Three-dimensional ordered porous carbon / manganese oxide composite wave-absorbing material as well as preparation method and application thereof
By preparing three-dimensional ordered porous carbon/manganese oxide composite materials, the orderly arrangement of nano-silicon oxide templates and hydrothermal reaction technology is used to solve the frequency band limitations of carbon materials in electromagnetic wave absorption, and the wide band absorption effect is achieved under low density , enhances the absorption capacity of the material.
Patent Information
- Application Number
- CN202411180062.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
Existing carbon materials have frequency band limitations in electromagnetic wave absorption, which cannot meet the absorption needs of wide frequency electromagnetic waves, and high conductivity leads to electromagnetic wave reflection and cannot be absorbed.
By preparing three-dimensional ordered porous carbon/manganese oxide composite materials, carbonization and etching are used to arrange nano-silicon oxide templates in an orderly manner to form a rich solid gas interface, and manganese oxide is introduced through hydrothermal reactions to optimize the impedance matching and loss of the material mechanism to achieve multiple reflections and scattering.
Achieving wide-band electromagnetic wave absorption at low density, enhancing the absorption capacity of the material, broadening the effective absorption frequency band, and improving the absorption performance through the synergistic action of multiple loss mechanisms.
Smart Images

Figure CN119060690A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of absorbing materials, and in particular to a three-dimensional ordered porous carbon / manganese oxide composite absorbing material and a preparation method and application thereof. Background Art
[0002] With the continuous progress and development of modern science and communication technology, the popularity of electronic equipment has brought great convenience to people's lives, but it has also inevitably generated a lot of electromagnetic radiation and pollution. In the field of national defense and military industry, radar technology is constantly updated, using electromagnetic waves to locate targets and carry out precise strikes. Therefore, the development of materials with excellent electromagnetic wave absorption and attenuation capabilities to improve its military anti-strike capabilities has become a current research hotspot.
[0003] Carbon materials (graphene, carbon nanotubes, carbon fibers, biochar, etc.) are widely used in the field of electromagnetic wave absorption and shielding by domestic and foreign scholars due to their low density, high specific surface area, high conductivity and excellent chemical stability. However, the skin effect caused by high conductivity causes electromagnetic waves to be strongly reflected on the surface of the material and cannot be absorbed. Therefore, it is necessary to carry out structural design or modification to achieve effective absorption of electromagnetic waves.
[0004] Three-dimensional ordered porous carbon materials with rich pore structures can further reduce density while retaining the general characteristics of carbon-based materials. In addition, the porous structure will affect the behavior of electromagnetic waves on the surface of the material, thereby improving impedance matching. However, a single loss mechanism limits its absorption of electromagnetic waves to a fixed frequency band, which cannot meet the application requirements of broadband absorbing materials. Therefore, it is necessary to introduce other loss mechanisms (dielectric, magnetic loss, etc.) to achieve response to electromagnetic waves with a wider frequency. Summary of the invention
[0005] The purpose of the present invention is to provide a three-dimensional ordered porous carbon / manganese oxide composite absorbing material and a preparation method and application thereof, so as to solve the problems existing in the above-mentioned prior art.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] The present invention provides a method for preparing a three-dimensional ordered porous carbon / manganese oxide composite wave absorbing material, comprising the following steps:
[0008] (1) impregnating an ordered nano-silicon oxide template in a phenolic resin solution, drying it, and then carbonizing it in an inert atmosphere to obtain a carbon / silicon oxide composite material;
[0009] (2) etching the carbon / silicon oxide composite material in hydrofluoric acid to obtain three-dimensional ordered porous carbon;
[0010] (3) The three-dimensional ordered porous carbon is subjected to a hydrothermal reaction with potassium permanganate to obtain a three-dimensional ordered porous carbon / manganese oxide composite absorbing material.
[0011] Furthermore, the immersion time is 20-28 hours.
[0012] Furthermore, the carbonization treatment is as follows: heating to 300-400°C at 1-2°C / min at room temperature, keeping the temperature for 2-3h, then heating to 800-900°C at 3-5°C / min, keeping the temperature for 2-3h.
[0013] Furthermore, the temperature of the hydrothermal reaction is 160-200° C., and the time is 20-28 hours.
[0014] More preferably, the phenolic resin solution is a mixture of phenolic resin and ethanol in a mass ratio of 1:4-1:5.
[0015] More preferably, 40% concentration hydrofluoric acid (HF) is used for immersion etching for 48 hours.
[0016] Furthermore, the method for preparing the ordered nano-silicon oxide template comprises the following steps:
[0017] a. stirring ethyl orthosilicate and aqueous ammonia in a mixed solvent of ethanol and water to obtain a silicon oxide dispersion;
[0018] b. The silicon oxide dispersion is sequentially centrifuged, washed, ultrasonically dispersed, and then dried, and then calcined to obtain the ordered nano-silicon oxide template.
[0019] Furthermore, the drying adopts a staged heating method; the staged heating method is drying at 20°C, 40°C, 60°C, 80°C and 100°C for 2 hours respectively.
[0020] Furthermore, the calcination treatment is: heating to 700-800°C at 2-5°C / min at room temperature and keeping the temperature for 8-16h.
[0021] The present invention further provides a three-dimensional ordered porous carbon / manganese oxide composite wave absorbing material prepared by the above preparation method.
[0022] The present invention also provides application of the three-dimensional ordered porous carbon / manganese oxide composite wave absorbing material in shielding electromagnetic radiation.
[0023] The present invention improves the microwave absorption performance of three-dimensional ordered porous carbon materials mainly from the following perspectives:
[0024] (1) Related studies have shown that the dielectric constant of pure carbon materials is insufficient to match the impedance of free space, resulting in strong reflection of electromagnetic waves on the surface of the material, but unable to enter the interior of the material and be absorbed. The three-dimensional ordered porous carbon prepared by the sacrificial template method in the present invention forms a rich solid-gas interface, which reduces the density and complex dielectric constant of the material at the same filling rate, which is conducive to the improvement of impedance matching. At the same time, this complex structure causes multiple reflections and scattering of electromagnetic waves, which is conducive to the further attenuation of electromagnetic waves by carbon materials.
[0025] (2) The introduction of low-dielectric manganese oxide reduces the overall dielectric constant of the material and further optimizes the impedance matching characteristics of the composite material to achieve a stronger electromagnetic wave absorption effect.
[0026] (3) A rich heterogeneous interface is formed between manganese oxide and carbon, causing the induced charge to accumulate at the interface due to the change in the direction of the alternating electromagnetic field, resulting in relaxation, which separates the overall positive and negative charge centers of the composite material, inducing interface polarization and dipole polarization. The emergence of polarization broadens the effective absorption frequency band of the composite material, achieving response to electromagnetic waves in more frequency bands.
[0027] (4) The present invention adjusts the ratio of manganese oxide to carbon so that the multiple loss mechanisms of conduction loss, interface polarization and dipole polarization loss work synergistically to enhance the wave absorption performance of the material, thereby enabling the composite material to achieve a wide frequency band and strong absorption effect at a low density.
[0028] The present invention uses regularly arranged nano silicon oxide as a template to prepare three-dimensional ordered porous carbon, and uses it as an absorber and carrier, and further uses a hydrothermal method to compound it with manganese oxide of different contents to obtain a three-dimensional ordered porous carbon / manganese oxide composite absorbing material. The three-dimensional ordered porous carbon prepared by the sacrificial template method of the present invention forms abundant solid-gas interfaces, thereby reducing the density and complex dielectric constant of the material, which is conducive to the improvement of impedance matching. At the same time, the complex structure causes multiple reflections and scattering of electromagnetic waves, which is conducive to the further attenuation of electromagnetic waves by carbon materials. The uniformly distributed low-dielectric manganese oxide nanoparticles bring abundant heterogeneous interfaces and dipole polarization losses, which improves the absorbing performance of the three-dimensional ordered porous carbon.
[0029] The present invention further adjusts the dielectric constant and polarization strength of the composite material by controlling the amount of manganese oxide introduced, so that the composite material exhibits the advantages of low density, wide absorption bandwidth and strong absorption capacity, thus opening up a new path for the development of efficient and multifunctional absorbing materials.
[0030] The present invention discloses the following technical effects:
[0031] The present invention utilizes the ordered porous structure design to make electromagnetic waves reflect and scatter multiple times, thereby showing a broadband wave absorption effect at a low filling rate. At the same time, the introduction of low-dielectric manganese oxide optimizes the impedance matching of the carbon material, making it easier for electromagnetic waves to enter the material and cause losses. In addition, charges accumulate at the heterogeneous interface between the carbon material and manganese oxide, inducing interface polarization.
[0032] The three-dimensional ordered porous carbon / manganese oxide composite material prepared by the present invention through structural design and component regulation strategy has the advantages of low density, wide absorption bandwidth and strong absorption capacity, and has opened up a new path for the development of efficient and multifunctional absorbing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 In the figure, (a) is a scanning electron microscopy (SEM) image of the ordered nano-silicon oxide template prepared in Example 1; (b) is a scanning electron microscopy (SEM) image of the three-dimensional ordered porous carbon prepared in Example 1; (c)-(f) are scanning electron microscopy (SEM) images of the three-dimensional ordered porous carbon / manganese oxide composite materials prepared in Example 1, Example 2, Example 3 and Example 4, respectively.
[0035] Figure 2 These are two-dimensional reflection loss images of the three-dimensional ordered porous carbon / manganese oxide composite materials prepared in Examples 1-6 in the frequency range of 2-18 GHz, wherein (a)-(f) are reflection loss images of the three-dimensional ordered porous carbon / manganese oxide composite materials prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Example 6, respectively.
[0036] Figure 3 This is the reflection loss image of the three-dimensional ordered porous carbon material prepared in Comparative Example 1 in the frequency range of 2-18 GHz. DETAILED DESCRIPTION
[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0038] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0039] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0040] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0041] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0042] Room temperature in the present invention refers to 25±2°C.
[0043] Potassium permanganate, ethyl orthosilicate, formaldehyde, phenol, ammonia water, hydrofluoric acid, hydrochloric acid, NaOH solution and anhydrous ethanol used in the embodiments of the present invention are all commercially available products, and the instruments and equipment used are all commonly used instruments and equipment in the field.
[0044] In the following embodiments of the present invention, a regularly arranged nano-silicon oxide template is prepared by combining ultrasonic dispersion and high-speed stirring. The template is immersed and dried in a phenolic resin solution, and then subjected to high-temperature carbonization treatment in an inert atmosphere of a tubular furnace to obtain a carbon / silicon oxide composite material. The carbon is etched with hydrofluoric acid to obtain a three-dimensional ordered porous carbon. The three-dimensional ordered porous carbon is then further compounded with manganese oxide of different contents through a hydrothermal reaction to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0045] Example 1
[0046] A method for preparing a three-dimensional ordered porous carbon / manganese oxide composite absorbing material:
[0047] (1) Add 29.16 g of ethyl orthosilicate to 400 mL of ethanol solution and continue stirring for 60 min to obtain liquid A. At the same time, add 60 mL of ammonia water to a mixed solution formed by 320 mL of ethanol and 18 mL of deionized water and stir for 60 min to obtain liquid B; then slowly add liquid A to liquid B and stir for 24 h to obtain a silicon oxide dispersion, centrifuge and wash four times with ethanol solvent at a speed of 6000 r / min, each time for 30 min, and ultrasonicate for 30 min after each centrifugal washing; then transfer to a vacuum drying oven and gradiently heat and dry at 20°C, 40°C, 60°C, 80°C, and 100°C for 2 h each to obtain a silicon oxide solid; the dried silicon oxide solid is calcined at 750°C in a muffle furnace for 12 h, with a heating rate of 2°C / min to obtain an ordered nano-silica template.
[0048] (2) 3 g of phenol was heated to melt at 40° C., and 0.65 g of 20 wt.% NaOH solution was added dropwise during stirring. The temperature was then raised to 70° C., 6.5 mL of 37% formaldehyde solution was added dropwise, and the mixture was stirred at 70° C. for 4 h. After cooling to room temperature, dilute hydrochloric acid was added dropwise to adjust the pH of the solution to neutral. The temperature was then raised to 70° C. and stirred until the mixture became viscous and colloid, and the colloid was dissolved in 50 mL of ethanol solution to obtain a phenolic resin solution.
[0049] (3) Take 10 mL of the phenolic resin solution obtained in step (2), immerse 1.0 g of the ordered nano-silica template prepared in step (1) in the solution for 24 h, dry it in a vacuum drying oven at 100 ° C for 24 h, and then place it in a tube furnace under an inert atmosphere (N 2 ) medium and high temperature carbonization treatment, the specific operation is: heating to 350°C at a heating rate of 1°C / min and keeping warm for 3h; then heating to 900°C at a heating rate of 5°C / min and keeping warm for 2h; to obtain a carbon-encapsulated silicon oxide composite material.
[0050] (4) The carbon-encapsulated silicon oxide composite material obtained in step (3) is etched in 40% hydrofluoric acid for 48 hours to obtain a three-dimensional ordered porous carbon after the silicon oxide is completely etched.
[0051] (5) Take 0.05mmol KMnO 4 The solid powder was dissolved in 30 mL of deionized water and stirred until completely dissolved. Subsequently, 0.04 g of the three-dimensional ordered porous carbon obtained in step (4) was added, stirred for 60 min, and then ultrasonically dispersed for 30 min. The mixture was transferred to a high-pressure reactor and kept at 180 ° C for 24 h. After the hydrothermal reaction was completed, it was centrifuged and washed three times with deionized water at 10000 r / min, and dried at 80 ° C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0052] Example 2
[0053] A method for preparing a three-dimensional ordered porous carbon / manganese oxide composite absorbing material:
[0054] Steps (1) to (4) are the same as in Example 1.
[0055] (5) Take 0.1mmol KMnO 4 The solid powder was dissolved in 30 mL of deionized water and stirred until completely dissolved. Subsequently, 0.04 g of the three-dimensional ordered porous carbon obtained in step (4) was added, stirred for 60 min, and then ultrasonically dispersed for 30 min. The mixture was transferred to a high-pressure reactor and kept at 180 ° C for 24 h. After the hydrothermal reaction was completed, it was centrifuged and washed three times with deionized water at 10000 r / min, and dried at 80 ° C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0056] Example 3
[0057] Steps (1) to (4) are the same as in Example 1.
[0058] (5) Take 0.2mmol KMnO 4 The solid powder was dissolved in 30 mL of deionized water and stirred until completely dissolved. Subsequently, 0.04 g of the three-dimensional ordered porous carbon obtained in step (4) was added, stirred for 60 min, and then ultrasonically dispersed for 30 min. The mixture was transferred to a high-pressure reactor and kept at 180 ° C for 24 h. After the hydrothermal reaction was completed, it was centrifuged and washed three times with deionized water at 10000 r / min, and dried at 80 ° C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0059] Example 4
[0060] Steps (1) to (4) are the same as in Example 1.
[0061] (5) Take 0.5mmol KMnO 4 The solid powder was dissolved in 30 mL of deionized water and stirred until completely dissolved. Subsequently, 0.04 g of the three-dimensional ordered porous carbon obtained in step (4) was added, stirred for 60 min, and then ultrasonically dispersed for 30 min. The mixture was transferred to a high-pressure reactor and kept at 180 ° C for 24 h. After the hydrothermal reaction was completed, it was centrifuged and washed three times with deionized water at 10000 r / min, and dried at 80 ° C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0062] Example 5
[0063] Steps (1) to (4) are the same as in Example 1.
[0064] (5) Take 0.1mmol KMnO 4The solid powder was dissolved in 30 mL of deionized water and stirred until completely dissolved. Subsequently, 0.04 g of the three-dimensional ordered porous carbon obtained in step (3) was added, stirred for 60 min, and then ultrasonically dispersed for 30 min. The mixture was transferred to a high-pressure reactor and kept at 160 ° C for 28 h. After the hydrothermal reaction was completed, it was washed three times with deionized water at 10000 r / min by centrifugation, and dried at 80 ° C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0065] Example 6
[0066] Steps (1) to (4) are the same as in Example 1.
[0067] (5) Take 0.1mmol KMnO 4 The solid powder was dissolved in 30 mL of deionized water and stirred until completely dissolved. Subsequently, 0.04 g of the three-dimensional ordered porous carbon obtained in step (3) was added, stirred for 60 min, and then ultrasonically dispersed for 30 min. The mixture was transferred to a high-pressure reactor and kept at 200 ° C for 20 h. After the hydrothermal reaction, the mixture was washed three times with deionized water at 10,000 r / min by centrifugation, and dried at 80 ° C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0068] Comparative Example 1
[0069] The only difference from Example 1 is that no KMnO is added before the hydrothermal reaction. 4 The steps are as follows:
[0070] Steps (1) to (4) are the same as in Example 1;
[0071] (5) 0.04 g of the three-dimensional ordered porous carbon obtained in step (4) was added to 30 mL of deionized water, stirred for 60 min, and then ultrasonically dispersed for 30 min; it was transferred to a high-pressure reactor and kept at 180°C for 24 h; after the hydrothermal reaction, it was centrifuged and washed three times with deionized water at 10,000 r / min, and dried at 80°C overnight to obtain a three-dimensional ordered porous carbon / manganese oxide composite material.
[0072] Effect verification example
[0073] Weigh 0.015g of each composite material prepared in Examples 1-6 and Comparative Example 1, mix with 0.085g of paraffin (melted by high temperature heating), and press them into microwave absorbing sample rings with an outer diameter of 7mm and an inner diameter of 3mm using a mold. The prepared sample rings were tested (2-18GHz frequency range) using a vector network analyzer of model Agilent N5245A, and the electromagnetic parameters of the samples were obtained and converted into the reflection loss constant of the material by calculation. The microwave absorption test results are shown in Table 1.
[0074] Table 1
[0075]
[0076] Figure 1 In the figure, (a) is a scanning electron microscopy (SEM) image of the ordered nano-silicon oxide template prepared in Example 1; (b) is a scanning electron microscopy (SEM) image of the three-dimensional ordered porous carbon prepared in Example 1; (c)-(f) are scanning electron microscopy (SEM) images of the three-dimensional ordered porous carbon / manganese oxide composite materials prepared in Example 1, Example 2, Example 3 and Example 4, respectively.
[0077] from Figure 1 As can be seen in (a), the silicon oxide microspheres are closely and orderly arranged together; Figure 1 (b) shows the ordered porous morphology of porous carbon. This porous morphology greatly reduces the density of the material and affects the behavior of electromagnetic waves on the surface of the carbon material, resulting in multiple reflections and scattering. Figure 1 As can be seen in (c), a small amount of manganese oxide nanoparticles are dispersed on the surface of the three-dimensional ordered porous carbon / manganese oxide composite material prepared in Example 1, and the accumulation of charges at the heterogeneous interface induces interface polarization and dipole polarization loss inside the material, thereby enhancing the electromagnetic wave absorption capability. Figure 1 As can be seen in (d), in Example 2, as the loading increases, more manganese oxide nanoparticles are evenly distributed on the surface, and the increase in the number and area of interfaces causes stronger polarization loss in the material. In addition, the manganese oxide particles are distributed in the pores of the porous carbon, which helps to form a continuous three-dimensional conductive network, thereby allowing the charge to move and jump. For Example 3-4 ( Figure 1 In (e)-(f)), the introduction of excessive manganese oxide destroys the ordered porous structure of carbon, and spontaneous agglomeration occurs between the manganese oxide particles, so the electromagnetic wave absorption performance is slightly reduced.
[0078] Figure 2 These are two-dimensional reflection loss images of the three-dimensional ordered porous carbon / manganese oxide composite materials prepared in Examples 1-6 in the frequency range of 2-18 GHz, wherein (a)-(f) are reflection loss images of the three-dimensional ordered porous carbon / manganese oxide composite materials prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Example 6, respectively.
[0079] Depend on Figure 2It can be seen that the reflection loss of the composite absorbing material prepared in Example 1 is -40.912 dB at 5.04 GHz, the corresponding thickness is 5.2 mm, and the absorption bandwidth is 4.64 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 2 is -58.361 dB at a low frequency of 13.04 GHz, the corresponding thickness is 3.0 mm, and the absorption bandwidth can reach 7.32 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 3 is -42.561 dB at 8.32 GHz, the corresponding thickness is 3.3 mm, and the absorption bandwidth is 3.39 GHz; the composite absorbing material corresponding to Example 4 has a microwave absorption performance of -38.030dB at a high frequency of 4.48GHz, the corresponding thickness is 5.9mm, and the absorption bandwidth is 4.67GHz; the composite absorbing material corresponding to Example 5 has a microwave absorption performance of -59.281dB at a high frequency of 12.4GHz, the corresponding thickness is 3.2mm, and the absorption bandwidth can reach 6.77GHz; the composite absorbing material corresponding to Example 6 has a microwave absorption performance of -43.756dB at a high frequency of 8.48GHz, and the corresponding thickness is 4.2mm.
[0080] Figure 3 This is the reflection loss image of the three-dimensional ordered porous carbon material prepared in Comparative Example 1 in the frequency range of 2-18 GHz. Figure 3 It can be seen that the minimum reflection loss of the composite absorbing material prepared in Comparative Example 1 is only -9.450 dB, corresponding to a thickness of 1.4 mm.
[0081] It can be seen that by adjusting the addition amount of manganese oxide, the microwave absorption performance of three-dimensional ordered porous carbon can be enhanced and broadband absorption can be achieved.
[0082] The three-dimensional ordered porous carbon / manganese oxide composite absorbing material prepared by the present invention exhibits a regular microscopic morphology after being composited with the three-dimensional ordered porous carbon under different manganese oxide attachments, and the absorbing performance is significantly enhanced. The quality of the absorbing performance can be reflected by the reflection loss (RL) value. It can be found that when manganese oxide is not present, the porous carbon material has poor absorbing performance, and the maximum reflection loss of the absorber is -9.450dB when the thickness is 1.4mm. When a small amount of manganese oxide is introduced (0.05mmol), the minimum reflection loss of the composite material reaches -40.912dB at 5.04GHz, and the absorption bandwidth is 4.64GHz; when the manganese oxide content is 0.1mmol, the excellent ratio of carbon and manganese oxide makes the composite material exhibit excellent absorbing performance, the minimum reflection loss reaches -58.361dB at 13.04GHz, and the effective absorption bandwidth is as high as 7.32GHz; when the manganese oxide content is 0.2mmol, the minimum reflection loss of the composite material at 5.04GHz reaches -42.561dB; the absorbing performance of the composite material begins to decline, and the minimum reflection loss at 4.48GHz is -38.03GHz as the manganese oxide loading is continued to increase.
[0083] The three-dimensional ordered porous carbon and manganese oxide composite material of the present invention is designed with a porous carbon structure to introduce more solid / gas interfaces, reduce the material filling rate, and realize multiple reflections of electromagnetic waves in the material; the introduction of manganese oxide brings abundant heterogeneous interfaces, optimizes the electromagnetic parameters and impedance matching of the material. The synergistic effect of conduction loss, interface polarization and dipole polarization loss makes the three-dimensional ordered porous carbon / manganese oxide composite material show excellent electromagnetic wave absorption performance.
[0084] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a three-dimensional ordered porous carbon / manganese oxide composite absorbing material, characterized in that: The following steps are involved: (1) impregnating an ordered nano-silicon oxide template in a phenolic resin solution, drying it, and then carbonizing it in an inert atmosphere to obtain a carbon / silicon oxide composite material; (2) etching the carbon / silicon oxide composite material in hydrofluoric acid to obtain three-dimensional ordered porous carbon; (3) The three-dimensional ordered porous carbon is subjected to a hydrothermal reaction with potassium permanganate to obtain a three-dimensional ordered porous carbon / manganese oxide composite absorbing material.
2. The preparation method according to claim 1, characterized in that: The immersion time is 20-28 hours.
3. The preparation method according to claim 1, characterized in that: The carbonization treatment is as follows: heating to 300-400°C at 1-2°C / min at room temperature, keeping the temperature for 2-3h, then heating to 800-900°C at 3-5°C / min, keeping the temperature for 2-3h.
4. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 160-200° C. and the time is 20-28 hours.
5. The preparation method according to claim 1, characterized in that: The method for preparing the ordered nano-silicon oxide template comprises the following steps: a. stirring ethyl orthosilicate and aqueous ammonia in a mixed solvent of ethanol and water to obtain a silicon oxide dispersion; b. The silicon oxide dispersion is sequentially centrifuged, washed, ultrasonically dispersed, and then dried, and then calcined to obtain the ordered nano-silicon oxide template.
6. The preparation method according to claim 5, characterized in that: The drying adopts a staged heating method; the staged heating method is drying at 20°C, 40°C, 60°C, 80°C, and 100°C for 2 hours respectively.
7. The preparation method according to claim 5, characterized in that: The calcination treatment is as follows: heating at room temperature to 700-800° C. at 2-5° C. / min and keeping the temperature for 8-16 hours.
8. The three-dimensional ordered porous carbon / manganese oxide composite absorbing material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the three-dimensional ordered porous carbon / manganese oxide composite absorbing material as claimed in claim 8 in shielding electromagnetic radiation.
Citation Information
Cited By
SiO2 / C composite material with multistage three-dimensional network structure as well as preparation method and application of SiO2 / C composite material
CN119707516A