Lithium supplementing piece, method for preparing lithium supplementing piece and negative pole piece

By using hollow metal foil and lithium layer design in lithium-ion batteries, the problem of irreversible loss of lithium-ion batteries during the first charging and discharging process is solved, and the efficient lithium replenishment of lithium-ion batteries is achieved, and the efficiency of the first circle of the battery is improved. and energy density, and improve battery performance and safety through electrochemical prelithiation.

CN119069704APending Publication Date: 2024-12-03TSINGHUA UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411058041.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the first charging and discharging process, the lithium ions are irreversible due to the formation of solid electrolyte membranes, which reduces the efficiency and energy density of the first circle of Coulombs, and there are many problems in the production and application of the prelithiation scheme.

Method used

The hollow metal foil is used as the lithium replenishing sheet, and the hollow pattern area accounts for 2/3-3/7. The lithium layer is located on the surface of the hollow metal foil. The lithium ions are supplemented during the battery charging and discharging process through the design of the hollow pattern and lithium layer, forming a An appropriate amount of lithium layer is used to compensate for irreversible losses and prelithiated the negative electrode active material by electrochemical methods.

Benefits of technology

Effectively compensates for the irreversible loss of lithium ions caused by SEI film formation and side reactions, improves the first circle of the lithium ion battery, extends the battery life, and improves the battery's battery through controllable preliminaries. Performance and security.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a lithium supplementing piece, a method for preparing the lithium supplementing piece and a negative pole piece, the lithium supplementing piece comprises a hollow metal foil, and the area ratio of hollow patterns in the hollow metal foil is 2 / 3-3 / 7; and the lithium layer is positioned on the surface of the hollow metal foil. The lithium supplement sheet can realize the technical effect of uniform lithium supplement, reduces the influence of over-lithiation or under-lithiation on the performance of a battery negative electrode active material, and further improves the performance and safety of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a lithium supplement sheet, a method for preparing the lithium supplement sheet, and a negative electrode sheet. Background Art

[0002] Lithium-ion batteries (LIBs) are one of the most important energy storage systems in today's era. They are widely used in portable electronic devices, energy storage stations, and automobiles. They have the advantages of high energy density, low self-discharge, and long life.

[0003] During the first charge and discharge process of a lithium-ion battery, a solid electrolyte membrane (SEI) will form at the negative electrode, causing a portion of the lithium ions to be "fixed" in the SEI membrane, resulting in irreversible loss of active lithium, which in turn leads to irreversible capacity loss and reduces the first-cycle coulombic efficiency. In addition, the SEI membrane will further grow or rupture and regenerate in subsequent charge and discharge cycles, resulting in further consumption of lithium ions. A pre-lithiation scheme is adopted, that is, additional lithium sources are introduced into the positive and negative electrodes by various means to compensate for the lithium loss caused by SEI formation, thereby improving the first-cycle coulombic efficiency of lithium-ion batteries and increasing energy density, which helps to extend the service life of the battery. However, the current pre-lithiation scheme still has many problems in actual production and application. Summary of the invention

[0004] In a first aspect of the present application, the present application proposes a lithium supplement sheet, comprising: a hollow metal foil, wherein the area of ​​the hollow pattern in the hollow metal foil accounts for 2 / 3-3 / 7; and a lithium layer, wherein the lithium layer is located on the surface of the hollow metal foil.

[0005] The lithium replenishing sheet proposed in the present application, wherein the area of ​​the hollow pattern in the hollow metal foil is within the aforementioned range, can appropriately replenish the lithium consumption during the battery charge / discharge reaction process, can be used to compensate for the irreversible lithium loss caused by SEI (fixed electrolyte interface) film formation and other side reactions, and has a good lithium replenishing effect.

[0006] In some embodiments, the unit area loading of the metal lithium on the hollow metal foil is 0.065 mg / cm 2 -0.075mg / cm 2 This helps to form a lithium layer of moderate thickness on the surface of the metal foil.

[0007] In some embodiments, the thickness of the lithium layer is 1.2 μm-1.4 μm; and / or the thickness of the metal foil is 6 μm-9 μm. Thus, the metal foil can provide sufficient manufacturing support for the lithium layer and is suitable for processing in battery production.

[0008] In some embodiments, the metal foil includes at least one of copper foil, composite copper foil, foam nickel, gold foil, silver foil, zinc foil, and cobalt foil. Thus, the aforementioned metal foils can be used as the base material of the lithium layer to support the lithium layer.

[0009] In some embodiments, the preset hollow pattern includes at least one of a rhombus, a trapezoid, a triangle, a quadrilateral, and a pentagon, thereby facilitating the deintercalation of lithium ions between the positive and negative electrodes.

[0010] In the second aspect of the present application, the present application proposes a method for preparing a lithium supplement sheet, comprising: removing a portion of a preset hollow pattern on a metal foil from the metal foil to obtain a hollow metal foil, wherein the area ratio of the preset hollow pattern to the metal foil is 2 / 3-3 / 7; forming a lithium layer on the surface of the hollow metal foil to obtain a lithium supplement sheet.

[0011] The present application proposes a method for preparing a lithium replenishment sheet. The lithium replenishment area and lithium replenishment dosage of the lithium replenishment sheet produced by this method are controllable and adjustable to achieve the technical effect of uniform lithium replenishment, reduce the impact of over-lithiation or under-lithiation on the performance of the battery's negative electrode active material, and thereby improve the battery's performance and safety.

[0012] In some embodiments, the method of forming a preset hollow pattern on the metal foil includes at least one of photolithography, laser etching, electrochemical etching, chemical etching, printing, and transfer; and / or, the method of removing a portion of the preset hollow pattern on the metal foil from the metal foil includes at least one of chemical etching, laser cutting, electrochemical etching, mechanical cutting, and electric spark machining.

[0013] Thus, a designed pattern shape can be formed on the metal foil material by a simple method, and then the metal foil is hollowed out by the above method to form a metal foil with a hollowed-out pattern.

[0014] In some embodiments, the method of forming a lithium layer on the surface of the hollow metal foil includes at least one of evaporation, rolling, and magnetron sputtering. Thus, a lithium layer can be formed on the surface of the hollow metal foil, and the thickness of the formed lithium layer is uniform and controllable.

[0015] In some embodiments, the method for preparing a lithium supplement sheet further comprises: washing the hollow metal foil, wherein the cleaning agent comprises at least one of deionized water, dilute hydrochloric acid, dilute sulfuric acid, dilute sodium hydroxide, isopropyl alcohol, and ethanol, thereby removing the residual chemical substances from the hollowing process or the debris generated during the cutting process.

[0016] In the third aspect of the present application, the present application proposes a negative electrode plate, including a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector, and the side of the negative electrode active material layer away from the negative electrode current collector has the lithium supplement sheet proposed in the present application.

[0017] The negative electrode plate proposed in the present application includes the lithium supplement sheet proposed in the present application. The pre-lithiation treatment of the lithium battery is completed by the lithium supplement sheet to increase the release of the positive electrode active material and the proportion of active lithium in the electrolyte used for charge transfer. The lithium battery composed of the negative electrode plate has excellent battery capacity and cycle stability. DETAILED DESCRIPTION

[0018] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field to which this application belongs; the terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application; unless otherwise specified, the numerical values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application).

[0019] The terms "including" and "having" in the specification and claims of the present application and any modifications thereof are open expressions, that is, including the contents specified in the present application but not excluding other contents.

[0020] In the description of this application, regardless of whether the words "about" or "approximately" are used, all the numbers disclosed herein are approximate values. The value of each number may differ by less than 10% or a reasonable difference considered by those skilled in the art, such as 1%, 2%, 3%, 4% or 5%.

[0021] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0022] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0023] The pre-lithiation is achieved by adding SLMP (stabilized lithium metal powder) during the homogenization process or coating the SLMP dispersion on the surface of the pole piece, or by rolling a lithium belt onto the pole piece. However, there are problems such as high preparation cost, and the method of rolling the lithium belt onto the pole piece is difficult to ensure the uniformity of the pre-lithiation of the negative electrode. The shortcomings of the chemical pre-lithiation method are that the organic lithium solution has low chemical stability and poor lithium source utilization. The pre-lithiation technology of controllable pre-lithiation treatment provided in the present application adopts an electrochemical method to pre-lithiate the negative electrode active material. A metal foil with a lithium layer is prepared and placed in contact with the surface of the negative electrode to achieve the purpose of introducing an additional lithium source.

[0024] The controllable pre-lithiation treatment pre-lithiation technology provided in the present application uses an electrochemical method to pre-lithiate the negative electrode active material. A metal foil with a lithium layer is prepared and placed in contact with the negative electrode surface to achieve the purpose of introducing an additional lithium source.

[0025] In a first aspect of the present application, a lithium supplement sheet is proposed, comprising: a hollow metal foil, wherein the area of ​​the hollow pattern in the hollow metal foil accounts for about 2 / 3-3 / 7; and a lithium layer, wherein the lithium layer is located on the surface of the hollow metal foil.

[0026] The lithium replenishment sheet proposed in this application is an electrochemical technology means to achieve negative electrode lithium replenishment. The lithium replenishment method of the lithium replenishment sheet is to design a hollow pattern and control the size of the hollow area per unit area to adjust the lithium replenishment area within an appropriate range. The lithium ions lost due to the formation of the SEI layer are replenished without affecting the ability of the negative electrode active material to react with lithium during the charge and discharge process.

[0027] In some embodiments, the lithium supplement sheet is arranged on the surface of the negative electrode active material layer, and the negative electrode sheet, the separator, and the negative electrode sheet can be wound into a battery cell.

[0028] In some embodiments, the unit area loading of the metal lithium on the hollow metal foil is 0.065 mg / cm 2 -0.075mg / cm 2 .

[0029] When the loading amount of metallic lithium on the hollow metal foil is within the aforementioned range, the lithium replenishment capacity of the lithium replenishment sheet is relatively appropriate and can achieve a reasonable lithium replenishment depth, thereby fully compensating for the lithium ions consumed by the SEI film formed by the negative electrode active material during the first charge and discharge process, so as to improve the first cycle efficiency of the battery.

[0030] In some embodiments, the thickness of the lithium layer is 1.2 μm-1.4 μm; and / or the thickness of the metal foil is 6 μm-9 μm.

[0031] When the thickness of the lithium layer is within the aforementioned range, the capacity of the battery including the lithium supplement sheet can be improved. The lithium layer on the lithium supplement sheet can compensate for the irreversible lithium loss in the first cycle of the battery. When the thickness of the metal foil is within the aforementioned range, the metal foil has a certain mechanical strength, and can maintain the required mechanical properties during the hollowing process and battery preparation and processing, which is conducive to improving the safety and reliability of the battery.

[0032] In some embodiments, the metal foil includes at least one of copper foil, composite copper foil, foam nickel, gold foil, silver foil, zinc foil, and cobalt foil. Thus, the aforementioned metal foils can be used as the base material of the lithium layer to support the lithium layer.

[0033] The metal foil has high mechanical strength, high conductivity, high strength, and high flexibility, can carry the lithium layer, and can adapt to the bending process of the negative electrode plate.

[0034] In some embodiments, the preset hollow pattern includes at least one of a rhombus, a trapezoid, a triangle, a quadrilateral, and a pentagon.

[0035] By changing the arrangement of the hollow patterns, the intervals between the hollow patterns, and the line width of the hollow patterns, the distribution of the lithium layer on the metal foil can be adjusted, thereby adjusting the dosage and location of the lithium replenishment treatment.

[0036] In the second aspect of the present application, the present application proposes a method for preparing a lithium supplement sheet, comprising: removing a portion of a preset hollow pattern on a metal foil from the metal foil to obtain a hollow metal foil, wherein the area ratio of the preset hollow pattern to the metal foil is 2 / 3-3 / 7; forming a lithium layer on the surface of the hollow metal foil to obtain a lithium supplement sheet.

[0037] The pre-lithium treatment is carried out by using the pre-lithium sheet, and the operation method is simple. The lithium supplement sheet has no effect on the cycle process of the negative electrode active material, making the lithium insertion process safer and more uniform.

[0038] In some embodiments, the method of forming a preset hollow pattern on the metal foil includes at least one of photolithography, laser etching, electrochemical etching, chemical etching, printing, and transfer; and / or, the method of removing a portion of the preset hollow pattern on the metal foil from the metal foil includes at least one of chemical etching, laser cutting, electrochemical etching, mechanical cutting, and electric spark machining.

[0039] In some embodiments, after the hollow metal foil is prepared, the hollow pattern area is polished and smoothed.

[0040] The metal foil that has been hollowed out is inspected and polished and smoothed to reduce the burrs on the corners of the hollowed-out pattern, which is beneficial to the formation of the lithium layer.

[0041] In some embodiments, the method of forming a lithium layer on the surface of the hollow metal foil includes at least one of evaporation treatment, calendering treatment, and magnetron sputtering treatment.

[0042] In some embodiments, lithium metal is evaporated onto a hollow metal foil by a vacuum evaporation system or an electron beam evaporation system to prepare a lithium supplement electrode.

[0043] Performing the evaporation process in a high vacuum environment can prevent the lithium metal from reacting with oxygen and moisture in the air during the evaporation process.

[0044] In some embodiments, lithium metal is evaporated onto a hollowed copper electrode according to the following method: (1) the cleaned hollowed metal foil and the lithium source stored and treated in a water-free and oxygen-free environment are loaded into an evaporation device. (2) the evaporation device is started, and the air in the cavity of the evaporation device is extracted to achieve a high vacuum state, i.e., 10 - 6 Torr-10 -7 Torr. (3) Heat the lithium source to its evaporation temperature, which is about 450°C, through resistance heating or electron beam heating to vaporize the lithium metal. (4) The lithium vapor diffuses in a vacuum environment, and the deposition rate and thickness of the lithium metal are controlled by adjusting the heating power and the evaporation time, so that the lithium vapor condenses on the surface of the hollow metal foil to form a uniform lithium layer. (5) After the lithium deposition is completed, gradually lower the cavity temperature to cool the hollow metal foil and the deposited lithium layer. (6) During the cooling process, slowly backfill the inert gas into the cavity of the evaporation equipment to prevent the lithium film from contacting oxygen and moisture in the air. (7) Open the cavity of the evaporation equipment and take out the hollow metal foil on which the lithium layer has been deposited. (8) Perform surface passivation treatment on the deposited lithium layer. (9) Package the hollow metal layer that forms the lithium layer

[0045] In some embodiments, the method for preparing a lithium supplement sheet further comprises: cleaning the hollow metal foil, wherein the cleaning agent comprises at least one of deionized water, dilute hydrochloric acid, dilute sulfuric acid, dilute sodium hydroxide, isopropanol, and ethanol.

[0046] The cleaning process can remove the debris generated during the metal foil processing and hollowing process or other impurities attached during the production process, which is conducive to the formation of a lithium layer on the surface of the metal foil.

[0047] In the third aspect of the present application, the present application proposes a negative electrode plate, including a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector, and the side of the negative electrode active material layer away from the negative electrode current collector has the lithium supplement sheet proposed in the present application.

[0048] In some embodiments, during the process of assembling the battery cell, the negative electrode plate and the positive electrode are assembled into a lithium battery, and the positive and negative electrodes are separated by an isolation membrane using a Z-shaped folding method, wherein the lithium supplement sheet is located between the negative electrode plate and the isolation membrane, and then the electrolyte is injected into the battery cell, and finally it is encapsulated with an aluminum-plastic film.

[0049] In some embodiments, the prepared copper foil with a quantitative lithium layer deposited thereon is placed on the surface of the negative electrode to form a negative electrode sheet, and then the positive and negative electrodes are wound to form a battery core, and an electrolyte is injected to prepare a lithium battery. In some embodiments, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes at least one of a graphite material, a hard carbon material, a soft carbon material, a silicon-based material, a tin-based material, a metal oxide, and a phosphide.

[0050] In some embodiments, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes at least one of lithium cobalt oxide (LiCoO2, LCO), lithium manganese oxide (LiMn2O4, LMO), a ternary material (Ni-Co-Mn or Ni-Co-Al), a lithium-rich manganese-based material (LRMO), and lithium iron phosphate (LiFePO4, LFP).

[0051] In some embodiments, the lithium salt in the electrolyte includes at least one of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium borofluoride (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium difluoroborate oxalate (LiODFB).

[0052] In some embodiments, the lithium salt concentration in the battery cell of the lithium battery has different concentration ranges and common concentrations according to different lithium salts: including lithium hexafluorophosphate (LiPF6) with a typical concentration range of 0.8-1.5M (mol) and a common concentration of 1M; lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) with a typical concentration range of 0.6mol / L-1.5mol / L and a common concentration of 1mol / L; lithium bis(fluorosulfonyl)imide (LiFSI) with a typical concentration range of 0.6mol / L-1.5mol / L and a common concentration of 1mol / L; lithium borofluoride (LiBF4) with a typical concentration range of 0.5mol / L-1.2mol / L and a common concentration of 1mol / L; lithium trifluoromethanesulfonate (LiCF3SO3) with a typical concentration range of 0.5mol / L-1mol / L and a common concentration of 1mol / L; lithium difluoroborate oxalate (LiODFB) with a typical concentration range of 0.8mol / L-1.5mol / L and a common concentration of 1mol / L.

[0053] In some embodiments, the solvent in the electrolyte includes at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), propylene carbonate (PC), 1,2-dimethoxyethane (DME), and diethylene glycol dimethyl ether (DEGDME).

[0054] In some embodiments, the electrolyte additives in the electrolyte include film-forming additives: vinyl carbonate (VC), fluoroethylene carbonate (Fluoroethylene Carbonate, FEC); high-voltage stabilizers: triethyl phosphate (TEP), 1,3-propane sultone (PS); flame retardant additives: triphenyl phosphate (TPP), lithium hexafluorophosphate (LiPF6) derivatives; overcharge protection additives: 2,5-difluorobenzene (2,5-Difluorobenzene), p-xylene (p-Xylene).

[0055] In some embodiments, the electrolyte additive in the electrolyte includes a conductive additive: lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0056] In some embodiments, the electrolyte additive of the lithium battery includes an interface modification additive: fluorinated ethylene carbonate (Fluorinated Ethylene Carbonate, FEC), vinylene carbonate (Vinylene Carbonate, VC).

[0057] In some embodiments, the electrolyte additive of the lithium battery includes an inhibitor: epoxide (such as propylene oxide).

[0058] In some embodiments, the electrolyte additive of the lithium battery includes a wetting agent: lithium perfluorohexane sulfonate (LiPFHS).

[0059] In some embodiments, the electrolyte additive of the lithium battery includes an acidic scavenger: lithium zinc hydrochloride (Li2ZnO2).

[0060] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.

[0061] Example 1

[0062] The diamond pattern was etched on the copper foil by chemical etching, and then 1g of lithium was evaporated on 2.7m 2 It was placed on a hollow copper foil, encapsulated and temporarily stored after passivation, and then placed on a graphite negative electrode sheet. A lithium-rich manganese-based material (LRMO) was used as the positive electrode. The negative electrode: positive electrode (N / P) was 1.05, and the electrolyte was 1 mol / L LiPF6. The EC:DMC volume ratio was 3:7 and assembled into a soft-pack battery. It was charged to 4.3V and discharged to 2.5V.

[0063] Example 2

[0064] A triangular pattern was cut on the copper foil by laser cutting, and then 0.5g of lithium was evaporated on the 1.3m 2 It is placed on a hollow copper foil, encapsulated and temporarily stored after passivation, and then placed on a silicon-carbon electrode. It is assembled into a soft-pack battery with lithium cobalt oxide material (LiCO2) as the positive electrode, the negative electrode: positive electrode (N / P) is 1.1, and the electrolyte is 1 mol / L LiPF6. The volume ratio of EC:EMC is 1:1. It is charged to 4.2V and discharged to 3.0V.

[0065] Example 3

[0066] A trapezoidal pattern was cut on the copper foil by physical cutting, and then 1.5g of lithium was evaporated on the 3.5m 2 It is placed on a hollow copper foil, encapsulated and temporarily stored after passivation, and then placed on a hard carbon electrode. It is assembled into a soft-pack battery with lithium iron phosphate material (LiFePO4) as the positive electrode, the negative electrode: positive electrode (N / P) is 1.05, and the electrolyte is 1 mol / L LiPF6. The mass ratio of EC:EMC:DMC is 1:1:1. It is charged to 3.5V and discharged to 2.0V.

[0067] Comparative Example 1

[0068] Comparative Example 1 is consistent with Example 1, except that 1 g of lithium is then evaporated on a 1.5 m 2 On copper foil.

[0069] The battery in the above embodiment and comparative example was subjected to cycle performance test. The test method is as follows. The test results are shown in Table 1.

[0070] Cycle performance:

[0071] The full battery with the positive electrode material being lithium nickel manganese oxide (LRMO) and the negative electrode material being graphite was charged at 0.1C, with the specific capacity set to 180 mAh / g and the operating voltage being 2.5 V-4.3 V. The capacity retention rate at the 100th cycle was analyzed.

[0072] The full battery with lithium cobalt oxide (LCO) as the positive electrode material and graphite as the negative electrode material was charged at 0.1C, with the specific capacity set to 160 mAh / g and the operating voltage set to 3 V-4.2 V. The capacity retention rate at the 100th cycle was analyzed.

[0073] The full battery with lithium iron phosphate (LFP) as the positive electrode material and graphite as the negative electrode material was charged at 0.1C, the specific capacity was set to 150mAh / g, and the operating voltage was 2V-3V. The capacity retention rate at the 100th cycle was analyzed.

[0074] Table 1

[0075] serial number Capacity retention rate / % Example 1 97.71% Example 2 90.30% Example 3 99.01% Comparative Example 1 <80% (failure)

[0076] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.

[0077] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A lithium supplement tablet, It is characterized in that include: Hollow metal foil, wherein the area of ​​the hollow pattern in the hollow metal foil accounts for 2 / 3-3 / 7; A lithium layer is located on the surface of the hollow metal foil.

2. The lithium supplement tablet according to claim 1, It is characterized in that The unit area loading of the metal lithium on the hollow metal foil is 0.065 mg / cm 2 -0.075mg / cm 2 .

3. The lithium supplement tablet according to claim 1 or 2, It is characterized in that The thickness of the lithium layer is 1.2 μm-1.4 μm; and / or the thickness of the metal foil is 6 μm-9 μm.

4. The lithium supplement tablet according to claim 1 or 2, It is characterized in that The metal foil includes at least one of copper foil, composite copper foil, foam nickel, gold foil, silver foil, zinc foil and cobalt foil.

5. The lithium supplement tablet according to claim 1 or 2, It is characterized in that The hollow pattern includes at least one of a rhombus, a trapezoid, a triangle, a quadrilateral, and a pentagon.

6. A method for preparing the lithium supplement tablet according to any one of claims 1 to 5, It is characterized in that include: Removing a portion of a preset hollow pattern on the metal foil from the metal foil to obtain a hollow metal foil, wherein the area ratio of the preset hollow pattern to the metal foil is 2 / 3-3 / 7; A lithium layer is formed on the surface of the hollow metal foil to obtain a lithium supplement sheet.

7. The method according to claim 6, It is characterized in that The method of forming the preset hollow pattern on the metal foil includes at least one of photolithography, laser etching, electrochemical etching, chemical etching, printing, and transfer; and / or, The method for removing the portion of the metal foil with a preset hollow pattern from the metal foil includes at least one of chemical etching, laser cutting, electrochemical etching, mechanical cutting, and electric spark machining.

8. The method according to claim 6, It is characterized in that The method for forming the lithium layer on the surface of the hollow metal foil includes at least one of evaporation treatment, rolling treatment, and magnetron sputtering treatment.

9. The method according to claim 6, It is characterized in that Further including: The hollow metal foil is cleaned, and the cleaning agent used in the cleaning process includes at least one of deionized water, dilute hydrochloric acid, dilute sulfuric acid, dilute sodium hydroxide, isopropyl alcohol, and ethanol.

10. A negative electrode sheet, It is characterized in that The invention comprises a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector, wherein the side of the negative electrode active material layer away from the negative electrode current collector has the lithium supplement sheet according to any one of claims 1 to 5.

Citation Information

Cited By

  • Liquid injection method of lithium battery

    CN120728197A