Electrolyte, preparation method of electrolyte, battery and electrochemical device

By adding hydrogen-containing negative ion compounds, such as borohydride compounds, to the lithium-ion battery electrolyte, the performance deterioration caused by trace amounts of water and hydrofluoric acid in lithium-ion batteries is solved, and the water and acid content is reduced through hydrogen exhaust, which significantly improves the battery. cyclic storage performance and stability.

CN119069799APending Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310650664.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the manufacturing process of lithium-ion batteries, the positive and negative electrode sheets and isolation films are prone to absorb moisture in the environment and cannot be completely removed after vacuum baking, resulting in trace amounts of water entering the electrolyte, causing the decomposition of lithium hexafluorophosphate, reducing the lithium salt content and corroding SEI. Interface mask, deteriorates electrochemical properties.

Method used

Add hydrogen-containing negative ions to the electrolyte, such as borohydride compounds. The hydrogen-containing negative ions react with trace amounts of water and hydrofluoric acid to form hydrogen, which is discharged through the negative pressure forming process, reduce the content of water and hydrofluoric acid, and enhance the ions at the electrode interface Conductivity and stability.

Benefits of technology

Significantly improve the circulating storage performance of lithium-ion batteries, reduce corrosion of SEI interface masks, maintain low water and hydrofluoric acid content, and improve battery stability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an electrolyte, a preparation method of the electrolyte, a battery and an electrochemical device. The electrolyte comprises a compound containing hydrogen anions, a lithium salt and a solvent. The compound containing the hydrogen anions is added into the electrolyte, the hydrogen anions are high in reaction activity and extremely easy to react with trace water and hydrofluoric acid in the electrolyte to generate hydrogen, and the generated hydrogen can be discharged from the interior of a battery system in a negative pressure formation process, so that corrosion of an SEI interface film is reduced. A compound containing hydrogen anions is introduced into the electrolyte, so that the water content and hydrofluoric acid content of a battery system can be maintained at a low level, and the cycle storage performance of the lithium ion battery is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to an electrolyte, a method for preparing the electrolyte, a battery and an electrochemical device. Background Art

[0002] The manufacturing cycle of lithium-ion batteries is long. The positive and negative pole pieces and the isolation membrane easily absorb moisture from the environment, which cannot be completely removed during the vacuum baking process. When the electrolyte is injected, trace amounts of water enter the electrolyte, causing the decomposition of lithium hexafluorophosphate, which reduces the lithium salt content. At the same time, hydrofluoric acid is also produced during the decomposition of lithium hexafluorophosphate, corroding the SEI interface film that plays a passivating role, resulting in deterioration of the battery's electrochemical performance. Summary of the invention

[0003] The present application is made in view of the above-mentioned problems, and its purpose is to provide an electrolyte that reduces the reduction of lithium salt content caused by the reaction of the electrolyte with trace water, and reduces the corrosion of SEI interface film caused by hydrofluoric acid produced by the reaction of the electrolyte with trace water.

[0004] In order to achieve the above objectives, the embodiments of the present application provide an electrolyte, a method for preparing the electrolyte, a battery and an electrochemical device.

[0005] In a first aspect, an embodiment of the present application provides an electrolyte comprising a compound containing hydrogen anions, a lithium salt, and a solvent.

[0006] Therefore, in the technical solution of the embodiment of the present application, a compound containing hydrogen anions is added to the electrolyte. Due to the high reactivity of hydrogen anions, it is very easy to react with trace water and hydrofluoric acid in the electrolyte to generate hydrogen. The generated hydrogen can be discharged from the inside of the battery system during the negative pressure formation process, thereby reducing the corrosion of the SEI interface film. The introduction of a compound containing hydrogen anions into the electrolyte can maintain the water content and hydrofluoric acid content of the battery system at a low level, significantly improving the cycle storage performance of lithium-ion batteries.

[0007] In any embodiment, the compound containing hydrogen anions includes a boron hydride compound. The introduction of boron ions into the electrolyte can make the reaction product after the electrolyte reacts with trace water introduce boron-containing substances into the electrode interface, thereby enhancing the ionic conductivity and interface stability of the electrode interface, and further improving the cycle storage performance of the lithium-ion battery.

[0008] In any embodiment, the hydrogen anion-containing compound includes at least one of alkyl lithium borohydride, alkyl sodium borohydride and alkoxy sodium borohydride. Alkyl and alkoxy groups easily form a planar triangular molecular structure of sp2 hybrid structure with the central boron atom, so the compound structure is more stable. Metallic sodium and lithium have strong reactivity, which can reduce the deterioration of battery performance caused by the introduction of other cations.

[0009] In any embodiment, the compound containing hydrogen anions includes at least one of lithium tri-sec-butyl borohydride, lithium triethyl borohydride, sodium trimethoxyborohydride, and sodium tri-sec-butyl borohydride. Boron has an atomic number of 5, two electrons in the first layer, and three electrons in the second layer. The three electrons in the second layer can be combined with three monomers providing p orbitals or s orbitals to form an sp2 hybridized planar triangular structure. Therefore, the structure of the compound containing hydrogen anions is more stable, and hydrogen anions and boron atoms can be provided better.

[0010] In any embodiment, the mass proportion of the hydrogen anion-containing compound in the electrolyte is 0.1-1%; hydrogen anions have strong reducing properties. When the mass proportion of the hydrogen anion-containing compound in the electrolyte is greater than 1%, the amount of the hydrogen anion-containing compound added is too much and the concentration is too high, which will cause part of the electrolyte solvent to polymerize, accompanied by the production of carbon dioxide, increase the viscosity of the electrolyte, and affect ion conduction. When the mass proportion of the hydrogen anion-containing compound in the electrolyte is less than 0.1%, the amount of the hydrogen anion-containing compound added is too small and the concentration is too low, which will not be enough to react with trace water and hydrofluoric acid, which is not conducive to reducing the content of trace water and hydrofluoric acid. Optionally, the mass proportion of the hydrogen anion-containing compound in the electrolyte is 0.1-0.5%.

[0011] In any embodiment, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonate imide), lithium bis(fluoromethanesulfonate imide), lithium difluorooxalatoborate and lithium difluorophosphate. At least one of the above lithium salts has a solvated structure that can play a role in lithium ion conduction, thereby improving ionic conductivity.

[0012] In any embodiment, the mass proportion of the lithium salt in the electrolyte is 5-20%; optionally, the mass proportion of the lithium salt in the electrolyte is 12-18%. When the mass proportion of the lithium salt in the electrolyte is greater than 20%, there is too much lithium salt, which will affect the solubility, increase the probability of crystallization, and affect the stability of the battery; when the mass proportion of the lithium salt in the electrolyte is less than 5%, the amount of lithium salt added is too little, the conductivity of the electrolyte is too low, and the performance of the battery is affected.

[0013] In any embodiment, the solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate. At least one of the above solvents can be used to dissolve lithium salts and compounds containing hydrogen anions, thereby improving the conductivity of the electrolyte.

[0014] In any embodiment, the mass proportion of the solvent in the electrolyte is 79-94.9%; when the mass proportion of the solvent in the electrolyte is greater than 94.9%, the lithium salt content is insufficient, the conductivity of the electrolyte is too low, and the performance of the battery is affected. When the mass proportion of the solvent in the electrolyte is less than 79%, the lithium salt content is too high, which affects the solubility, increases the probability of crystallization, and affects the stability of the battery. Optionally, the mass proportion of the solvent in the electrolyte is 81.5-87.9%.

[0015] In a second aspect, an embodiment of the present application provides a method for preparing an electrolyte, which is used to prepare the electrolyte of the first aspect of the present application, comprising the following steps:

[0016] mixing the solvent and the lithium salt to obtain a mixed solution;

[0017] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0018] By mixing the solvent with the lithium salt and then adding a compound containing hydrogen anions to obtain an electrolyte, the lithium salt can be fully contacted with the solvent and dissolved in the solvent, thereby facilitating the dissolution of the lithium salt.

[0019] In any embodiment, the step of mixing the solvent with the lithium salt to obtain a mixed solution comprises:

[0020] The solvent is cooled and mixed with the lithium salt to obtain a mixed solution.

[0021] The process of lithium salt dissolving in solvent is an exothermic process. The temperature of the mixed liquid rises, and the heat released by the lithium salt dissolving in the solvent is absorbed by cooling the solvent, thereby reducing the decomposition and deterioration of the lithium salt and the generation of hydrofluoric acid.

[0022] In any embodiment, in the step of cooling the solvent and mixing it with the lithium salt to obtain a mixed solution,

[0023] The cooling temperature is 10-20°C; optionally, the cooling temperature is 13-18°C.

[0024] The appropriate temperature can make the lithium salt dissolve without decomposition. The process of lithium salt dissolving in the electrolyte is an exothermic process. When the temperature is higher than 20°C, the excessively high temperature after exothermic release will cause the lithium salt to decompose and deteriorate, producing a large amount of hydrofluoric acid, which will reduce the conductivity and thus reduce the conductive properties of the electrolyte. When the temperature is lower than 10°C, the temperature is too low, the solubility of the lithium salt decreases, and crystallization occurs, which is not conducive to the stability of the electrolyte.

[0025] In a third aspect, an embodiment of the present application provides a battery, comprising the electrolyte of the first aspect of the present application. It is understood that the battery includes a primary battery and a secondary battery.

[0026] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising the battery of the fourth aspect of the present application. DETAILED DESCRIPTION

[0027] The following specifically discloses the embodiments of the electrolyte, the preparation method of the electrolyte, the solar power generation device, and the power-consuming device of the present application. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art.

[0028] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0029] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0030] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0031] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0032] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0033] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0034] The manufacturing cycle of lithium-ion batteries is long. The positive and negative pole pieces and the isolation membrane easily absorb moisture from the environment, which cannot be completely removed during the vacuum baking process. When the electrolyte is injected, trace amounts of water enter the electrolyte, causing the decomposition of lithium hexafluorophosphate, which reduces the lithium salt content. At the same time, hydrofluoric acid is also produced during the decomposition of lithium hexafluorophosphate, corroding the SEI interface film that plays a passivating role, resulting in deterioration of the battery's electrochemical performance.

[0035] Therefore, there are endless technologies for removing water and reducing acid in electrolytes. For example, a water removal additive and an electrolyte and a lithium-ion battery containing the additive disclose a methanesulfonic acid silicone grease water removal additive, which hydrolyzes Si-O bonds and converts water into sulfonic acid compounds and silanols, thereby achieving the purpose of water removal. However, the sulfonic acid product is still acidic, and the hydrofluoric acid content will still increase significantly, deteriorating the performance of the battery cell.

[0036] Unexpectedly, by adding compounds containing negative hydrogen ions to the electrolyte, the negative hydrogen ions can easily react with trace water and hydrofluoric acid in the electrolyte to generate hydrogen gas, which is discharged from the inside of the battery system during the negative pressure formation process, thereby reducing the moisture in the electrode liquid and reducing the content of hydrofluoric acid.

[0037] Based on this, the present application provides an electrolyte, a method for preparing the electrolyte, a positive electrode sheet, a method for preparing the positive electrode sheet, and an electrochemical device.

[0038] In a first aspect, embodiments of the present application provide an electrolyte, a method for preparing the electrolyte, a battery, and an electrochemical device.

[0039] Therefore, in the technical solution of the embodiment of the present application, a compound containing hydrogen anions is added to the electrolyte. Due to the high reactivity of hydrogen anions, it is very easy to react with trace water and hydrofluoric acid in the electrolyte to generate hydrogen. The generated hydrogen can be discharged from the inside of the battery system during the negative pressure formation process, thereby reducing the corrosion of the SEI interface film. The introduction of a compound containing hydrogen anions into the electrolyte can maintain the water content and hydrofluoric acid content of the battery system at a low level, significantly improving the cycle storage performance of lithium-ion batteries.

[0040] In any embodiment, the compound containing hydrogen anions includes a boron hydride compound. The introduction of boron ions into the electrolyte can make the reaction product after the electrolyte reacts with trace water introduce boron-containing substances into the electrode interface, thereby enhancing the ionic conductivity and interface stability of the electrode interface, and further improving the cycle storage performance of the lithium-ion battery.

[0041] In any embodiment, the hydrogen anion-containing compound includes at least one of alkyl lithium borohydride, alkyl sodium borohydride and alkoxy sodium borohydride. Alkyl and alkoxy groups easily form a planar triangular molecular structure of sp2 hybrid structure with the central boron atom, so the compound structure is more stable. Metallic sodium and lithium have strong reactivity, which can reduce the deterioration of battery performance caused by the introduction of other cations.

[0042] In any embodiment, the compound containing hydrogen anions includes at least one of lithium tri-sec-butyl borohydride, lithium triethyl borohydride, sodium trimethoxyborohydride, and sodium tri-sec-butyl borohydride. Boron has an atomic number of 5, two electrons in the first layer, and three electrons in the second layer. The three electrons in the second layer can be combined with three monomers providing p orbitals or s orbitals to form an sp2 hybridized planar triangular structure. Therefore, the structure of the compound containing hydrogen anions is more stable, and hydrogen anions and boron atoms can be provided better.

[0043] In any embodiment, the mass proportion of the compound containing hydrogen anions in the electrolyte is 0.1-1%; hydrogen anions have strong reducing properties. When the mass proportion of the compound containing hydrogen anions in the electrolyte is greater than 1%, the amount of the compound containing hydrogen anions added is too much and the concentration is too high, which will cause some electrolyte solvents to polymerize, accompanied by the production of carbon dioxide, increase the viscosity of the electrolyte, and affect ion conduction. When the mass proportion of the compound containing hydrogen anions in the electrolyte is less than 0.1%, the amount of the compound containing hydrogen anions added is too small and the concentration is too low, which will not be enough to react with trace water and hydrofluoric acid, which is not conducive to reducing the content of trace water and hydrofluoric acid. The mass proportion of the compound containing hydrogen anions in the electrolyte can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% and 1%. Optionally, the mass proportion of the compound containing hydrogen anions in the electrolyte is 0.1-0.5%.

[0044] In any embodiment, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonate imide), lithium bis(fluoromethanesulfonate imide), lithium difluorooxalatoborate and lithium difluorophosphate. At least one of the above lithium salts has a solvated structure that can play a role in lithium ion conduction, thereby improving ionic conductivity.

[0045] In any embodiment, the mass proportion of the lithium salt in the electrolyte is 5-20%; when the mass proportion of the lithium salt in the electrolyte is greater than 20%, there is too much lithium salt, which will affect the solubility, increase the probability of crystallization, and affect the stability of the battery; when the mass proportion of the lithium salt in the electrolyte is less than 5%, the amount of lithium salt added is too little, the conductivity of the electrolyte is too low, and the performance of the battery is affected. The mass proportion of the lithium salt in the electrolyte can be 5%, 8%, 10%, 12%, 15%, 18% and 20%. Optionally, the mass proportion of the lithium salt in the electrolyte is 12-18%.

[0046] In any embodiment, the solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate. At least one of the above solvents can be used to dissolve lithium salts and compounds containing hydrogen anions, thereby improving the conductivity of the electrolyte.

[0047] In any embodiment, the mass proportion of the solvent in the electrolyte is 79-94.9%; when the mass proportion of the solvent in the electrolyte is greater than 94.9%, the lithium salt content is insufficient, the conductivity of the electrolyte is too low, and the performance of the battery is affected. When the mass proportion of the solvent in the electrolyte is less than 79%, the lithium salt content is too much, which affects the solubility, increases the probability of crystallization, and affects the stability of the battery. The mass proportion of the solvent in the electrolyte can be 79%, 80%, 83%, 85%, 87%, 90%, 92% and 94.9%. Optionally, the mass proportion of the solvent in the electrolyte is 81.5-87.9%.

[0048] In a second aspect, an embodiment of the present application provides a method for preparing an electrolyte, which is used to prepare the electrolyte of the first aspect of the present application, comprising the following steps:

[0049] mixing the solvent and the lithium salt to obtain a mixed solution;

[0050] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0051] By mixing the solvent with the lithium salt and then adding a compound containing hydrogen anions to obtain an electrolyte, the lithium salt can be fully contacted with the solvent and dissolved in the solvent, thereby facilitating the dissolution of the lithium salt.

[0052] In any embodiment, the step of mixing the solvent with the lithium salt to obtain a mixed solution comprises:

[0053] The solvent is cooled and mixed with the lithium salt to obtain a mixed solution.

[0054] The process of lithium salt dissolving in solvent is an exothermic process. The temperature of the mixed liquid rises, and the heat released by the lithium salt dissolving in the solvent is absorbed by cooling the solvent, thereby reducing the decomposition and deterioration of the lithium salt and the generation of hydrofluoric acid.

[0055] In any embodiment, in the step of cooling the solvent and mixing it with the lithium salt to obtain a mixed solution,

[0056] The cooling temperature is 10-20°C; optionally, the cooling temperature is 13-18°C.

[0057] The appropriate temperature can make the lithium salt dissolve without decomposition. The process of lithium salt dissolving in the electrolyte is an exothermic process. When the temperature is higher than 20°C, the excessively high temperature after exothermic release will cause the lithium salt to decompose and deteriorate, producing a large amount of hydrofluoric acid, which will reduce the conductivity and thus reduce the conductive properties of the electrolyte. When the temperature is lower than 10°C, the temperature is too low, the solubility of the lithium salt decreases, and crystallization occurs, which is not conducive to the stability of the electrolyte.

[0058] In a third aspect, an embodiment of the present application provides a battery, comprising the electrolyte of the first aspect of the present application. It is understood that the battery includes a primary battery and a secondary battery.

[0059] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising the battery of the fourth aspect of the present application.

[0060] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0061] Example

[0062] The parameters of the electrolytes of Examples 1 to 26 of the present application and Comparative Example 1 are as shown in Table 1.

[0063] Table 1 Electrolyte parameters of Examples 1 to 26 and Comparative Example 1

[0064]

[0065]

[0066] Comparative Example 2

[0067] Comparative Example 2 is consistent with Example 1 except that trimethyl silyl methanesulfonate is used to replace the hydrogen anion compound.

[0068] Embodiment 27

[0069] A method for preparing an electrolyte comprises the following steps:

[0070] mixing the solvent and the lithium salt to obtain a mixed solution;

[0071] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0072] Embodiment 28

[0073] A method for preparing an electrolyte comprises the following steps:

[0074] The solvent is cooled and mixed with the lithium salt to obtain a mixed solution;

[0075] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0076] Embodiment 29

[0077] A method for preparing an electrolyte comprises the following steps:

[0078] The solvent is cooled to 15°C and mixed with the lithium salt to obtain a mixed solution;

[0079] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0080] Embodiment 30

[0081] A method for preparing an electrolyte comprises the following steps:

[0082] The solvent is cooled to 10°C and mixed with the lithium salt to obtain a mixed solution;

[0083] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0084] Embodiment 31

[0085] A method for preparing an electrolyte comprises the following steps:

[0086] The solvent is cooled to 18°C ​​and mixed with the lithium salt to obtain a mixed solution;

[0087] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0088] Embodiment 32

[0089] A method for preparing an electrolyte comprises the following steps:

[0090] The solvent is cooled to 20°C and mixed with the lithium salt to obtain a mixed solution;

[0091] The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

[0092] Embodiment 33

[0093] In a glove box filled with argon, the water content is less than 1ppm, the oxygen content is less than 1ppm, dimethyl carbonate, ethyl methyl carbonate and ethylene carbonate are preheated to 60°C to melt, mixed evenly in a mass ratio of 2:5:3, and cooled to 15°C; 10% by mass of lithium hexafluorophosphate is slowly added while stirring, and stirred until completely dissolved to obtain a mixed solution;

[0094] Add 1% by mass of vinylene carbonate and 1% by mass of vinyl sulfate to the mixed solution; add 0.3% of lithium triethylborohydride; and stir evenly to obtain an electrolyte.

[0095] Performance Testing

[0096] 1. Determination of water and hydrofluoric acid content

[0097] The water and hydrofluoric acid contents of the electrolytes of Examples 1 to 26 and Comparative Examples 1 to 2 at different storage times at 25° C. are detected, and the results are shown in Table 2, wherein the water content is detected by the Karl Fischer coulometric method, and the hydrofluoric acid content is detected by the triethylamine-mixed indicator titration method.

[0098] Table 2 Performance measurement of electrolytes of Examples 1 to 26 and Comparative Examples 1 to 2

[0099]

[0100]

[0101] It can be seen from the data in Table 2 that compared with Comparative Example 1 which does not contain a hydrogen anion compound, Examples 1-26 all have water removal and acid reduction effects. Compared with Comparative Example 2 containing a sulfonic acid additive, Examples 1-26 have a water removal effect equivalent to that of Comparative Example 2, but Examples 1-26 can effectively inhibit the increase in the acid content of the system, indicating that the electrolyte of the present invention can reduce water and hydrofluoric acid in the electrolyte and greatly improve the storage stability of the electrolyte.

[0102] 2. Electrochemical performance test

[0103] Preparation of positive electrode sheet: lithium iron phosphate, conductive carbon black and polyvinylidene fluoride were dispersed in nitrogen methyl pyrrolidone in a ratio of 94.9%: 2.5%: 2.5% and stirred evenly to prepare a slurry with a solid content of 65%, and then evenly coated on the surface of 13 micron thick aluminum foil with a coating weight of 220g / m 2 , drying, cold pressing, and cutting into positive electrode sheets;

[0104] Preparation of negative electrode sheet: Graphite, conductive carbon black, sodium carboxymethyl cellulose, and polystyrene butadiene rubber were dispersed in deionized water at a ratio of 96%:1%:1%:2% and stirred evenly to prepare a slurry with a solid content of 53%, and then evenly coated on the surface of a 6-micron thick copper foil with a coating weight of 110 g / m 2 , drying, cold pressing, and cutting into negative electrode sheets;

[0105] Preparation of lithium-ion battery: The positive electrode sheet, the separator, and the negative electrode sheet are wound into a battery core, and then the battery is prepared into a soft-package lithium-ion battery with a rated capacity of 2Ah after liquid injection, formation, and capacity testing. The electrolyte injected in the liquid injection process is the electrolyte of Examples 1-26 and Comparative Examples 1-5.

[0106] The capacity, first coulomb efficiency and DCR of the soft pack battery are tested. The DCR test process is as follows:

[0107] 1) At room temperature, charge at constant current to 3.65V, charge at constant voltage to a cut-off current of 100mA at 3.65V, let stand for 5 minutes, discharge at 2A constant current to 2.5V, let stand for 5 minutes, and test the initial capacity;

[0108] 2) 2A constant current discharge to 50% SOC, stand for 1h (the static end voltage is V0), continue 8A constant current discharge for 30S, the discharge end voltage is (static end voltage is V1)

[0109] Among them, DCR = (V0-V1) / 8A, and the secondary capacity and coulomb efficiency test results are shown in Table 3. The DCR test results reflect the impedance of the battery charging and discharging process. The lower the value, the smaller the polarization during the charging and discharging process, the higher the ion conduction efficiency, and the better the battery capacity.

[0110] Table 3 First capacity and coulombic efficiency test

[0111]

[0112]

[0113] It can be seen from Table 3 that the electrolyte of the present application can reduce the side reactions of the battery and improve the capacity and the first efficiency. By comparing Examples 12 to 20, as the content of the hydrogen-containing anion compound increases, the capacity and the first efficiency both increase first and then decrease, indicating that excessive hydrogen anions will affect the solvation structure of the electrolyte and will be oxidized to form a film at the positive electrode, resulting in an excessively thick interface layer, further increasing the DCR.

[0114] It can be seen from Examples 20 to 26 that the content of lithium salt and the content of solvent will affect the capacity of the electrolyte. When the mass proportion of lithium salt in the electrolyte is greater than 20%, there is too much lithium salt, which will affect the solubility, increase the probability of crystallization, and affect the stability of the battery; when the mass proportion of lithium salt in the electrolyte is less than 5%, the amount of lithium salt added is too little, the conductivity of the electrolyte is too low, and the performance of the battery is affected. When the mass proportion of the solvent in the electrolyte is greater than 94.9%, the lithium salt content is insufficient, the conductivity of the electrolyte is too low, and the performance of the battery is affected. When the mass proportion of the solvent in the electrolyte is less than 79%, the lithium salt content is too much, which affects the solubility, increases the probability of crystallization, and affects the stability of the battery.

[0115] In summary, the electrolyte proposed in this application adds a compound containing hydrogen anions to the electrolyte. Due to the high reactivity of hydrogen anions, it is very easy to react with trace water and hydrofluoric acid in the electrolyte to generate hydrogen. The generated hydrogen can be discharged from the inside of the battery system during the negative pressure formation process, thereby reducing the corrosion of the SEI interface film. The introduction of a compound containing hydrogen anions into the electrolyte can maintain the water content and hydrofluoric acid content of the battery system at a low level, significantly improving the cycle storage performance of lithium-ion batteries.

[0116] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. An electrolyte, It is characterized in that Includes compounds containing hydrogen ions, lithium salts and solvents.

2. The electrolyte according to claim 1, It is characterized in that The hydride ion-containing compound includes a boron hydride compound.

3. The electrolyte according to claim 2, It is characterized in that The compound containing hydrogen anions includes at least one of alkyl lithium borohydride, alkyl sodium borohydride and alkoxy sodium borohydride.

4. The electrolyte according to claim 3, It is characterized in that The compound containing hydrogen anions includes at least one of lithium tri-sec-butylborohydride, lithium triethylborohydride, sodium trimethoxyborohydride, and sodium tri-sec-butylborohydride.

5. The electrolyte according to any one of claims 1 to 4, It is characterized in that The mass proportion of the compound containing hydrogen anions in the electrolyte is 0.1-1%; optionally, the mass proportion of the compound containing hydrogen anions in the electrolyte is 0.1-0.5%.

6. The electrolyte according to any one of claims 1 to 5, It is characterized in that The lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonate imide), lithium bis(fluoromethanesulfonate imide), lithium difluorooxalatoborate and lithium difluorophosphate.

7. The electrolyte according to any one of claims 1 to 6, It is characterized in that The mass proportion of the lithium salt in the electrolyte is 5-20%; optionally, the mass proportion of the lithium salt in the electrolyte is 12-18%.

8. The electrolyte according to any one of claims 1 to 7, It is characterized in that The solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate.

9. The electrolyte according to any one of claims 1 to 8, It is characterized in that The mass proportion of the solvent in the electrolyte is 79-94.9%; optionally, the mass proportion of the solvent in the electrolyte is 81.5-87.9%.

10. A method for preparing the electrolyte according to any one of claims 1 to 9, It is characterized in that The following steps are involved: mixing the solvent and the lithium salt to obtain a mixed solution; The mixed solution is mixed with a compound containing hydrogen anions to obtain an electrolyte.

11. The method for preparing the electrolyte according to claim 10, It is characterized in that The steps of mixing the solvent and the lithium salt to obtain a mixed solution include: The solvent is cooled and mixed with the lithium salt to obtain a mixed solution.

12. The method for preparing the electrolyte according to claim 11, It is characterized in that In the step of cooling the solvent and mixing it with the lithium salt to obtain a mixed solution, The cooling temperature is 10-20°C; optionally, the cooling temperature is 13-18°C.

13. A battery, It is characterized in that Comprising the electrolyte according to any one of claims 1 to 9.

14. An electrical device, It is characterized in that Comprising the battery of claim 13.