battery according to claim 1, characterized in that: The binder is at least one of sodium polyacrylate, sodium carboxymethyl cellulose and polyvinylidene fluoride.
9. A high-efficiency sodium ion battery hard carbon negative electrode prepared by the preparation method according to any one of claims 1 to 8.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the high-efficiency sodium ion battery hard carbon negative electrode according to claim 9.
Citation Information
Cited By
Derivative biomass hard carbon material pulverization process
CN120607237A