Flash memory structure and forming method thereof
The multi-step floating gate structure in the flash memory design addresses the need for improved erasing capability by concentrating electric fields, enhancing erasure and write speed through optimized floating gate and erase gate interaction.
Patent Information
- Application Number
- CN202310652981.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
The existing floating gate flash memory structure requires improvements in erasing capability and efficiency.
A flash memory structure is designed with a multi-step floating gate structure where each floating gate region is stacked along the substrate surface, with the side wall of one region protruding relative to the next, and each region extends into the erase gate, enhancing electric field concentration points for improved erasure efficiency.
The multi-step floating gate design increases electric field concentration, leading to enhanced erasure and write speed by improving the contact interface and electric field gathering points between the floating gate and erase gate.
Smart Images

Figure CN119072125A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a flash memory structure and a forming method thereof. Background Art
[0002] Flash memory is a non-volatile memory that can retain data for a long time even without current supply, that is, data will not be lost even when power is off. Floating gate flash memory is widely used in various embedded electronic products such as financial IC cards, automotive electronics, etc. because it helps save chip area and improve storage integration density.
[0003] The existing floating gate flash memory structure usually includes an erase gate, a control gate, and a floating gate. The control gate is located above the floating gate and is isolated by a dielectric layer. The erase gate is located between two pairs of control gates and floating gates and is a common erase gate. The two word lines are located on both sides of the two pairs of control gates and floating gates and are isolated by a dielectric layer. The oxide layer between the erase gate and the floating gate is a tunnel dielectric layer. The floating gate will extend partly under the erase gate to form an overlapping wrap frame structure (Wrap round). This unique structure can improve the ability and efficiency of erasure. The above structure has the advantages of high reliability, good manufacturing process compatibility, low startup voltage, and prevention of over-erasure.
[0004] However, the erasing capability and efficiency of the existing floating gate flash memory structure need to be further improved. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a flash memory structure and a forming method thereof, so as to improve the performance of the formed flash memory structure.
[0006] In order to solve the above technical problems, the technical solution of the present invention provides a flash memory structure, comprising: a substrate; two separate storage gate structures located on the substrate, an opening is provided between the two storage gate structures, each storage gate structure comprises a floating gate and a control gate structure located on the floating gate, the control gate structure comprises a control gate dielectric layer and a control gate located on the control gate dielectric layer, each floating gate comprises N floating gate regions stacked along the normal direction of the substrate surface, the i+1th floating gate region of the N floating gate regions is located on the surface of the i-th floating gate region, and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, wherein N is a natural number greater than or equal to 2, and i is a natural number greater than or equal to 1 and less than N; an erase gate structure located in the opening; and word line structures located on both sides of the storage gate structure and the erase gate structure, respectively.
[0007] Optionally, it further includes: a sidewall structure located at the control gate dielectric layer and the control gate sidewall; and each sidewall of the floating gate region protrudes relative to the control gate sidewall.
[0008] Optionally, a size range of a sidewall of the Nth floating gate region in the floating gate exposed by the opening protruding relative to a sidewall of the control gate is 15 nm to 60 nm.
[0009] Optionally, the angle between the top of the sidewall of each floating gate region and the sidewall surface ranges from 80 degrees to 90 degrees.
[0010] Correspondingly, the technical solution of the present invention also provides a method for forming a flash memory structure, comprising: providing a substrate; forming a floating gate material layer and a plurality of control gate structures separated from each other on the floating gate material layer on the surface of the substrate; after forming the control gate structure, etching the floating gate material layer by N steps forming processes until the floating gate material layer is penetrated to form a plurality of floating gates, each of the floating gates and the control gate structure on the floating gate forming a storage gate structure, and an opening is provided between two adjacent storage gate structures, each of the floating gates comprises N stacked along the normal direction of the substrate surface. A floating gate region, wherein the i+1th floating gate region among the N floating gate regions is located on the surface of the i-th floating gate region and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, wherein N is a natural number greater than or equal to 2, and i is a natural number greater than or equal to 1 and less than N, and the method for the i-th step formation process comprises: etching the exposed floating gate material layer to form an i-th groove in the floating gate material layer; forming an i-th protective sidewall on the side wall of the i-th groove; forming an erase gate structure in the opening; and forming a word line structure on the substrate on both sides of the storage gate structure and the erase gate structure.
[0011] Optionally, the process of etching the exposed floating gate material layer includes a dry etching process; the process parameters of the dry etching process include: the etching gas includes one or more of Cl2, HBr, He, O2, CF4, SF6, N2, the gas flow range is 6sccm to 200sccm, and the power range is 200w to 800w.
[0012] Optionally, the material of the i-th protective sidewall includes a dielectric material, and the dielectric material includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride and silicon carbon oxynitride.
[0013] Optionally, the method for forming the i-th protective sidewall includes: forming an i-th protective sidewall material layer on the surface of the control gate structure and the sidewalls and bottom surfaces of the i-th groove; and etching back the i-th protective sidewall material layer until the bottom surface of the i-th groove is exposed.
[0014] Optionally, each of the control gate structures includes a control gate dielectric layer and a control gate located on the control gate dielectric layer; the method for forming the control gate structure includes: forming a floating gate material layer, a control gate dielectric material layer located on the floating gate material layer, and a control gate material layer located on the control gate dielectric material layer on the surface of the substrate; etching the control gate material layer and the control gate dielectric material layer until the floating gate material layer is exposed, forming the control gate with the control gate material layer, and forming the control gate dielectric layer with the control gate dielectric material layer.
[0015] Optionally, the method for etching the control gate material layer and the control gate dielectric material layer also includes: forming a hard mask layer on the surface of the control gate material layer, the hard mask layer exposing a portion of the surface of the control gate material layer; and etching the control gate material layer and the control gate dielectric material layer using the hard mask layer as a mask.
[0016] Optionally, after forming the control gate structure and before etching the floating gate material layer, the method further includes: forming a sidewall structure on the control gate dielectric layer and the control gate sidewall.
[0017] Optionally, the method for forming the sidewall structure includes: forming a sidewall material layer on the surfaces of the floating gate material layer, the control gate and the control gate dielectric layer; and etching back the sidewall material layer until the surface of the floating gate material layer is exposed.
[0018] Optionally, a size range of a sidewall of the Nth floating gate region in the floating gate exposed by the opening protruding relative to a sidewall of the control gate is 15 nm to 60 nm.
[0019] Optionally, the angle between the top of the sidewall of each floating gate region and the sidewall surface ranges from 80 degrees to 90 degrees.
[0020] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:
[0021] In a method for forming a flash memory structure provided by the technical solution of the present invention, the formed floating gate includes a plurality of N floating gate regions stacked along the normal direction of the substrate surface, the i+1th floating gate region among the N floating gate regions is located on the surface of the i-th floating gate region, and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, the floating gate is designed to be a multi-step structure, each floating gate region goes deep into the erase gate, which can effectively improve the contact interface, and at the same time, each floating gate region has a corner adjacent to the erase gate, each corner is conducive to the concentration of the electric field between the floating gate and the erase gate, thereby increasing the electric field concentration points between the floating gate and the erase gate, which is conducive to improving the erasure efficiency, thereby improving the erase and write speed of the memory.
[0022] Furthermore, the process of etching the exposed floating gate material layer includes a dry etching process. By controlling the parameters of the dry etching process in each step formation process, the height of each floating gate region and the number of floating gate regions can be adjusted to make the structure of the formed floating gate more flexible.
[0023] Furthermore, the i-th protective sidewall in each step formation process is formed by back-etching the i-th protective sidewall material layer, and the thickness of the i-th protective sidewall is controlled by adjusting the thickness of the i-th protective sidewall material layer, thereby further controlling the protruding size of each floating gate region sidewall relative to the floating gate region sidewall located on its surface, so as to adjust the size of each floating gate region and make the structure of the formed floating gate more flexible.
[0024] A flash memory structure provided by the technical solution of the present invention comprises a plurality of N floating gate regions stacked along the normal direction of the substrate surface, wherein the i+1th floating gate region among the N floating gate regions is located on the surface of the i-th floating gate region, and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, and the floating gate is designed to be a multi-step structure, and each floating gate region goes deep into the erase gate, which can effectively improve the contact interface, and at the same time, each floating gate region has a corner adjacent to the erase gate, and each corner is conducive to the gathering of the electric field between the floating gate and the erase gate, thereby increasing the electric field gathering points between the floating gate and the erase gate, which is conducive to improving the erasing efficiency, thereby improving the erasing and writing speed of the memory. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figures 1 to 4 It is a structural schematic diagram of a flash memory structure formation process;
[0026] Figures 5 to 10 It is a structural schematic diagram of each step of the method for forming a flash memory structure in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] It should be noted that the terms “surface” and “on” in this specification are used to describe relative positional relationships in space and are not limited to direct contact.
[0028] As described in the background art, the erasing capability and efficiency of the existing floating gate flash memory structure need to be further improved. Now, a flash memory structure is used for explanation and analysis.
[0029] Figures 1 to 4 The present invention is a structural schematic diagram of a flash memory structure formation process.
[0030] Please refer to Figure 1, providing a substrate 101; forming a floating gate oxide material layer 102 on the substrate 101; forming a floating gate material layer 103 on the surface of the floating gate oxide material layer 102; forming a plurality of control gate structures on the surface of part of the floating gate material layer 103, each control gate structure comprising two separate control gates, the control gate comprising a dielectric layer 104, a control gate layer 105 located on the dielectric layer 104, and a hard mask layer 106 located on the control gate layer 105, in each of the control gate structures, each control gate comprises a first side wall adjacent to another control gate (not shown in the figure).
[0031] Please refer to Figure 2 , forming a first sidewall spacer 107 on each control gate sidewall; after forming the first sidewall spacer 107 , forming a second sidewall spacer 108 on the first sidewall of the control gate, the first sidewall spacer 107 is located between the first sidewall and the second sidewall spacer 108 .
[0032] Please refer to Figure 3 The floating gate material layer 103 is etched using the first spacer 107 , the second spacer 108 and the control gate as masks until the floating gate oxide material layer 102 is exposed to form a floating gate 109 .
[0033] Please refer to Figure 4 An erase gate structure is formed on the surface of the substrate 101 between adjacent control gate layers 105 in each of the control gate structures, wherein the erase gate structure includes an erase gate dielectric layer 110 and an erase gate 111 located on the surface of the erase gate dielectric layer 110; and a word line 112 is formed on the surface of the substrate 101 on both sides of the control gate structure and the erase gate structure.
[0034] In the flash memory structure formed by the above method, the charge is stored in the floating gate 109. The erasing process requires a strong electric field to be formed between the floating gate 109 and the erase gate 111 to effectively extract the electrons in the floating gate 109. The effective electric field and the electron channel are more concentrated at the corner A of the floating gate 109 (such as Figure 4 As shown in FIG. 1 , the sharper the corner A is, the stronger the electric field near it is, which is more conducive to electron extraction and improving signal erasing efficiency.
[0035] However, due to the limitation of the etching process, it is difficult to form a sharp corner during the dry etching process of forming the floating gate 109. In addition, during the device processing after forming the floating gate 109 and before forming the erase gate 111, there are usually multiple thermal oxidation processes. Under the influence of the thermal oxidation process, the corner A is also easily passivated into a rounded corner, which is not conducive to forming a high electric field here, thereby seriously affecting the erase efficiency.
[0036] In order to solve the above problems, the present invention provides a method for forming a flash memory structure, wherein the formed floating gate includes a plurality of N floating gate regions stacked along the normal direction of the substrate surface, the i+1th floating gate region among the N floating gate regions is located on the surface of the i-th floating gate region, and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, and the floating gate is designed to be a multi-step structure, each floating gate region penetrates into the erase gate, which can effectively improve the contact interface, and at the same time, each floating gate region has a corner adjacent to the erase gate, and each corner is conducive to the concentration of the electric field between the floating gate and the erase gate, thereby increasing the electric field concentration points between the floating gate and the erase gate, which is conducive to improving the erasure efficiency, thereby improving the erase and write speed of the memory.
[0037] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0038] Figures 5 to 10 It is a structural schematic diagram of each step of the method for forming a flash memory structure in an embodiment of the present invention.
[0039] Please refer to Figure 5 , providing a substrate 200.
[0040] In this embodiment, the material of the substrate 200 includes silicon. In other embodiments, the material of the substrate includes silicon carbide, silicon germanium, a multinary semiconductor material composed of III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI). Among them, the multinary semiconductor material composed of III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.
[0041] Please refer to Figure 6 A floating gate material layer 201 and a plurality of separate control gate structures located on the floating gate material layer 201 are formed on the surface of the substrate 200 .
[0042] In this embodiment, each of the control gate structures includes a control gate dielectric layer 202 and a control gate 203 located on the control gate dielectric layer 202 .
[0043] In this embodiment, the method for forming the control gate structure includes: forming a floating gate material layer (not shown in the figure), a control gate dielectric material layer (not shown in the figure) located on the floating gate material layer, and a control gate material layer (not shown in the figure) located on the control gate dielectric material layer on the surface of the substrate 200; etching the control gate material layer and the control gate dielectric material layer until the floating gate material layer 201 is exposed, forming the control gate 203 with the control gate material layer, and forming the control gate dielectric layer 202 with the control gate dielectric material layer.
[0044] In this embodiment, the method for etching the control gate material layer and the control gate dielectric material layer also includes: forming a hard mask layer 204 on the surface of the control gate material layer, the hard mask layer 204 exposing a portion of the surface of the control gate material layer; and etching the control gate material layer and the control gate dielectric material layer using the hard mask layer 204 as a mask.
[0045] In this embodiment, after the control gate structure is formed and before the floating gate material layer is etched, a spacer structure 205 is formed on the sidewalls of the control gate dielectric layer 202 and the control gate 203 .
[0046] In this embodiment, the sidewall structure 205 is a double-layer material layer of silicon oxide and silicon nitride. In other embodiments, the sidewall structure can also be a single-layer or multi-layer material layer.
[0047] In this embodiment, the method for forming the sidewall structure 205 includes: forming a sidewall material layer (not shown in the figure) on the surface of the floating gate material layer, the control gate 203 and the control gate dielectric layer 202; and etching back the sidewall material layer until the surface of the floating gate material layer is exposed.
[0048] In this embodiment, before forming the floating gate material layer 201 , an oxide material layer 206 is formed on the surface of the substrate 200 .
[0049] Subsequently, after forming the control gate structure, the floating gate material layer 201 is etched through the floating gate material layer 201 by N steps forming processes to form a plurality of floating gates, each of which constitutes a storage gate structure with the control gate structure on the floating gate, and there is an opening between two adjacent storage gate structures, each of which comprises N floating gate regions stacked along the normal direction of the substrate surface, the i+1th floating gate region of the N floating gate regions being located on the surface of the i-th floating gate region and the sidewall of the i-th floating gate region protruding relative to the sidewall of the i+1th floating gate region, wherein N is a natural number greater than or equal to 2, and i is a natural number greater than or equal to 1 and less than N. For the method of the i-th step forming process, please refer to Figures 7 and 8 .
[0050] Please refer to Figure 7 , etching the exposed floating gate material layer 201 to form an i-th groove 207 in the floating gate material layer 201.
[0051] In this embodiment, the process of etching the exposed floating gate material layer 201 includes a dry etching process.
[0052] In this embodiment, the process parameters of the dry etching process include: the etching gas includes one or more of Cl2, HBr, He, O2, CF4, SF6, and N2, the gas flow range is 6sccm to 200sccm, and the power range is 200w to 800w.
[0053] By controlling the parameters of the dry etching process in each step formation process, the height of each floating gate region and the number of floating gate regions can be adjusted to make the structure of the formed floating gate more flexible.
[0054] Please refer to Figure 8 , an i-th protective sidewall 208 is formed on the sidewall of the i-th groove 207 .
[0055] In this embodiment, the method for forming the i-th protective side wall 208 includes: forming an i-th protective side wall material layer (not shown in the figure) on the surface of the control gate structure and the side walls and bottom surface of the i-th groove 207; and etching back the i-th protective side wall material layer until the bottom surface of the i-th groove 207 is exposed.
[0056] The i-th protective sidewall 208 in each step formation process is formed by back-etching the i-th protective sidewall material layer. The thickness of the i-th protective sidewall material layer is adjusted to control the thickness of the i-th protective sidewall, and the protruding size of each floating gate region sidewall relative to the floating gate region sidewall located on its surface is further controlled to adjust the size of each floating gate region, so as to make the structure of the formed floating gate more flexible.
[0057] In this embodiment, the material of the i-th protective spacer 208 includes a dielectric material, and the dielectric material includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride and silicon carbon oxynitride.
[0058] Repeat multiple times Figure 7 and Figure 8 until the oxide material layer 206 is exposed, thereby obtaining a plurality of floating gate regions.
[0059] In this embodiment, each of the floating gates 209 includes three floating gate regions stacked along the normal direction of the surface of the substrate 200, each of the floating gates 209 and the control gate structure on the floating gate 209 form a storage gate structure, and there is an opening 210 between two adjacent storage gate structures. In other embodiments, each of the floating gates may include two floating gate regions stacked along the normal direction of the substrate surface or more than two floating gate regions.
[0060] The floating gate 209 is designed to have a multi-step structure, and each floating gate region extends deep into the erase gate, which can effectively improve the contact interface. At the same time, each floating gate region has a corner adjacent to the erase gate, and each corner is conducive to the gathering of the electric field between the floating gate and the erase gate, thereby increasing the electric field gathering points between the floating gate and the erase gate, which is beneficial to improving the erasure efficiency, thereby improving the erase and write speed of the memory.
[0061] In this embodiment, the sidewall of the Nth floating gate region in the floating gate exposed by the opening 210 protrudes relative to the sidewall of the control gate 203 by a dimension d ranging from 15 nm to 60 nm.
[0062] In this embodiment, the angle between the top of the sidewall of each floating gate region and the sidewall surface ranges from 80 degrees to 90 degrees.
[0063] Please refer to Fig.10 , forming an erase gate structure in the opening 210 ; and forming a word line structure on the substrate 200 on both sides of the storage gate structure and the erase gate structure.
[0064] In this embodiment, the erase gate structure includes a tunnel oxide layer 211 and an erase gate 212 located on the surface of the tunnel oxide layer 211 .
[0065] In this embodiment, the word line structure includes a word line oxide layer 213 and a word line 214 located on the surface of the word line oxide layer 213 .
[0066] In this embodiment, the method for forming the erase gate structure and the word line structure includes: after forming the floating gate 209, forming an oxide material layer (not shown in the figure) on the surface of the substrate 200 and the storage gate structure; forming a gate material layer (not shown in the figure) on the surface of the oxide material layer, and the surface of the gate material layer is higher than the top surface of the storage gate structure; planarizing the gate material layer and the oxide material layer until the top surface of the storage gate structure is exposed, forming the tunneling oxide layer 211 and the word line oxide layer 213 with the oxide material layer, and forming the erase gate 212 and the word line 214 with the gate material layer.
[0067] Accordingly, the embodiment of the present invention also provides a flash memory structure formed by the above method, please continue to refer to Fig.10 , comprising: a substrate 200; two separate storage gate structures located on the substrate 200, with an opening 210 (such as Fig. 9As shown), each storage gate structure includes a floating gate 209 and a control gate structure located on the floating gate 209, the control gate structure includes a control gate dielectric layer 202 and a control gate 203 located on the control gate dielectric layer 202, each floating gate 209 includes N floating gate regions stacked along the normal direction of the surface of the substrate 200, the i+1th floating gate region among the N floating gate regions is located on the surface of the i-th floating gate region, and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, wherein N is a natural number greater than or equal to 2, and i is a natural number greater than or equal to 1 and less than N; an erase gate structure located in the opening 210; and word line structures located on both sides of the storage gate structure and the erase gate structure, respectively.
[0068] The floating gate 209 is designed to have a multi-step structure, and each floating gate region extends deep into the erase gate, which can effectively improve the contact interface. At the same time, each floating gate region has a corner adjacent to the erase gate, and each corner is conducive to the gathering of the electric field between the floating gate and the erase gate, thereby increasing the electric field gathering points between the floating gate and the erase gate, which is beneficial to improving the erasure efficiency, thereby improving the erase and write speed of the memory.
[0069] In this embodiment, the erase gate structure includes a tunnel oxide layer 211 and an erase gate 212 located on the surface of the tunnel oxide layer 211 .
[0070] In this embodiment, the word line structure includes a word line oxide layer 213 and a word line 214 located on the surface of the word line oxide layer 213 .
[0071] In this embodiment, the flash memory structure further includes: a sidewall structure 205 located on the sidewalls of the control gate dielectric layer 202 and the control gate 203 ; and each sidewall of the floating gate region protrudes relative to the sidewall of the control gate 203 .
[0072] In this embodiment, the sidewall of the Nth floating gate region in the floating gate 209 exposed by the opening 210 protrudes relative to the sidewall of the control gate 203 by a dimension d ranging from 15 nm to 60 nm.
[0073] In this embodiment, the angle between the top of the sidewall of each floating gate region and the sidewall surface ranges from 80 degrees to 90 degrees.
[0074] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A flash memory structure, characterized in that: include: substrate; Two separate storage gate structures located on the substrate, with an opening between the two storage gate structures, each storage gate structure comprising a floating gate and a control gate structure located on the floating gate, the control gate structure comprising a control gate dielectric layer and a control gate located on the control gate dielectric layer, each floating gate comprising N floating gate regions stacked along a normal direction of the substrate surface, an i+1th floating gate region among the N floating gate regions being located on a surface of an i-th floating gate region, and a sidewall of the i-th floating gate region protruding relative to a sidewall of the i+1th floating gate region, wherein N is a natural number greater than or equal to 2, and i is a natural number greater than or equal to 1 and less than N; an erase gate structure located in the opening; Word line structures are respectively located on both sides of the storage gate structure and the erase gate structure.
2. The flash memory structure according to claim 1, wherein: Also includes: A sidewall structure located at the control gate dielectric layer and the sidewall of the control gate; The sidewalls of each floating gate region protrude relative to the sidewalls of the control gate.
3. The flash memory structure according to claim 2, characterized in that: The sidewall of the Nth floating gate region in the floating gate exposed by the opening protrudes relative to the sidewall of the control gate in a size ranging from 15 nm to 60 nm.
4. The flash memory structure according to claim 1, wherein: The included angle between the top of the sidewall of each floating gate region and the sidewall surface is in the range of 80 degrees to 90 degrees.
5. A method for forming a flash memory structure, characterized in that: include: providing a substrate; Forming a floating gate material layer and a plurality of control gate structures separated from each other on the floating gate material layer on the surface of the substrate; After forming the control gate structure, the floating gate material layer is etched through the floating gate material layer by N steps forming processes to form a plurality of floating gates, each of the floating gates and the control gate structure on the floating gate constitutes a storage gate structure, and an opening is provided between two adjacent storage gate structures, each of the floating gates comprises N floating gate regions stacked along the normal direction of the substrate surface, the i+1th floating gate region of the N floating gate regions is located on the surface of the i-th floating gate region and the side wall of the i-th floating gate region protrudes relative to the side wall of the i+1th floating gate region, wherein N is a natural number greater than or equal to 2, i is a natural number greater than or equal to 1 and less than N, and the method for the i-th step forming process comprises: Etching the exposed floating gate material layer to form an i-th groove in the floating gate material layer; forming an i-th protective sidewall on the sidewall of the i-th groove; forming an erase gate structure in the opening; A word line structure is formed on the substrate at both sides of the storage gate structure and the erase gate structure.
6. The method for forming a flash memory structure according to claim 5, wherein: The process of etching the exposed floating gate material layer includes a dry etching process; the process parameters of the dry etching process include: the etching gas includes one or more of Cl2, HBr, He, O2, CF4, SF6, N2, the gas flow range is 6sccm to 200sccm, and the power range is 200w to 800w.
7. The method for forming a flash memory structure according to claim 5, wherein: The material of the i-th protective sidewall includes a dielectric material, and the dielectric material includes one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride and silicon carbon oxynitride.
8. The method for forming a flash memory structure according to claim 5, wherein: The method for forming the i-th protective sidewall comprises: forming an i-th protective sidewall material layer on the surface of the control gate structure and the sidewall and bottom surface of the i-th groove; and etching back the i-th protective sidewall material layer until the bottom surface of the i-th groove is exposed.
9. The method for forming a flash memory structure according to claim 5, wherein: Each of the control gate structures comprises a control gate dielectric layer and a control gate located on the control gate dielectric layer; The method for forming the control gate structure comprises: forming a floating gate material layer, a control gate dielectric material layer located on the floating gate material layer, and a control gate material layer located on the control gate dielectric material layer on the substrate surface; The control gate material layer and the control gate dielectric material layer are etched until the floating gate material layer is exposed, the control gate is formed with the control gate material layer, and the control gate dielectric layer is formed with the control gate dielectric material layer.
10. The method for forming a flash memory structure according to claim 9, wherein: The method for etching the control gate material layer and the control gate dielectric material layer also includes: forming a hard mask layer on the surface of the control gate material layer, the hard mask layer exposing a portion of the surface of the control gate material layer; and etching the control gate material layer and the control gate dielectric material layer using the hard mask layer as a mask.
11. The method for forming a flash memory structure according to claim 9, wherein: After forming the control gate structure and before etching the floating gate material layer, the method further includes: forming a sidewall structure on the control gate dielectric layer and the control gate sidewall.
12. The method for forming a flash memory structure according to claim 11, wherein: The method for forming the spacer structure comprises: forming a spacer material layer on the surfaces of the floating gate material layer, the control gate and the control gate dielectric layer; and etching back the spacer material layer until the surface of the floating gate material layer is exposed.
13. The method for forming a flash memory structure according to claim 5, wherein: The sidewall of the Nth floating gate region in the floating gate exposed by the opening protrudes relative to the sidewall of the control gate in a size ranging from 15 nm to 60 nm.
14. The method for forming a flash memory structure according to claim 5, wherein: The included angle between the top of the sidewall of each floating gate region and the sidewall surface is in the range of 80 degrees to 90 degrees.
Citation Information
Cited By
Floating gate type flash memory structure, forming method and electronic equipment
CN121284966A