Method for producing carrier foil for catalyst

Through the preparation method of iron-chromium aluminum alloy catalyst support foil at application temperatures of ≤900°C, the manufacturing process is simplified, the problems of brittle phase formation and high-temperature insulation are solved, and the high-temperature oxidation resistance and manufacturing efficiency are improved.

CN119072553APending Publication Date: 2024-12-03VDM METALS INTERNATIONAL GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035992.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-24
Filing Date
2023-04-06
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing iron-chromium aluminum alloy catalyst support foil has good oxidation resistance at high temperatures, but it is easy to form a brittle phase during low temperature treatment, resulting in material breakage. In the existing preparation process, the high-temperature insulation stage consumes a lot, affecting manufacturing efficiency.

Method used

The preparation method of iron-chromium aluminum alloy catalyst carrier foil at application temperatures of ≤900℃ is adopted. By insulating the thick plates made of hot rolled or forged between 475℃ and 700℃ for 0.5-100 hours, the high-temperature insulation stage is eliminated. , and further cooled to room temperature in air/oil/water to simplify the manufacturing process.

Benefits of technology

It achieves sufficient oxidation resistance at temperatures of 750°C to 900°C, meets the requirements of high-temperature application, and simplifies the manufacturing process and reduces the consumption in the high-temperature insulation stage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Process for preparing a carrier foil for a catalyst having an application temperature of < = 900 DEG C, consisting of an iron-chromium-aluminum alloy having the following (in wt.%) content: Cr 8-14, Al 1-4, the balance Fe and impurities resulting from melting, by casting the alloy into a block, hot-rolling or forging the block into a thick plate with a thickness of between 150 and 400 mm, cooling the thick plate in the hot state to room temperature in air / oil / water or first placing it with means in a furnace installation in the temperature range of 475 DEG C to 700 DEG C and after a holding phase with a holding time of between 0.5 and 100 hours at a holding temperature of between 475 DEG C and 700 DEG C, cooling outside said furnace installation to a chamber and warming.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing a support foil for a catalyst.

[0002] Iron-chromium-aluminum alloys with >10% by weight of chromium and >2% by weight of aluminum are used as metallic support foils for catalysts at application temperatures of 1000° C. and above. The chromium content of these alloys is then typically >18% by weight and the aluminum content >4.5% by weight. Due to this alloy composition, these alloys have very good oxidation resistance at high temperatures (>1000° C.), but on the other hand, if temperatures below about 500° C. occur during process control, the higher chromium and aluminum contents lead to the formation of brittle phases (so-called 475° C. embrittlement) during the ingot production process in hot forming processes on thick plates, hot-rolled strips, cold-rolled strips and foils. In combination with material stresses, these brittle phases can lead to significant material fractures.

[0003] For catalysts to be used up to maximum temperatures of ≤900° C., the oxidation resistance of the metallic support foils (foil thickness of approximately 50 μm) which must be present up to this lower application temperature must be sufficiently good.

[0004] DE 10 2012 004 488 A1 discloses an iron-chromium-aluminum alloy with improved heat resistance, low chromium evaporation rate and good workability, which has (in mass %) 2.0-4.5% Al, 12-25% Cr, 1.0-4.0% W, 0.25-2.0% Nb, 0.05-1.2% Si, 0.001-0.70% Mn, 0.001-0.030% C, 0.0001-0.05% Mg, 0.0001-0.03% Ca, 0.001-0.030% P, maximum 0.03% N, maximum 0.01% S, the remainder being iron and common impurities resulting from melting. The elements Y, Hf and Zr can be added to the alloy as required. Fields of application of such alloys are components in interconnecting plates and / or accessories (such as heat exchangers, in particular) of solid oxide fuel cells and as carrier foils and / or wire meshes in metal exhaust catalysts.

[0005] DE 103 10 865 B3 discloses the use of an iron-chromium-aluminium alloy with good oxidation resistance, which alloy contains (in mass %) 2.5-5.0% Al, 10-25% Cr and 0.05-0.8% Si and additions of >0.01-0.1% Y and / or >0.01-0.1% Hf and / or >0.01-0.2% Zr and / or >0.01-0.2% cerium mixed metal (Ce, La, Nd) and impurities resulting from the production, for components in diesel vehicles and two-stroke equipment, in particular diesel engines and two-stroke engines. After annealing at 1100° C. for 400 hours, the components produced from the alloy have a length change of <4% at a metal thickness of 50 μm. In this context, carrier foils in exhaust metal catalysts and components in exhaust gas purification systems can be considered as components.

[0006] DE 101 57 749 A1 relates to an iron-chromium-aluminum alloy with a long service life, with (in mass %) >2-2.6% aluminum and >10-20% chromium and additions of 0.1-1% Si, up to 0.5% Mn, 0.01-0.2% Y and / or 0.01-0.2% Hf and / or 0.01-0.3% Zr, up to 0.01% Mg, up to 0.01% Ca, up to 0.08% C, up to 0.04% N, up to 0.04% P, up to 0.01% S, up to 0.05% Cu and up to 0.1% Mo and / or W respectively, the remainder being iron and impurities resulting from the production. The alloy can be used, for example, as a heating element for household appliances or as a building material for furnace construction. In addition, the alloy can be used in the form of a foil as a carrier foil for catalysts.

[0007] The materials mentioned in the prior art are prepared industrially as follows:

[0008] The alloy is melted in a melting device such as an arc furnace or an induction furnace and then cast into blocks. These blocks are hot rolled into thick plates and the thick plates are hot rolled into hot strips. Other forming processes are provided with multiple cold rolling steps and intermediate annealing, and the hot strips are cold rolled into strips or foils. Between the individual hot and cold rolling steps, a grinding process of the surface and the separation of the ends of the thick plates are carried out. Each transport step from the location of the rolling plant is carried out with so-called hot transport, in which the material temperature must be kept above 500° C. to above 700° C. in order to suppress the embrittlement phase. After the hot transport, when arriving at the plant where the subsequent rolling process is carried out, the material blocks are placed in a furnace device with a temperature>500° C. and heated to the rolling temperature. Even in the case of a long waiting period before the further transport of the hot rolled pieces to the next process step, these pieces are kept at a higher temperature in the furnace device so that they can be transported to the next process location at a later time by means of hot transport for logistics reasons. The individual process steps and the thermal transport as well as the re-insertion into the furnace system with a temperature > 500 °C include the following stations and transport:

[0009] -Hot transport ingot

[0010] - Place the block in a furnace at >500°C and heat to rolling temperature

[0011] -Hot rolling of blocks into thick plates

[0012] - Place the block in a furnace at >500°C and heat to a higher soak temperature and hold

[0013] - Hot transport thick plates

[0014] - Place the slab into a furnace at >500°C and heat to rolling temperature

[0015] -Hot rolling of thick plates into hot rolled strips

[0016] -Hot transport hot rolled strip

[0017] - Place the hot rolled strip into a furnace at >500°C

[0018] - Hot rolling the hot strip into a strip with certain preset dimensions, cold rolling into strip, and finally cold rolling into foil, with additional intermediate annealing.

[0019] If required, hot rolling of the blocks into thick plates can be replaced by a forging process. A hot grinding process can also be performed during the process.

[0020] The object of the present invention is to provide a method for producing a support foil for a catalyst having an application temperature of ≤900° C., in which the previously described complex production processes, in particular heat transport, are unnecessary.

[0021] Furthermore, protection is sought for the use of the method for specific applications.

[0022] This object is achieved by a method for producing a support foil for a catalyst having an application temperature of ≤900° C., the support foil consisting of an iron-chromium-aluminum alloy having the following contents (in wt. %):

[0023] Cr 8–14%

[0024] Al 1–4%

[0025] The remaining Fe and impurities generated by melting,

[0026] The method comprises casting the alloy into a block,

[0027] The blocks are hot rolled or forged into thick plates with a thickness between 150 and 400 mm.

[0028] Cool to room temperature in air / oil / water

[0029] or

[0030] Firstly, it is placed in a furnace device at a temperature range of 475° C. to 700° C. and after a holding phase at a holding temperature between 475° C. and 700° C. with a holding time between 0.5 and 100 hours, it is cooled outside the furnace device to room temperature.

[0031] Advantageous developments of the method according to the invention can be gathered from the dependent claims.

[0032] The content of the elements Cr, Al, Fe can be modified within the initial distribution range as follows, i.e. Cr 10-13%

[0033] 9-13%

[0034] 9-12%

[0035] Al 1-4%

[0036] 1-3.5%

[0037] 2-3.5%

[0038] 1.5-3%

[0039] The balance is Fe and impurities generated by melting.

[0040] Furthermore, there is the possibility of optionally also providing the following elements in the alloy:

[0041] Up to 0.3% of Y and / or

[0042] Up to 0.3% Hf and / or

[0043] Up to 0.3% La and / or

[0044] Maximum 0.3% cerium, whereby the cerium may be present in the form of mixed metals (Ce, La, Nd).

[0045] Furthermore, there is the possibility of optionally also adding the element Zr to the alloy, with contents of >0 up to 0.5% by weight being conceivable.

[0046] The method according to the invention now makes it possible to dispense with a long holding phase of several hours or even days in a furnace system at a holding temperature significantly above 500° C. in the case of materials with an alloy composition of 8-14% by weight chromium and 1-4% by weight aluminum, the remainder being iron and impurities. In the production process according to the subject matter of the invention, in contrast to the prior art, after the hot rolling process or forging process from block to plate, the plate with a thickness of 150-400 mm, preferably 150 to 250 mm, is directly stored in air / oil / water in a hot state and cooled to room temperature, or is placed in a furnace system at a temperature between 475° C. and 700° C., cooled from the rolling / forging temperature to a temperature between 475° C. and 700° C. and held at a defined holding temperature between 475° C. and 700° C. for a holding period of between 0.5 and 100 hours to achieve temperature equilibrium over the cross section of the plate. The plate is subsequently removed from the furnace system and further cooled in air / oil / water to room temperature.

[0047] This process makes it possible to dispense with complex holding processes (in some cases holding phases lasting longer at holding temperatures significantly above 500° C.), thereby achieving a significant simplification of the production process. Furthermore, in oxidation tests at temperatures of 750° C. to approximately 900° C. for 400 hours, the foil has a sufficiently good oxidation resistance, which in particular meets the requirements as a carrier foil for catalysts with a maximum application temperature between 750 and 900° C.

[0048] Furthermore, protection is claimed for the use of the method according to one or more of claims 1 to 7 for producing a support foil for catalysts having an application temperature of ≤900° C.

[0049] Table 1 discloses the chemical composition (in wt %) of exemplary batch 155408.

[0050] element Actual content% C 0.019 S 0.002 N 0.005 Cr 11.63 Ni 0.15 Mn 0.23 Si 0.18 Ti 0.01 Cu 0.02 Fe 84.71 P 0.014 Al 2.90 Ca 0.001 Zr 0.04 Co 0.01

[0051] Listed in Table 2 are the limits of the preferred chemical compositions of alloys that may be selected for use in the manufacturing process of the present invention and the applications described.

[0052] Table 2

[0053] element Minimum % maximum% C 0.001 0.05 S 0.01 N 0.02 Cr 11 13 Ni 0.5 Mn 0.05 1 Si 0.02 0.5 Ti 0.05 Cu 0.5 Fe margin P 0.03 Al 2.5 3.5 Ca 0.01 Zr 0.01 0.1 Co 0.5

[0054] The alloys described may optionally contain additional elements (such as yttrium and / or hafnium and / or lanthanum and / or cerium) within certain ranges.

Claims

1. A method for producing a support foil for a catalyst having an application temperature of ≤900° C., the support foil consisting of an iron-chromium-aluminum alloy having the following contents (in wt. %): Cr 8–14% Al 1–4% The remaining Fe and impurities generated by melting, The method comprises casting the alloy into a block, The blocks are hot rolled or forged into thick plates with a thickness between 150 and 400 mm, The hot slab is cooled to room temperature in air / oil / water or First, it is placed in a furnace device in a temperature range of 475° C. to 700° C. and, after a holding phase at a defined holding temperature between 475° C. and 700° C. with a holding time between 0.5 and 100 hours, is cooled outside the furnace device to room temperature.

2. The method according to claim 1, wherein the element content in the alloy is set to Cr 9-13% Al 1.0–3.5% The balance is Fe and impurities generated by melting.

3. The method according to claim 1 or 2, wherein the element content in the alloy is set to Cr 10-13% Al 2–3.5% The balance is Fe and impurities generated by melting.

4. The method according to claim 1 or 2, wherein the element content in the alloy is set to Cr 9-12% Al 1.5–3% The balance is Fe and impurities generated by melting.

5. The method according to any one of claims 1 to 4, wherein the following elements are optionally also added to the alloy: Up to 0.3% of Y and / or Up to 0.3% Hf and / or Up to 0.3% La and / or Maximum 0.3% cerium.

6. The method according to any one of claims 1 to 5, wherein the element Zr is optionally also added to the alloy in a content of >0.0 to 0.5%.

7. The method according to any one of claims 1 to 6, characterized in that The thick plate is rolled into a strip or foil by a hot rolling-cold rolling process after cooling to room temperature, wherein at least one heat treatment process is performed on the strip or foil as required.

8. Use of the method according to any one of claims 1 to 7 for producing a support foil for catalysts having an application temperature of ≤900°C.