Interface double-end passivated top incidence quantum dot device and preparation method thereof

The top-incident quantum dot device with double-end passivation addresses surface defects by using a silicon-oxygen or aluminum-oxygen structure interface layer, enhancing bonding and reducing dark current, thereby improving thermal stability and performance.

CN119072140APending Publication Date: 2024-12-03HUAZHONG UNIV OF SCI & TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311845469.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Conventional photodetectors using quantum dots face challenges with surface defects and poor passivation, leading to high ohmic leakage currents and reduced thermal stability due to weak bonding and damage from oxide electron transport layers, which affect device performance.

Method used

A top-incident quantum dot device with double-end passivation using a silicon-oxygen or aluminum-oxygen structure interface passivation layer, enhancing bonding strength and passivation through chemical bonds, reducing dark current and improving thermal stability.

Benefits of technology

The double-end passivation layer significantly reduces dark current and enhances thermal stability, achieving improved device performance comparable to existing quantum dot photodiodes and transistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072140A_ABST
    Figure CN119072140A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of top incidence quantum dot devices, in particular to an interface double-end passivated top incidence quantum dot device and a preparation method thereof.The interface double-end passivated top incidence quantum dot device comprises a bottom electrode, a hole transport layer, a PbS quantum dot light absorption layer, an interface passivation layer, an electron transport layer and a top electrode which are sequentially arranged; the interface passivation layer comprises a PbS quantum dot with a silicon-oxygen structure or an aluminum-oxygen structure at one end of a ligand. The method has the effects of improving the binding force between the films, reducing the overall dark current of the device and improving the thermal stability of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of top-incident quantum dot devices, and in particular to a top-incident quantum dot device with double-end passivation of the interface and a preparation method thereof. Background Art

[0002] A photodetector is a device that can capture light signals in a specific wavelength range and convert them immediately into electrical signals. Photodetectors have important and widespread applications in optical imaging, optical communications, automatic control, biochemical sensing, and other fields. Therefore, it is of great significance to develop photodetectors with superior performance. At present, photodetectors based on semiconductor materials such as silicon, germanium, indium, gallium arsenide, and gallium nitride are widely used in commercial products to cover different spectral ranges due to their different band gaps.

[0003] Compared with the materials of conventional photodetectors on the market, colloidal quantum dots have cheap raw materials, simple processes, and good photoelectric properties, such as adjustable bandgap width and adjustable infrared absorption, which provide a basis for the rapid application and development of colloidal quantum dot materials in the field of optoelectronics. However, as the size of quantum dots increases, the polarity of the (100) plane increases, and the passivation difficulty of the quantum dot surface increases. After film formation, there are many nano-scale cracks and holes on its surface. In particular, when the quantum dot detector is working under reverse bias, these surface defects will cause a large ohmic leakage current, affecting the performance of the device. At the same time, when making an oxide electron transport layer on the quantum dot light absorption layer, according to existing methods, such as magnetron sputtering, atomic layer deposition (ALD), etc., certain damage will be caused to the surface of the quantum dot layer to provide more defect recombination sites, affecting carrier transport.

[0004] In the relevant documents, C is introduced to reduce damage 60 Interface layer, C 60 The interface layer has poor mechanical properties, weak bonding between films, and cannot effectively passivate the surface of quantum dots. Summary of the invention

[0005] In order to improve the bonding strength between thin films and enhance the passivation effect of surface defects of quantum dots, the purpose of the present application is to provide a top-incident quantum dot device with double-end passivation of the interface and a preparation method thereof.

[0006] In the first aspect, the top-incident quantum dot device with double-end passivation of the interface provided in the present application adopts the following technical solution:

[0007] A top-incident quantum dot device with double-end passivation of the interface, comprising:

[0008] The bottom electrode, hole transport layer, PbS quantum dot light absorption layer, electron transport layer and top electrode are arranged in sequence, characterized in that it also includes an interface passivation layer arranged between the PbS quantum dot light absorption layer and the electron transport layer, and the interface passivation layer includes PbS quantum dots with a silicon-oxygen structure or an aluminum-oxygen structure at one end of the ligand.

[0009] By adopting the above technical scheme, based on the existing top-incident quantum dot detector device structure, PbS quantum dots including a silicon-oxygen structure or an aluminum-oxygen structure at one end of the ligand are introduced between the PbS quantum dot light-absorbing layer and the electron transport layer as an interface passivation layer. The interface passivation layer is in homogeneous contact with the lower PbS quantum dot light-absorbing layer, thereby optimizing the interface contact effect. The silicon-oxygen structure or the aluminum-oxygen structure between the upper electron transport layer is coordinated and connected through chemical bonds, thereby achieving a passivation effect. The inter-membrane bonding force is greatly increased, and the double-end passivation of the active layer (PbS quantum dot light-absorbing layer)-electron transport layer is comprehensively realized, thereby reducing the overall dark current of the device and improving the thermal stability of the device.

[0010] Optionally, the silicon-oxygen structure is shown in formula (I): (I);

[0011] Or the aluminum oxide structure is shown in the following formula (II): (Ⅱ);

[0012] Wherein, R1 is methoxy or ethoxy, and R2 is methyl or R1.

[0013] By adopting the above technical solution, the silicon oxide structure or aluminum oxide structure is specifically defined, and a cross-linked siloxane or aluminum oxide protective layer relative to the electron transport layer is formed through the methoxy or ethoxy groups thereon, thereby achieving a coordination connection between chemical bonds to achieve a passivation effect.

[0014] Optionally, the thickness of the interface passivation layer is 4.5-12 nm.

[0015] By adopting the above technical solution, the thickness of the interface passivation layer is limited to meet the passivation requirements, improve the bonding strength between the films, reduce the overall dark current of the device, improve the thermal stability of the device, and reduce the impact of the addition of the interface passivation layer on the device structure and performance.

[0016] Optionally, the thickness of the interface passivation layer is 8.5-9.5 nm.

[0017] By adopting the above technical solution, the thickness of the interface passivation layer is limited, the bonding strength between the films is further improved, the overall dark current of the device is reduced, and the thermal stability of the device is improved.

[0018] In the second aspect, the preparation method of the top-incident quantum dot device with double-end passivation of the interface provided in the present application adopts the following technical solution:

[0019] The preparation method of the top-incident quantum dot device with double-end interface passivation comprises sequentially preparing a bottom electrode, a hole transport layer, a PbS quantum dot light absorption layer, an interface passivation layer, an electron transport layer and a top electrode, wherein the preparation of the interface passivation layer is specifically as follows:

[0020] S1, preparing a PbS quantum dot ink layer on the PbS quantum dot light absorbing layer;

[0021] S2, drop the double-terminal ligand solution on the surface of the PbS quantum dot ink layer, let it stand and then spin away the double-terminal ligand solution on the surface, wash it, and obtain an interface passivation layer, wherein the double-terminal ligand is X-(CH 2 ) 2-3 -A compound, wherein X is -HS, -NH 2 , -Br, -I or -Cl; A is a silicon-oxygen structure or an aluminum-oxygen structure.

[0022] By adopting the above technical solution, first, one end of the double-terminal ligand is HS - NH 2 - Br - ,I - , Cl - The functional group can passivate the lead vacancies exposed on the surface of the quantum dots, cooperate with the PbS quantum dot ink to form a stable connection, and at the same time, make homogeneous contact with the lower PbS quantum dot light-absorbing layer to optimize the interface contact effect; the other end is connected to the methoxy or ethoxy group through silicon or aluminum oxide to form a cross-linked siloxane or aluminoxane protective layer relative to the electron transport layer, and further connect to the upper electron transport layer through chemical bonds, which has a passivation effect and greatly increases the inter-film bonding force; secondly, it improves the deposition quality of the electron transport layer on the interface passivation layer, realizes the double-end passivation between the PbS quantum dot light-absorbing layer and the electron transport layer, enhances the bonding force between the thin films, realizes the reduction of the overall dark current of the device, and improves the thermal stability of the device.

[0023] Optionally, the concentration of the PbS quantum dot ink is 10-40 mg / ml.

[0024] By adopting the above technical solution, the concentration of PbS quantum dot ink is limited to 10-40 mg / ml, avoiding the problem of too thick interface passivation layer due to too high concentration and too thin interface passivation layer due to too low concentration, both of which affect device performance.

[0025] Optionally, the volume fraction of the double-terminal ligand solution is 0.5-15%.

[0026] By adopting the above technical solution, on the basis of limiting the concentration of PbS quantum dot ink, the volume fraction of the double-terminal ligand solution is further limited, the exchange effect is improved, the optimal exchange degree is determined, and the device performance is improved.

[0027] Optionally, the step further includes S3, repeating the steps S1-S2 1-2 times.

[0028] By adopting the above technical solution, multiple spin coatings can be performed to reduce the problem of uneven coating that exists in a single coating.

[0029] Optionally, the concentration of the PbS quantum dot ink is 18-22 mg / ml, the volume fraction of the double-terminal ligand solution is 0.8-1.2%, and the S1-S2 operations are repeated once.

[0030] By adopting the above technical solution, the concentration of PbS quantum dot ink is limited to 18-22 mg / ml, the volume fraction of the double-terminal ligand solution is 0.8-1.2%, and the double coating is further limited to improve the coating effect. Compared with single coating, the existing spin coating unevenness problem is reduced; compared with three coatings, the number of coating times is reduced and the coating uniformity is improved.

[0031] Optionally, the step S2 is left to stand for 18-22 seconds.

[0032] By adopting the above technical solution, a better exchange effect can be achieved.

[0033] In summary, the present application includes at least one of the following beneficial technical effects:

[0034] 1. Based on the existing top-incident quantum dot detector device structure, a double-end passivation interface passivation layer is introduced between the PbS quantum dot light-absorbing layer and the electron transport layer. The interface passivation layer includes a PbS quantum dot with a silicon-oxygen structure or an aluminum-oxygen structure at one end of the ligand, so as to achieve double-end passivation of the active layer (PbS quantum dot light-absorbing layer)-electron transport layer, improve the inter-film bonding force and device performance, and reduce the overall dark current of the device, thereby improving the thermal stability of the device. Specifically, the dark current of the device is reduced from the original 60nA / cm 2 @-0.01V down to 28nA / cm 2 @-0.01V, 700nA / cm 2 @-0.5V down to 270nA / cm 2 @-0.5V;

[0035] The above effects are equivalent to those of existing quantum dot photodiode QDPD structures, transistors, and batteries. 60The interface layer mainly relies on intermolecular forces to combine with the quantum dot light-absorbing layer. The bonding force between the thin films is poor and the application scenarios are small. In this method, the interface passivation layer and the lower PbS quantum dot light-absorbing layer are in homogeneous contact, which optimizes the interface contact effect. The interface passivation layer and the upper electron transport layer are connected by chemical bonds, which greatly increases the bonding force between the films and increases the passivation effect.

[0036] 2. One end of the double-terminal ligand is HS - NH 2 - Br - ,I - , Cl - The functional group can passivate the lead vacancies exposed on the surface of the quantum dots. The other end is mainly composed of a silicon-oxygen bond or an aluminum-oxygen bond, which is connected to a methoxy group or an ethoxy group to form a cross-linked siloxane or aluminum-oxane protective layer relative to the electron transport layer, thereby improving the deposition quality of the electron transport layer on the interface passivation layer and realizing double-end passivation between the PbS quantum dot light absorption layer and the electron transport layer.

[0037] 3. In the process of preparing the interface passivation layer, the complicated vacuum thermal evaporation process is avoided (C 60 The method uses a vapor deposition process to rapidly form a film through solid phase exchange, which has low cost and simple steps. Furthermore, the film thickness is reduced, and the impact on the device is reduced while achieving double-end passivation. Furthermore, during the preparation process, the interface passivation layer is obtained by spin coating twice by adjusting the concentration of the quantum dot ink and coordinating the concentration of the double-end ligands, which has a better film-forming effect than single film formation and triple film formation. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a schematic diagram of the structure of the top-incident quantum dot device with double-end passivation of the interface of the present application;

[0039] Figure 2 This is a film-substrate bonding strength test diagram at the interface of the corresponding products of Example 1 and Comparative Example 2 of the present application;

[0040] Figure 3 This is an optical contact angle test diagram of the products corresponding to Example 1 and Comparative Example 2 of the present application;

[0041] Figure 4 This is a wide spectrum spectrum test chart of the corresponding products of Example 1 and Comparative Example 2 of the present application;

[0042] Figure 5 It is the IV curve related to the effect of thickness control on device performance in this application;

[0043] Figure 6 It is the IV curve related to the effect of MDMS ligand concentration on device performance in this application;

[0044] Figure 7 It is the IV curve related to the effect of the PbS quantum dot ink of the present application on the device performance;

[0045] Figure 8 is the IV curve of the device prepared in Example 9 of the present application;

[0046] Fig. 9 This is the IV curve related to the effect of the number of spin coating times of the PbS quantum dot ink on the device performance of the present application;

[0047] Fig.10 This is a graph showing the change in dark current of the device prepared in Comparative Example 2 of the present application under aging conditions of 85°C;

[0048] Fig.11 This is a graph showing the change in dark current of the device prepared in Example 1 of the present application under aging conditions of 85° C.;

[0049] Fig.12 This is a photocurrent variation diagram of the device prepared in Comparative Example 2 of the present application under aging conditions of 85°C;

[0050] Fig.13 This is a graph showing the photocurrent variation of the device prepared in Example 1 of the present application under aging conditions of 85°C. DETAILED DESCRIPTION

[0051] As the size of quantum dots increases, the polarity of the (100) plane increases, and the passivation difficulty of the quantum dot surface increases. After film formation, there are many nano-scale cracks and holes on the surface. Furthermore, when the quantum dot detector works under reverse bias, these surface defects will cause a large ohmic leakage current, affecting the device performance. At the same time, when making an oxide electron transport layer on the quantum dot light absorption layer, according to existing methods, such as magnetron sputtering, atomic layer deposition (ALD), etc., some damage will be caused to the surface of the quantum dot layer to provide more defect recombination sites, affecting carrier transport. In order to reduce the damage to the C introduced in the related technology 60 interface layer, but the applicant found that C 60 The mechanical properties are poor and the bonding force with the quantum dot film is weak, which makes it impossible to effectively passivate the defects on the surface of the quantum dots, and thus fail to reduce the overall dark current of the device and improve the thermal stability of the device.

[0052] The embodiment of the present application provides a top-incident quantum dot device with double-end interface passivation, comprising a bottom electrode, a hole transport layer, a PbS quantum dot light absorption layer, an interface passivation layer, an electron transport layer and a top electrode arranged in sequence, wherein: the interface passivation layer comprises a PbS quantum dot with a silicon-oxygen structure or an aluminum-oxygen structure at one end of the ligand. During the test, in order to determine whether it belongs to the interface passivation layer, it can be first determined whether it has the exciton absorption peak of the PbS quantum dot to determine whether it belongs to the quantum dot; secondly, a series of characterizations such as spectroscopy are used to determine whether it has a silicon-oxygen bond or an aluminum-oxygen bond. If so, it is determined that it includes a PbS quantum dot with a silicon-oxygen structure or an aluminum-oxygen structure at one end of the ligand.

[0053] In certain embodiments, the silicon-oxygen structure is as shown in formula (I): (I);

[0054] Or the aluminum oxide structure is shown in the following formula (II): (Ⅱ);

[0055] Wherein, R1 is methoxy or ethoxy, and R2 is methyl or R1.

[0056] In some embodiments, the thickness of the interface passivation layer is 4.5-12 nm, and more preferably, the thickness of the interface passivation layer is 8.5-9.5 nm.

[0057] The present application also provides a method for preparing a top-incident quantum dot device with double-end passivation of the interface, referring to Figure 1 , including the following steps:

[0058] A1. Making a bottom electrode. Specifically, making a bottom electrode on a substrate. The bottom electrode may be a gold (Au) electrode.

[0059] A2. A hole transport layer is prepared on the bottom electrode. The methods that can be used include magnetron sputtering and sol-gel method. Further, the magnetron sputtering method can refer to Stallone's report: Stallone. Device physics research of colloidal quantum dot short-wave infrared detectors [D]. Huazhong University of Science and Technology, 2021; the sol-gel method can refer to Wang Min's report: Wang Min. Preparation of NiO / SiC junction by sol-gel method and study of its photoelectric properties [D]. Xi'an University of Technology, 2020; the hole transport layer can specifically include at least one of NiOx, CuO, PEDOT, and TAPC;

[0060] A3. Prepare the PbS quantum dot light absorption layer, which can be specifically:

[0061] Take appropriate amounts of lead iodide and lead bromide and dissolve them in DMF (N,N-dimethylformamide) to obtain a first solution;

[0062] dissolving the quantum dot powder coated with oleic acid in an n-octane solution to obtain a second solution;

[0063] After filtering the first solution and the second solution respectively, the second solution was slowly injected into the first solution and shaken vigorously for 40 seconds to allow for full exchange. The quantum dots were transferred from the upper n-octane phase to the lower DMF phase. The short-chain iodine and bromine ligands replaced the original long-chain oleic acid ligands on the surface of the quantum dots, and iodine- and bromine-coated quantum dots were obtained.

[0064] Wash the iodine- and bromine-coated quantum dots at least twice with n-octane solution;

[0065] The quantum dots are precipitated by centrifugation, and the precipitated quantum dots are placed in a vacuum chamber for vacuum drying to obtain dry iodine- and bromine-coated quantum dot powders.

[0066] The iodine- and bromine-coated quantum dot powders were dissolved in a pre-prepared dispersant to obtain a quantum dot slurry of a certain concentration. The slurry was centrifuged, and the supernatant was dropped on the hole transport layer, and the film was formed by spin coating at 2500 rpm, and then annealed at 90°C for 10-15 minutes.

[0067] A4. Make an interface passivation layer, specifically:

[0068] S1. Preparing a PbS quantum dot ink layer on the PbS quantum dot light absorbing layer, specifically:

[0069] PbS quantum dot ink is obtained by dissolving oleic acid-coated quantum dot powder in n-octane solution;

[0070] Dropping PbS quantum dot ink on the PbS quantum dot light absorbing layer and performing spin coating to form a film; wherein, in another technical solution, the concentration of the PbS quantum dot ink can be 10-40 mg / ml;

[0071] S2:

[0072] S21, dropping the double-terminal ligand solution on the surface of the PbS quantum dot ink layer, specifically:

[0073] S211, double-terminal ligand is X-(CH 2 ) 2-3 -A compound, wherein A is a silicon-oxygen structure or an aluminum-oxygen structure. For example, when n=2 and A is a silicon-oxygen structure, the double-terminal ligand can be the following structure:

[0074]

[0075] When n=2, and A is an aluminum oxide structure, the double-terminal ligand can be the following structure:

[0076] Furthermore, X is -HS, -NH 2 , -Br, -I or -Cl, wherein X-(CH2 ) 3 -A, A is a silicon-oxygen structure, and R1 and R2 are both ethoxy groups, for example:

[0077]

[0078]

[0079] That is, the double-terminal ligand has a silicon-oxygen bond or an aluminum-oxygen bond as the main structure, and a methoxy group or an ethoxy group may be attached thereto to form a cross-linked siloxane or aluminum-oxane protective layer relative to the electron transport layer, and X may be HS - NH 2 - Br - ,I - , Cl - Functional groups are used to passivate the surface of quantum dots. The functional groups at one end of the above-mentioned molecules can passivate the lead vacancies exposed on the surface of quantum dots, and the functional groups at the other end can reduce the corrosion of water and oxygen on the underlying quantum dots, while improving the deposition quality of the electron transport layer on the interface layer, thus achieving double-end passivation between the active layer (PbS quantum dot light absorbing layer) and the electron transport layer.

[0080] S212, dissolving the double-terminal ligand in an acetonitrile solution to obtain a double-terminal ligand solution, wherein in another technical solution, the volume fraction of the double-terminal ligand solution is 0.5-15%, and more preferably, the volume fraction of the double-terminal ligand solution is 0.8-2%;

[0081] S213, dropping a double-terminal ligand solution on the surface of the PbS quantum dot ink layer;

[0082] S22, standing still to allow the double-terminal molecules to fully exchange the oleic acid ligands on the surface of the PbS quantum dot ink, and then spinning away the surface double-terminal ligand solution, and finally spin-coating with an orthogonal solution (acetonitrile) at least twice to clean the MDMS solution remaining on the surface to obtain an interface passivation layer, wherein the standing time is usually 18-30s;

[0083] A5. Prepare the electron transport layer. The applicable preparation methods include magnetron sputtering, atomic layer deposition, and sol-gel method. For details, the magnetron sputtering and atomic layer deposition methods can be referred to Zhang Linxiang's report: Zhang Linxiang. PbS quantum dot short-wave infrared detector: SnO 2 Research on electron transport layer and device performance optimization [D]. Huazhong University of Science and Technology, 2023; The sol-gel method can refer to Zhang Shuai's report: Zhang Shuai. Preparation of water-alcohol soluble tin oxide and its application in new solar cells [D]. Beijing University of Chemical Technology, 2022; The hole transport layer can specifically include ZnO, SnO 2 、TiO 2 At least one of the following;

[0084] A6. Make the top electrode, which is a transparent conductive electrode. The top electrode can be prepared by magnetron sputtering. For details, please refer to Stallone’s report: Stallone. Device physics research on colloidal quantum dot short-wave infrared detectors [D]. Huazhong University of Science and Technology, 2021.

[0085] In some embodiments, the step further includes S3, repeating the operations S1-S2 1-2 times.

[0086] In some embodiments, the concentration of the PbS quantum dot ink is 18-22 mg / ml, the volume fraction of the double-terminal ligand solution is 0.8-1.2%, and the S1-S2 operations are repeated twice.

[0087] In some embodiments, a buffer layer PbS-EDT is fabricated on the hole transport layer, and the PbS quantum dot light absorption layer is fabricated on the buffer layer PbS-EDT. The buffer layer PbS-EDT may be fabricated as follows:

[0088] Prepare 1,2-ethanedithiol (EDT) in acetonitrile solution;

[0089] The oleic acid-coated quantum dot powder is dissolved in an n-octane solution to prepare an n-octane solution of PbS quantum dots;

[0090] Take an appropriate amount of n-octane solution of PbS quantum dots and drop it on the hole transport layer film, spin coat it at a certain speed, then take a certain amount of 1,2-ethanedithiol (EDT) acetonitrile solution and soak it for 30s, spin coat it at the same speed, and finally wash it with anhydrous acetonitrile at least twice.

[0091] The present application is further described in detail below in conjunction with embodiments.

[0092] Embodiment 1:

[0093] A method for preparing a top-incident quantum dot device with double-end passivation of the interface comprises the following steps:

[0094] A1. Make bottom electrode;

[0095] A2. A hole transport layer is formed on the bottom electrode, and a buffer layer PbS-EDT is formed on the hole transport layer;

[0096] A3, making a PbS quantum dot light absorbing layer;

[0097] A4. Make an interface passivation layer, specifically:

[0098] S1. Preparing a PbS quantum dot ink layer on the PbS quantum dot light absorbing layer, wherein the concentration of the PbS quantum dot ink may be 20 mg / ml;

[0099] S2: The double-terminal ligand is 3-mercaptopropyl(dimethoxy)methylsilane (3-Mercaptopropyl(dimethoxy)methylsilane), denoted as MDMS, and its structure is shown in the following formula:

[0100]

[0101] Dissolving the double-terminal ligand in an acetonitrile solution to obtain a double-terminal ligand solution, wherein the volume fraction of the double-terminal ligand solution is 1%;

[0102] Dropping the double-terminal ligand solution on the surface of the PbS quantum dot ink layer;

[0103] After standing for 20 seconds to allow the double-terminal molecules to fully exchange the oleic acid ligands on the surface of the PbS quantum dot ink, the double-terminal ligand solution on the surface was removed by spin coating, and finally the orthogonal solution (acetonitrile) was used for two more spin coatings to clean the MDMS solution remaining on the surface to obtain an interface passivation layer;

[0104] S3, repeat S1-S2 once;

[0105] A5. Making electron transport layer;

[0106] A6. Make the top electrode.

[0107] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0108] Example 2

[0109] A method for preparing a top-incident quantum dot device with double-end passivation on the interface is the same as that in Example 1, except that the volume fraction of the double-end ligand solution is 5%.

[0110] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0111] Example 3

[0112] A method for preparing a top-incident quantum dot device with double-end passivation on the interface is the same as that in Example 1, except that the volume fraction of the double-end ligand solution is 10%.

[0113] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0114] Example 4

[0115] A method for preparing a top-incident quantum dot device with double-end passivation on the interface is the same as that in Example 1, except that the volume fraction of the double-end ligand solution is 15%.

[0116] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0117] Example 5

[0118] A method for preparing a top-incident quantum dot device with double-end passivation of the interface is the same as that of Example 1, except that step S3 is not included.

[0119] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0120] Embodiment 6:

[0121] A method for preparing a top-incident quantum dot device with double-end passivation of the interface is the same as that of Example 1, except that step S3 specifically comprises repeating the operations S1-S2 twice.

[0122] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0123] Embodiment 7:

[0124] A method for preparing a top-incident quantum dot device with double-end passivation of the interface comprises the following steps:

[0125] A1-A3 are the same as in Example 1;

[0126] A4. Make an interface passivation layer, specifically:

[0127] S1. Preparing a PbS quantum dot ink layer on the PbS quantum dot light absorbing layer, wherein the concentration of the PbS quantum dot ink may be 40 mg / ml;

[0128] S2: Double-terminal ligands are denoted as MDMS;

[0129] Dissolving the double-terminal ligand in an acetonitrile solution to obtain a double-terminal ligand solution, wherein the volume fraction of the double-terminal ligand solution is 2%;

[0130] Dropping the double-terminal ligand solution on the surface of the PbS quantum dot ink layer;

[0131] After standing for 30 seconds to allow the double-terminal molecules to fully exchange the oleic acid ligands on the surface of the PbS quantum dot ink, the double-terminal ligand solution on the surface was removed by spin coating, and finally the orthogonal solution (acetonitrile) was used for two more spin coatings to clean the MDMS solution remaining on the surface to obtain an interface passivation layer;

[0132] A5-A6 are the same as in Example 1.

[0133] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0134] Embodiment 8:

[0135] A method for preparing a top-incident quantum dot device with double-end passivation of the interface comprises the following steps:

[0136] A1-A3 are the same as in Example 1;

[0137] A4. Make an interface passivation layer, specifically:

[0138] S1. Preparing a PbS quantum dot ink layer on the PbS quantum dot light absorbing layer, wherein the concentration of the PbS quantum dot ink may be 13 mg / ml;

[0139] S2: Double-terminal ligands are denoted as MDMS;

[0140] Dissolving the double-terminal ligand in an acetonitrile solution to obtain a double-terminal ligand solution, wherein the volume fraction of the double-terminal ligand solution is 1%;

[0141] Dropping the double-terminal ligand solution on the surface of the PbS quantum dot ink layer;

[0142] After standing for 20 seconds to allow the double-terminal molecules to fully exchange the oleic acid ligands on the surface of the PbS quantum dot ink, the double-terminal ligand solution on the surface was removed by spin coating, and finally the orthogonal solution (acetonitrile) was used for two more spin coatings to clean the MDMS solution remaining on the surface to obtain an interface passivation layer;

[0143] S3, repeat S1-S2 operation twice;

[0144] A5-A6 are the same as in Example 1.

[0145] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0146] Embodiment 9:

[0147] A method for preparing a top-incident quantum dot device with double-end passivation of the interface is the same as that of Example 1, except that the double-end ligand is (3-mercaptopropyl)trimethoxysilane (MTMS (3-Mercaptopropyl)trimethoxysilane)), denoted as MTMS, and its molecular formula is specifically as follows:

[0148] The top-incident quantum dot device with double-end passivation of the interface is prepared by the method for preparing the top-incident quantum dot device with double-end passivation of the interface as described above.

[0149] Comparative Example 1

[0150] A method for preparing a top-incident quantum dot device with double-end passivation on the interface is the same as that in Example 1, except that the volume fraction of the double-end ligand solution is 0.02%.

[0151] Comparative Example 2

[0152] A method for preparing a top-incident quantum dot device with double-end passivation of the interface, which is the same as that of Example 1, except that the interface passivation layer is C with a thickness of 18-22 nm. 60 .

[0153] Comparative Example 3

[0154] A method for preparing a top-incident quantum dot device with double-end passivation of the interface is the same as that of Example 1, except that step A4, preparing an interface passivation layer, is specifically as follows:

[0155] The double-terminal ligand is dissolved in an acetonitrile solution to obtain a double-terminal ligand solution, and the double-terminal ligand solution is dropped on the surface of the PbS quantum dot light-absorbing layer and allowed to stand for 20 seconds. Finally, an orthogonal solution (acetonitrile) is used for spin coating twice to clean the MDMS solution remaining on the surface; wherein the double-terminal ligand is 3-mercaptopropyl (dimethoxy) silane, denoted as MDMS, and the volume fraction of the double-terminal ligand solution is 1%;

[0156] Repeat the above operation once to obtain an interface passivation layer.

[0157] test

[0158] 1. Water erosion test

[0159] A single-layer film of a PbS quantum dot light-absorbing layer (sample 1) was prepared in the same manner as in Example 1;

[0160] After preparing the PbS quantum dot light absorbing layer in the manner of Example 1, an interface passivation layer is stacked on the PbS quantum dot light absorbing layer (Sample 2);

[0161] The above two samples were treated as follows:

[0162] 1. Leave in air to eliminate the influence of water and oxygen in the air, and obtain sample 1-sample 1a and sample 2-sample 2a;

[0163] 2. Perform 200 water cycles to simulate the effect of water heat on the samples, and obtain sample 1-sample 1b and sample 2-sample 2b;

[0164] The above samples were tested for absorption spectrum and fluorescence emission spectrum respectively. According to the test, after water circulation, the peak-to-valley ratio of sample 1 decreased, the peak position blue-shifted, and the fluorescence excitation decreased significantly; while for sample 2, an interface passivation layer was prepared by superimposing it on sample 1. After water circulation, the fluorescence of the sample was significantly enhanced, and the peak position and peak-to-valley ratio did not change significantly, indicating that the interface passivation layer can effectively block water erosion.

[0165] 2. Membrane-substrate bonding strength test at the interface

[0166] A PbS quantum dot light absorption layer was prepared in the same manner as in Example 1, and an interface passivation layer was stacked on the PbS quantum dot light absorption layer, and an electron transport layer was stacked on the interface passivation layer (Sample 3);

[0167] A PbS quantum dot light absorption layer was prepared in the same manner as in Comparative Example 2, and a C 60 layer, in C 60 An electron transport layer is prepared by stacking the layers (sample 4);

[0168] Sample 3 and Sample 4 were respectively pasted with tape on the sample surface, and then the tape was removed. The results were compared with Figure 2 ;

[0169] Figure 2 (b) The sample 4 above the dotted line is not taped, and the sample below the dotted line is the sample with the tape removed after taping. Figure 2 (b) It can be seen that C 60 For the sample of the interface passivation layer, after being pasted with the tape, the film at the pasting location was taken away by the tape, leaving only the PbS quantum dot light absorption layer, and there was a problem of weak bonding between the electron transport layer and the PbS quantum dot light absorption layer;

[0170] Figure 2 (a) The sample 3 is above the dotted line, and the sample 3 after the tape is removed is below the dotted line. It can be seen that after the tape was pasted on the sample surface, the film at the pasting point was not removed by the tape, but left residual adhesive on the sample surface. It can be seen that using MDMS as the ligand-exchanged PbS as the interface passivation layer greatly improves the binding force between the electron transport layer and the PbS quantum dot light absorption layer, which is better than using C 60 This is the interface passivation layer sample.

[0171] 3. Optical contact angle test

[0172] A single layer of PbS quantum dot light absorbing layer (denoted as pristine) was prepared in the same manner as in Example 1;

[0173] A PbS quantum dot light absorption layer was prepared in the manner of Example 1, and then an interface passivation layer (With MDMS) was stacked on the PbS quantum dot light absorption layer;

[0174] A PbS quantum dot light absorption layer was prepared in the same manner as in Comparative Example 2, and then an interface passivation layer (With C 60 );

[0175] The above three samples were tested for optical contact angles. The results are as follows: Figure 3 As shown;

[0176] Depend on Figure 3 It can be seen that the interface passivation layer prepared by stacking the PbS quantum dot light-absorbing layer in the manner of Example 1 has a smaller optical contact angle.

[0177] 4. External Quantum Efficiency

[0178] The top-incident quantum dot device with double-end passivation of the interface prepared in Example 1 and the top-incident quantum dot device with double-end passivation of the interface prepared in Comparative Example 2 were tested for a wide spectrum of 300nm-1650nm. The results are as follows: Figure 4 As shown:

[0179] according to Figure 4 It can be seen that the external quantum efficiency of the top-incident quantum dot device with double-end passivation of the interface prepared in Example 1 is 40.75%, which is better than the external quantum efficiency of the top-incident quantum dot device prepared in Comparative Example 2 (33.93%).

[0180] 5. Dark current IV curve of the device

[0181] 5.1 Impact of thickness control on device performance

[0182] The top-incident quantum dot devices prepared in Example 1, Example 5, Example 6, and Comparative Example 2 were tested for dark current IV curves. The results are as follows: Figure 5 As shown:

[0183] Depend on Figure 5 It can be seen that the dark current suppression effect of Example 1, Example 5, and Example 6 is better than that of Comparative Example 2, that is, the PbS quantum dots exchanged with MDMS as the interface passivation layer have a better suppression effect on the device dark current than C 60 ; Further, when the quantum dot concentration and the MDMS concentration are fixed, the number of spin coating times is adjusted, and then the thickness of the interface passivation layer is adjusted. It can be seen that with the increase or decrease of the spin coating thickness, the dark current suppression effect of the device first increases and then decreases, that is, the corresponding thickness when spin-coated twice has a better dark current suppression effect on the device than the thickness of spin-coating once and three times; further, the thickness of spin-coating once has a better dark current suppression effect on the device than the thickness of spin-coating three times.

[0184] Specifically, the film thickness test is as follows: after the interface passivation layer repeats S1-S2 operations 20 times in the manner of Example 1, the total thickness of the film layer is measured multiple times and the average value is calculated, and then divided by the number of repetitions to obtain a film thickness of 4.5 nm for each operation.

[0185] 5.2 Effect of MDMS ligand concentration on device performance

[0186] The top-incident quantum dot devices prepared in Example 1, Example 2, Comparative Example 1, Example 3, Example 4, and Comparative Example 2 were tested for dark current IV curves. The results are as follows: Figure 6 As shown:

[0187] Depend on Figure 6 It can be seen that when the concentration of the MDMS solution is 0.02%, the suppression effect on the dark current of the device is worse than that of the comparative example 2C. 60 The suppression effect on the dark current of the device may be due to the incomplete exchange of PbS quantum dot ink caused by the low concentration of MDMS solution;

[0188] When the concentration of the MDMS solution is increased to 1%, the dark current suppression effect of the device is greatly improved. On the basis of 1%, the concentration of the MDMS solution is further increased to 5%, 10%, and 15%, respectively. Although the dark current suppression effect of the three is better than that of comparative example 1 (0.02% concentration), it is only slightly better than that of C. 60 effect.

[0189] 5.3 Effect of PbS CQDs ink on device performance

[0190] The top-incident quantum dot devices prepared in Example 1, Comparative Example 2, and Comparative Example 3 were tested for dark current IV curves. The results are as follows: Figure 7 As shown:

[0191] Depend on Figure 7 It can be seen that in Comparative Example 3, the quantum dot ink is not spin-coated on the surface of the quantum dot light absorbing layer, and only the MDMS solution is directly spin-coated, which has no obvious inhibitory effect on the dark current of the device, and is similar to the use of C 60 There is no obvious difference compared with the samples used as the interface layer, and the effect is even worse; while in Example 1, after spin coating the quantum dot ink, the device treated with MDMS molecules has a significantly lower dark current than that of Comparative Example 3.

[0192] 5.4 Impact of MTMS on Device Performance

[0193] The top-incident quantum dot devices prepared in Example 1, Example 9, and Comparative Example 2 were tested for dark current IV curves. The results are as follows: Figure 8 As shown:

[0194] Depend on Figure 8 It can be seen that the dark current suppression effect of Example 9 is better than that of Comparative Example 2, that is, the dark current suppression effect of the device using MTMS as the ligand exchanged PbS quantum dots as the interface passivation layer is better than that of C 60 It is the interface passivation layer.

[0195] 5.5. Effect of Spin Coating Times on Device Performance

[0196] The top-incident quantum dot devices prepared in Example 1, Example 7, Example 8, and Comparative Example 2 were tested for dark current IV curves. The results are as follows: Fig. 9 As shown:

[0197] Depend on Fig. 9 It can be seen that the dark current suppression effects of Example 1, Example 7, and Example 8 are all better than those of Comparative Example 2; further, in Example 7, relative to Example 1, the concentration of the quantum dot ink is doubled, and after a single spin coating, the dark current suppression effect of the device is weaker than that of Example 1; further, in Example 6, relative to Example 1, the concentration of the quantum dot ink is reduced, and after three spin coatings, the dark current suppression effect of the device is also weaker than that of Example 1, indicating that under the condition of equivalent thickness, the dark current suppression effect of the device coated twice is better than that of single spin coating and three spin coatings.

[0198] 6. Device stability test

[0199] The performance of the devices of Example 1 and Comparative Example 2 under 85°C aging conditions is compared. Figure 10-13 As shown:

[0200] Depend on Figure 10-13 It can be seen that with the increase of aging time, the photocurrent turn-on of the device in comparative example 2 with C as the interface passivation layer is severely delayed, and the device gradually loses the rectification characteristic; while the photocurrent turn-on of the device in embodiment 1 with PbS-MDMS as the interface passivation layer is delayed slowly, and the performance deterioration is significantly slower than the former.

[0201] The embodiments of this specific implementation are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. The same components are represented by the same figure marks. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A top-incident quantum dot device with double-end passivation of the interface, comprising a bottom electrode, a hole transport layer, a PbS quantum dot light absorption layer, an electron transport layer and a top electrode arranged in sequence, characterized in that: It also includes an interface passivation layer arranged between the PbS quantum dot light absorption layer and the electron transport layer, and the interface passivation layer includes a PbS quantum dot with a silicon-oxygen structure or an aluminum-oxygen structure at one end of the ligand.

2. The top-incident quantum dot device with double-end passivation according to claim 1, characterized in that: The silicon-oxygen structure is shown in formula (I): Or the aluminum oxide structure is shown in the following formula (II): Wherein, R1 is methoxy or ethoxy, and R2 is methyl or R1.

3. The top-incident quantum dot device with double-end passivation according to claim 1, characterized in that: The thickness of the interface passivation layer is 4.5-12 nm.

4. The top-incident quantum dot device with double-end passivation according to claim 1, characterized in that: The thickness of the interface passivation layer is 8.5-9.5 nm.

5. The method for preparing a top-incident quantum dot device with double-end passivation of the interface according to any one of claims 1 to 4, characterized in that: The method comprises sequentially manufacturing a bottom electrode, a hole transport layer, a PbS quantum dot light absorption layer, an interface passivation layer, an electron transport layer and a top electrode, wherein manufacturing the interface passivation layer is specifically as follows: S1, preparing a PbS quantum dot ink layer on the PbS quantum dot light absorbing layer; S2, drop the double-terminal ligand solution on the surface of the PbS quantum dot ink layer, let it stand and then spin away the double-terminal ligand solution on the surface, wash it, and obtain an interface passivation layer, wherein the double-terminal ligand is X-(CH2) 2-3 -A compound, wherein X is any group selected from -HS, -NH2, -Br, -I or -Cl; and A is a silicon-oxygen structure or an aluminum-oxygen structure.

6. The method for preparing a top-incident quantum dot device with double-end passivation of the interface according to claim 5, characterized in that: The concentration of PbS quantum dot ink is 10-40 mg / ml.

7. The method for preparing a top-incident quantum dot device with double-end passivation of the interface according to claim 6, characterized in that: The volume fraction of the double-terminal ligand solution is 0.5-15%.

8. The method for preparing a top-incident quantum dot device with double-end passivation of the interface according to claim 7, characterized in that: It also includes S3, repeating S1-S2 operations 1-2 times.

9. The method for preparing a top-incident quantum dot device with double-end passivation of the interface according to claim 8, characterized in that: The concentration of the PbS quantum dot ink is 18-22 mg / ml, the volume fraction of the double-terminal ligand solution is 0.8-1.2%, and the S1-S2 operations are repeated once.

10. The method for preparing a top-incident quantum dot device with double-end passivation of the interface according to claim 5, characterized in that: In step S2, the mixture is allowed to stand for 18-22 seconds.

Citation Information

Cited By

  • Quantum dot room temperature medium wave infrared detector and preparation method thereof

    CN119836111A