Biofuel cell, electrode for biofuel cell, enzyme electrode, and electrode slurry for biofuel cell
By using polymers of nonionic ethylenically unsaturated monomers and anionic ethylenically unsaturated monomers as electrode binders, environmental problems of organic solvents in biofuel cells and insufficient adhesion of conductive materials are solved. , realizes biofuel cell electrodes with low ambient load and high output characteristics.
Patent Information
- Application Number
- CN202480001713.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-12-03
AI Technical Summary
The organic solvents used in existing biofuel cells cause damage to the equipment and have a large environmental load, insufficient adhesion of the conductive materials, resulting in insufficient enzyme fixation and poor output characteristics.
Polymers containing nonionic ethylenically unsaturated monomers, anionic ethylenically unsaturated monomers and crosslinking agents are used as electrode binders to form electrodes through screen printing to improve the immobility of enzymes and conductivity of electrodes. .
It achieves low environmental load, low cost and good output characteristics, and is suitable for the electrodes and enzyme electrodes of biofuel cells, improving the immobility of enzymes and the performance of electrodes.
Smart Images

Figure BDA0005017546710000091 
Figure BDA0005017546710000101 
Figure BDA0005017546710000102
Abstract
Description
Technical Field
[0001] The present invention relates to a biofuel cell, and an electrode, an enzyme electrode and an electrode slurry used in the biofuel cell. Background Art
[0002] As a next-generation fuel cell, research and development of biofuel cells that use enzymes and microorganisms as electrode catalysts and generate electricity using biomass resources such as sugars, alcohols, and organic waste liquids as fuels has been conducted (for example, see Patent Documents 1 and 2).
[0003] Biofuel cells using enzymes generally generate electricity by oxidizing and decomposing fuel at the negative electrode (anode) using oxidase to release electrons, and reducing oxygen at the positive electrode (cathode) using reductase to generate water.
[0004] As one of the processes for manufacturing such a biofuel cell in a simple and low-cost manner, a method of patterning an electrode material by screen printing is known. Specifically, a method is generally a method of preparing a slurry (electrode slurry) by dispersing a conductive material such as carbon powder in a binder (electrode binder) obtained by dissolving polyvinylidene fluoride (PVDF) in an organic solvent such as N-methylpyrrolidone (NMP), screen-printing the slurry on a substrate, and drying it to form an electrode pattern (for example, refer to Patent Document 1).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 6994184
[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-140988 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, there is a concern that an electrode binder using NMP as an organic solvent may damage a screen printing device, and the environmental load caused by the organic solvent is also a problem.
[0011] In addition, for electrode slurries using PVDF, it cannot be said that the adhesiveness of the conductive material is necessarily sufficient. Furthermore, PVDF has high water repellency, and for electrode slurries using PVDF, there are also problems such as insufficient fixation of enzymes to electrodes, or enzymes are easily inactivated, and biofuel cells that cannot display sufficient output characteristics are not obtained.
[0012] The present invention has been made to solve such problems, and has as its object to provide a biofuel cell that has low environmental load and low cost and exhibits good output characteristics, and a biofuel cell electrode, an enzyme electrode, and a biofuel cell electrode slurry that are suitable for use in the biofuel cell.
[0013] Means for solving problems
[0014] The present invention is based on the discovery that a predetermined polymer is suitable as an electrode binder when forming an electrode for a biofuel cell by screen printing.
[0015] The present invention provides the following means.
[0016] [1] A biofuel cell that generates electricity through a redox reaction using an enzyme as a catalyst, wherein an enzyme is immobilized on at least one of an anode and a cathode, the anode comprising a conductive material (1) and an electrode binder (1), the cathode comprising a conductive material (2) and an electrode binder (2), at least one of the electrode binder (1) and the electrode binder (2) comprising a polymer (A), the polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), wherein the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0017] [2] A biofuel cell that generates electricity through a redox reaction using an enzyme as a catalyst, wherein at least one of the anode and the cathode comprises a conductive material and an electrode binder, and the enzyme is immobilized thereon, the electrode binder comprising a polymer (A), the polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), wherein the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0018] [3] An electrode for a biofuel cell, comprising a conductive material and an electrode binder, wherein the electrode binder comprises a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), wherein the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0019] [4] An enzyme electrode, comprising the electrode for a biofuel cell described in [3] to which an enzyme is immobilized.
[0020] [5] An electrode slurry for a biofuel cell, comprising an electrode binder, a conductive material and an aqueous medium, wherein the electrode binder comprises a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), wherein the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0021] [6] The biofuel cell electrode slurry according to [5], wherein the content of the electrode binder is 10 to 200 parts by mass based on 100 parts by mass of the conductive material.
[0022] Effects of the Invention
[0023] According to the present invention, it is possible to provide a biofuel cell, an electrode for a biofuel cell, and an enzyme electrode which have low environmental load and low cost and exhibit good output characteristics.
[0024] Furthermore, according to the present invention, it is possible to provide an electrode slurry for a biofuel cell which has a low environmental load, is suitable for screen printing, and can produce a biofuel cell that exhibits good output characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic cross-sectional view schematically showing an example of the configuration of a biofuel cell according to an embodiment of the present invention.
[0026] Figure 2 This is a schematic cross-sectional view schematically showing another example of the structure of the biofuel cell according to the embodiment of the present invention.
[0027] Figure 3 To show schematically Figure 1 A schematic cross-sectional view of an example of an embodiment of a biofuel cell. DETAILED DESCRIPTION
[0028] Definitions and meanings of terms and expressions used in this specification are shown below.
[0029] The electrode for a biofuel cell is also simply referred to as an "electrode", which refers to an electrode in a state before an enzyme is immobilized, and is distinguished from a so-called "enzyme electrode" to which an enzyme is immobilized.
[0030] The expression "X to Y" (X and Y are numerical values) refers to a numerical range with X as the lower limit and Y as the upper limit. In a numerical range (e.g., a range of content, etc.), the lower limit and upper limit recorded in stages can be combined independently. The lower limit and upper limit of the numerical range can be replaced with the numerical values recorded in the examples.
[0031] The content of each structural unit constituting the polymer is a ratio calculated based on the blending amount of the compound from which each structural unit is derived, which is a synthetic raw material for the polymer.
[0032] The term "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid. Similarly, the term "(meth)acrylate" is a general term for acrylate and methacrylate, and the term "(meth)acryloyl" is a general term for acryloyl and methacryloyl.
[0033] The glass transition temperature is the peak top temperature of a temperature differential curve of differential scanning calorimetry (DSC), and is specifically measured by the method described in Examples.
[0034] The median particle size D50 is a 50% cumulative particle size on a volume basis determined from a particle size distribution curve measured by a dynamic light scattering (DLS) method for an aqueous dispersion sample.
[0035] [Biofuel Cell]
[0036] A biofuel cell according to an embodiment of the present invention (hereinafter referred to as the present embodiment) is a biofuel cell that generates electricity by a redox reaction using an enzyme as a catalyst. Furthermore, an enzyme is immobilized on at least one of the anode and the cathode. The anode includes a conductive material (1) and an electrode binder (1), the cathode includes a conductive material (2) and an electrode binder (2), and at least one of the electrode binder (1) and the electrode binder (2) includes a polymer (A), and the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0037] By forming an electrode using an electrode binder containing a polymer (A) having such a predetermined structure, a biofuel cell having a low environmental load and low cost and exhibiting good output characteristics can be obtained.
[0038] The electrode to which the enzyme is immobilized may be only one of the anode and the cathode, or both.
[0039] As the electrode on which the enzyme is immobilized, an enzyme electrode of the present embodiment described later is preferable.
[0040] The biofuel cell of the present embodiment is also preferably a biofuel cell that generates electricity by a redox reaction using an enzyme as a catalyst, wherein at least one of the anode and the cathode comprises a conductive material and an electrode binder, and the enzyme is immobilized. The electrode binder is a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), wherein the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0041] That is, only one of the anode and the cathode may be the enzyme electrode of the present embodiment, or both may be the enzyme electrodes of the present embodiment.
[0042] When both the anode and cathode are enzyme electrodes of this embodiment, the substrates, electrode binders (1) and (2), and conductive materials (1) and (2) of the enzyme electrodes of the anode and cathode may be the same or different.
[0043] As the substrate of the enzyme electrode, for example, paper, cloth, resin film, inorganic materials such as metal materials and ceramics are used.
[0044] When the cathode is not the enzyme electrode of the present embodiment, the cathode may be, for example, a substance on which an oxygen reduction catalyst containing a metal such as platinum is immobilized instead of an enzyme.
[0045] The fuel in the biofuel cell is not particularly limited as long as it is a substance that promotes oxidation by an enzyme. As the fuel, for example, sugars, alcohols, aldehydes, amino acids, amines, lactic acid, uric acid, etc. can be mentioned. The fuel can be a substance that is oxidized after being hydrolyzed by an enzyme (for example, starch or cellulose that is hydrolyzed to become glucose). The fuel can be a single type, or two or more types can be used in combination. Among them, from the viewpoints of output stability, ease of operation, etc., sugars are preferred. The type of sugar is not particularly limited, and monosaccharides, disaccharides, oligosaccharides, polysaccharides, sugar alcohols, etc. can be mentioned. For example, glucose is suitable for use.
[0046] The conductive material (1) and the electrode binder (1) constituting the anode, and the conductive material (2) and the electrode binder (2) constituting the cathode are described below.
[0047] Figure 1 An example of the structure of the biofuel cell according to this embodiment is schematically shown in FIG. Figure 1 The biofuel cell 10 shown has an anode 2 and a cathode 3 formed on the same surface of one surface of a substrate 1 containing a fuel.
[0048] also, Figure 2Another example of the structure of the biofuel cell according to this embodiment is schematically shown in FIG. Figure 2 The biofuel cell 20 shown has an anode 2 formed on one surface of a substrate 1 having a fuel, and a cathode 3 formed on the other (opposite) surface. In this case, the substrate 1 also functions as a separator between the anode 2 and the cathode 3.
[0049] The biofuel cell of this embodiment can generate electricity by supplying only gum syrup or the like as fuel, for example. In another embodiment, for example, sugar as a fuel can be included in the substrate in advance, thereby generating electricity using water.
[0050] In addition, as another embodiment, for example, Figure 3 The method of sticking it on the skin and using it as shown in the figure. Figure 3 In the example, we use Figure 1 The biofuel cell 10 of the embodiment shown in the figure has lead portions 4 formed on each of the anode 2 and the cathode 3. The lead portions 4 are covered with a covering sheet 5, and the substrate 1 is brought into contact with the skin 6, so that the biofuel cell 10 is fixed to the skin 6. The biofuel cell 10 can be fixed to the skin 6 by attaching the covering sheet 6 to the skin 6 using an adhesive sheet, or can be attached to the skin 6 using an adhesive tape or the like.
[0051] exist Figure 3 In the embodiment shown, for example, an enzyme electrode immobilized with lactate oxidase can be used as the anode 2, and an enzyme electrode immobilized with bilirubin oxidase can be used as the cathode 3. In this case, sweat secreted from the skin 6 is absorbed by the substrate 1, and electricity is generated using lactic acid contained in the sweat as fuel. The electricity can be taken out to the outside through the lead portion 4.
[0052] As described above, the biofuel cell of this embodiment can also be used as a biosensor when applied to a living body. For example, the biofuel cell can be installed on an adherend such as skin, clothing, or diapers, and the amount of substances in body fluids such as sweat, urine, blood, tears, and saliva supplied from the adherend can be detected as electricity, and its changes can be measured. This is expected to be used as a wearable device for health management, measurement and management of exercise volume, and the like.
[0053] [Electrodes for biofuel cells]
[0054] The electrode of this embodiment is an electrode for a biofuel cell comprising a conductive material and an electrode binder, wherein the electrode binder comprises a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0055] By using an electrode produced using an electrode binder containing a polymer (A) having such a predetermined structure, a biofuel cell having low environmental load and low cost and exhibiting good output characteristics can be obtained.
[0056] Preferably, at least one of the anode and cathode of the biofuel cell electrode uses the electrode of this embodiment. More preferably, both the anode and the cathode use the electrode of this embodiment. In this case, the electrode binder included in the anode and the electrode binder included in the cathode may have the same composition or different compositions.
[0057] The electrode preferably has at least a conductive material and the electrode binder bonded to a substrate. Such an electrode can be produced by applying an electrode slurry containing the electrode binder, the conductive material, and an aqueous medium to a substrate and drying the slurry.
[0058] As substrate, for example, cloth, paper, resin film, etc. can be cited. In order to make the conductive material close at high density, the substrate is preferably porous, and shows good adhesion with the electrode binder. From the perspective of concerns about environmental load when the biofuel cell is discarded, for example, Japanese paper, etc. are suitable for use. In addition, from the perspective of durability, for example, oil-resistant and water-resistant paper are suitable for use. The coating of the electrode slurry can be implemented on one side of the substrate, or it can be implemented on both sides.
[0059] The details of the electrode slurry, as well as the electrode binder, the conductive material and the aqueous medium are described below.
[0060] The coating method of the electrode slurry is not particularly limited. As the coating method, for example, screen printing, reverse roll method, direct roll method, scraper method, etc. can be cited. Among them, screen printing is preferably used from the viewpoint of being able to form a simple and efficient pattern. In the case of screen printing, for example, a lead portion using a conductive material such as carbon paste and an electrode pattern printed with a plurality of electrodes can also be formed on a substrate.
[0061] The electrode slurry coated on the substrate is dried to fully remove the aqueous medium in the electrode slurry. The drying method is not particularly limited as long as the aqueous medium is fully removed. As the drying method, for example, a method performed under conditions such as hot air, low temperature air, reduced pressure or vacuum, (far) infrared irradiation, etc. can be cited. These drying conditions can be combined.
[0062] [Enzyme electrode]
[0063] The enzyme electrode of the present embodiment has an enzyme immobilized on the electrode.
[0064] In the case of an enzyme electrode for the anode, an enzyme that promotes oxidation of the fuel of the biofuel cell is used. Alternatively, an enzyme that facilitates oxidation of the fuel by hydrolysis or the like may be used in combination.
[0065] As the enzyme used for the anode enzyme electrode, for example, when the fuel is glucose, glucose oxidase or a combination thereof with glucose dehydrogenase etc. can be mentioned. When the fuel is fructose, fructose oxidase or a combination thereof with fructose dehydrogenase etc. can be mentioned. When the fuel is sucrose, invertase or a combination thereof with glucose dehydrogenase etc. can be mentioned. When the fuel is starch, amylase or a combination thereof with glucose dehydrogenase etc. can be mentioned. When the fuel is lactic acid, lactate oxidase etc. can be mentioned.
[0066] In the case of an enzyme electrode for the cathode, an enzyme that promotes the reduction of oxygen is preferably used.
[0067] Examples of the enzyme used in the cathode enzyme electrode include bilirubin oxidase and laccase.
[0068] The enzyme electrode can be produced, for example, by immobilizing an enzyme on an electrode. Alternatively, the enzyme electrode can be produced by applying an enzyme-containing electrode slurry in which an enzyme and an electrode slurry are mixed to a substrate and drying the mixture.
[0069] The method for fixing the enzyme to the electrode is not particularly limited, and for example, the enzyme solution may be applied to the electrode and then dried. The enzyme application may be performed, for example, by dripping or impregnating the enzyme solution. The enzyme may be applied after the mediator is applied.
[0070] The mediator is a redox compound that mediates electron transfer between the electrode and the enzyme, and is appropriately selected according to the types of the fuel and the enzyme. The mediator is supported on the electrode or dissolved in the electrolyte for use.
[0071] When the mediator is supported on the electrode, the mediator may be added to the electrode slurry and applied to the electrode, or the mediator may be applied after the electrode is formed. The mediator may be supported on either the anode or the cathode, or on both.
[0072] Examples of the mediator include organic sulfur compounds such as thionine, thionine acetic acid, tetrathiafulvalene, and 2,2'-azinobis(3-ethylbenzothiazoline-6-sulfonate ammonium); quinone compounds such as hydroquinone, 1,2-naphthoquinone, and 1,4-naphthoquinone; ferrocene; ferrocyanide; osmium coordination compounds, and polymers modified with these compounds. The mediator may be used alone or in combination of two or more.
[0073] From the viewpoint of sufficiently promoting power generation, the concentration of the enzyme immobilized on the electrode is preferably 0.001 U / cm 2 More preferably 0.01 U / cm 2 More preferably, 0.1 U / cm 2 The amount of enzyme immobilized on the electrode is preferably as large as possible, for example, 2000 U / cm 2 Below, can be 1000U / cm 2 Below, can be 500U / cm 2 the following.
[0074] [Electrode binder for biofuel cells]
[0075] The electrode adhesive of this embodiment includes a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), wherein the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
[0076] The electrode binder containing the polymer (A) having such a specified structure has a low environmental load and can obtain an electrode slurry that has good dispersibility of the conductive material and is suitable for screen printing. By using this electrode slurry, a biofuel cell with low environmental load and low cost and showing good output characteristics can be manufactured.
[0077] Hereinafter, the electrode binder is a general term for the electrode binder (1) constituting the anode and the electrode binder (2) constituting the cathode. In addition, the conductive material is a general term for the conductive material (1) constituting the anode and the conductive material (2) constituting the cathode.
[0078] The electrode binder of the present embodiment contains a polymer (A), and may further contain a water-soluble cellulose derivative (B) and other additives described below.
[0079] In order to fully exert the effects of the present invention, the content of the polymer (A) in the electrode binder is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 80% by mass or more, and may be 100% by mass.
[0080] (Polymer (A))
[0081] The polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3).
[0082] Polymer (A) may also have other structural units in addition to the first structural unit, the second structural unit and the third structural unit. In order to fully exert the effect of the present invention, in 100% by mass of all structural units constituting polymer (A), the total of the first structural unit, the second structural unit and the third structural unit is preferably 80 to 100% by mass, more preferably 85% by mass or more, further preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0083] <First structural unit>
[0084] The first structural unit constituting the polymer (A) is derived from the nonionic ethylenically unsaturated monomer (a1).
[0085] In order to obtain a polymer (A) that fully exerts the effects of the present invention, the content of the first structural unit in the total amount of the first structural unit, the second structural unit and the third structural unit constituting the polymer (A) is preferably 60 to 98% by mass, more preferably 75% by mass or more, further preferably 90% by mass or more, and more preferably 97% by mass or less, further preferably 96% by mass or less.
[0086] The nonionic ethylenically unsaturated monomer (a1) serving as a source of the first structural unit has one ethylenically unsaturated bond in one molecule and has neither anionic functional groups nor cationic functional groups. The nonionic ethylenically unsaturated monomer (a1) may be used alone or in combination of two or more.
[0087] As the nonionic ethylenically unsaturated monomer (a1), at least one selected from aromatic ethylenically unsaturated compounds, (meth)acrylic acid alkyl esters, and polar group-containing ethylenically unsaturated carboxylic acid esters is preferably used, and it is preferred that all of them are contained.
[0088] The aromatic ethylenically unsaturated compound contributes to good adhesion of the conductive material and the like.
[0089] Examples of the aromatic ethylenically unsaturated compound include styrene, tert-butylstyrene, α-methylstyrene, p-methylstyrene, 1,1-diphenylethylene, benzyl (meth)acrylate, etc. The aromatic ethylenically unsaturated compound may be used alone or in combination of two or more. Among them, an aromatic vinyl compound is preferred, and styrene is more preferred.
[0090] From the viewpoints of the adhesiveness of the conductive material and the adhesion to the substrate, the proportion of the aromatic ethylenically unsaturated compound in the nonionic ethylenically unsaturated monomer (a1) is preferably 25 to 70% by mass, more preferably 35% by mass or more, further preferably 45% by mass or more, and more preferably 65% by mass or less, further preferably 60% by mass or less.
[0091] The alkyl (meth)acrylate contributes to the ease of synthesis and durability of the polymer (A).
[0092] As the alkyl (meth)acrylate, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, etc. can be mentioned. The alkyl (meth)acrylate can be used alone or in combination of two or more. Among them, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and more preferably 2-ethylhexyl (meth)acrylate.
[0093] As the alkyl (meth)acrylate, the alkyl group bonded to the (meth)acryloyloxy group preferably has 2 to 9 carbon atoms, more preferably 4 to 9 carbon atoms, and even more preferably an alkyl group having 4 to 9 carbon atoms bonded to the acryloyloxy group.
[0094] From the viewpoints of the flexibility of the electrode binder, the adhesiveness of the conductive material, the adhesion to the substrate, etc., the proportion of the (meth)acrylic acid alkyl ester in the nonionic ethylenically unsaturated monomer (a1) is preferably 20 to 70% by mass, more preferably 30% by mass or more, further preferably 40% by mass or more, and more preferably 60% by mass or less, further preferably 50% by mass or less.
[0095] The polar group-containing ethylenically unsaturated carboxylic acid ester contributes to good polymerizability during synthesis of the polymer (A), mechanical stability of the electrode binder, and the like.
[0096] Examples of the polar group of the polar group-containing ethylenically unsaturated carboxylic acid ester include a hydroxyl group and a cyano group.
[0097] As the ethylenically unsaturated carboxylic acid ester containing a polar group, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl acrylate, (meth)acrylonitrile, etc. can be mentioned. The ethylenically unsaturated carboxylic acid ester containing a polar group can be used alone or in combination of two or more. Among them, 2-hydroxyethyl (meth)acrylate is preferred, and 2-hydroxyethyl methacrylate is more preferred.
[0098] From the viewpoints of good polymerizability when synthesizing the polymer (A), adhesion to conductive materials, adhesion to substrates, and swelling resistance of electrode binders when used in batteries, the proportion of the polar group-containing ethylenically unsaturated carboxylic acid ester in the nonionic ethylenically unsaturated monomer (a1) is preferably 0.50 to 20% by mass, more preferably 1.0% by mass or more, further preferably 2.0% by mass or more, and more preferably 15% by mass or less, further preferably 10% by mass or less.
[0099] <Second structural unit>
[0100] The second structural unit constituting the polymer (A) is derived from the anionic ethylenically unsaturated monomer (a2).
[0101] In order to obtain a polymer (A) that fully exerts the effect of the present invention, the content of the second structural unit in the total amount of the first structural unit, the second structural unit and the third structural unit constituting the polymer (A) is preferably 1.5 to 20% by mass, more preferably 3.0% by mass or more, further preferably 4.5% by mass or more, and more preferably 15% by mass or less, further preferably 10% by mass or less.
[0102] The anionic ethylenically unsaturated monomer (a2) serving as a source of the second structural unit has one ethylenically unsaturated bond in one molecule and has an anionic functional group. The anionic ethylenically unsaturated monomer (a2) may be used alone or in combination of two or more.
[0103] Examples of the anionic functional group include a carboxyl group, a sulfo group, a phosphoric acid group, etc. The anionic functional group can form a salt.
[0104] As the anionic ethylenically unsaturated monomer (a2), one or more selected from ethylenically unsaturated carboxylic acids and salts thereof, and ethylenically unsaturated sulfonic acids and salts thereof are preferably used, and it is more preferable to contain all of them.
[0105] Examples of ethylenically unsaturated carboxylic acids and salts thereof include unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; half esters of unsaturated dicarboxylic acids, and salts thereof. Ethylenically unsaturated carboxylic acids and salts thereof may be used alone or in combination of two or more. Among them, (meth)acrylic acid and itaconic acid are preferred.
[0106] From the viewpoints of good polymerizability when synthesizing polymer (A), adhesion to conductive materials, adhesion to substrates, etc., the proportion of ethylenically unsaturated carboxylic acids and salts thereof in anionic ethylenically unsaturated monomers (a2) is preferably 70 to 99% by mass, more preferably 80% by mass or more, further preferably 85% by mass or more, and more preferably 98% by mass or less, further preferably 95% by mass or less.
[0107] Examples of the ethylenically unsaturated sulfonic acid and its salt include p-styrenesulfonic acid and its salt. The ethylenically unsaturated sulfonic acid may be used alone or in combination of two or more. Among them, sodium p-styrenesulfonate is preferred.
[0108] From the viewpoints of good polymerizability when synthesizing the polymer (A), adhesion to conductive materials, adhesion to substrates, etc., the proportion of the ethylenically unsaturated sulfonic acid and its salt in the anionic ethylenically unsaturated monomer (a2) is preferably 1.0 to 30% by mass, more preferably 2.0% by mass or more, further preferably 3.0% by mass or more, and more preferably 20% by mass or less, further preferably 15% by mass or less.
[0109] <Third structural unit>
[0110] The third structural unit constituting the polymer (A) is derived from the cross-linking agent (a3).
[0111] From the viewpoint of the swelling resistance of the electrode binder when the battery is used, the content of the third structural unit in the total amount of the first structural unit, the second structural unit and the third structural unit constituting the polymer (A) is preferably 0.010 to 0.50 mass%, more preferably 0.020 mass% or more, further preferably 0.030 mass% or more, and more preferably 0.30 mass% or less, further preferably 0.10 mass% or less.
[0112] The crosslinking agent (a3) serving as a source of the third structural unit has two or more ethylenically unsaturated bonds in one molecule. The crosslinking agent (a3) may be used alone or in combination of two or more.
[0113] The crosslinking agent (a3) can form a crosslinked structure by addition reaction of two or more ethylenically unsaturated bonds with ethylenically unsaturated bonds of other synthetic raw material compounds of the polymer (A). That is, the polymer (A) is a crosslinked polymer.
[0114] Examples of the crosslinking agent (a3) include divinylbenzene, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 2-hydroxy-3-acryloyloxypropyl methacrylate. Among these, divinylbenzene is preferred.
[0115] <Glass transition temperature>
[0116] From the viewpoints of the adhesiveness of the conductive material, the adhesion to the substrate, the good flexibility of the electrode binder, etc., the glass transition temperature of the polymer (A) is preferably -30 to 100°C, more preferably -20°C or higher, further preferably -10°C or higher, and more preferably 90°C or lower, further preferably 80°C or lower.
[0117] <Particle size>
[0118] The polymer (A) exists as dispersed particles in the electrode binder composition containing an aqueous dispersion medium. The suitable particle size of the dispersed particles varies depending on the form of the conductive material, the particle size, etc. In order to fully exert the effect of the present invention, the median particle size D50 of the particles in the aqueous dispersion is preferably 0.10 to 1.0 μm. It is more preferably 0.15 μm or more, and more preferably 0.20 μm or more. In addition, it is more preferably 0.80 μm or less, and more preferably 0.50 μm or less.
[0119] <Synthesis method>
[0120] The polymer (A) can be produced by polymerizing a synthetic raw material containing a nonionic ethylenically unsaturated monomer (a1), an anionic ethylenically unsaturated monomer (a2), and a crosslinking agent (a3). The polymerization method is not particularly limited, and a suitable example thereof is emulsion polymerization.
[0121] Emulsion polymerization is carried out in an aqueous medium in the presence of a polymerization initiator, with the addition of a surfactant and other additives as required. The synthetic raw materials may be added all at once or may be supplied in succession by dropwise addition. Usually, the reaction is carried out at 30 to 90°C while stirring.
[0122] Furthermore, from the viewpoint of the stability of the polymer (A) in the reaction system, it is preferred to add a basic substance for neutralization and pH adjustment during or after the polymerization reaction as necessary.
[0123] Preferred examples of the alkaline substance include ammonia, triethylamine, ethanolamine, morpholine, 2-amino-2-methyl-1-propanol, lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. The alkaline substance may be used alone or in combination of two or more.
[0124] The aqueous medium is water, a hydrophilic solvent, or a mixture thereof. Examples of the hydrophilic solvent include methanol, ethanol, isopropanol, N-methylpyrrolidone (NMP), and 1,3-butanediol.
[0125] The aqueous medium is preferably water from the viewpoint of dispersion stability of synthetic raw materials and polymers, reduction of environmental load, etc. A mixture of water and a hydrophilic solvent is also preferred as long as the dispersion stability is not impaired.
[0126] The aqueous medium used in the synthesis of the polymer (A) may be used as the aqueous medium constituting the electrode binder composition, and may remain as it is after the synthesis.
[0127] The amount of the aqueous medium used is appropriately adjusted according to the dispersibility of the synthetic raw materials in the aqueous medium, the viscosity of the reaction system, etc. From the viewpoint of carrying out a moderate polymerization reaction, the amount of the aqueous medium used is preferably 50 to 300 parts by mass relative to 100 parts by mass of the total of the nonionic ethylenically unsaturated monomer (a1), the anionic ethylenically unsaturated monomer (a2), and the crosslinking agent (a3). More preferably, it is 80 parts by mass or more, and more preferably, it is 100 parts by mass or more, and more preferably, it is 250 parts by mass or less, and more preferably, it is 200 parts by mass or less.
[0128] The polymerization initiator is not particularly limited, and a free radical polymerization initiator can be used, for example, peroxides such as ammonium persulfate, potassium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide can be mentioned. One polymerization initiator can be used alone, or two or more polymerization initiators can be used in combination. In addition, redox polymerization using these polymerization initiators in combination with a reducing agent such as sodium bisulfite, Rongalite, and ascorbic acid can also be used.
[0129] As the surfactant, one or more selected from nonionic surfactants and anionic surfactants are preferably used from the viewpoint of dispersion stability of the synthetic raw materials and the produced polymer (A) in the aqueous medium.
[0130] Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, etc. The nonionic surfactant may be used alone or in combination of two or more.
[0131] Examples of the anionic surfactant include alkylbenzene sulfonates, alkyl sulfate ester salts, polyoxyethylene alkyl ether sulfate ester salts, and fatty acid salts.
[0132] As the anionic surfactant, a reactive surfactant having an ethylenically unsaturated bond can also be preferably used.
[0133] As the reactive surfactant, for example, compounds represented by the following formulae (1) to (4) can be mentioned. The reactive surfactant may be used alone or in combination of two or more. Among them, the compound represented by formula (4) is preferred, and alkyl allyl sodium sulfosuccinate is more preferred.
[0134]
[0135] In formula (1), R 1 is an alkyl group, and p is an integer from 10 to 40. 1 An alkyl group having 10 to 40 carbon atoms is preferred, and a linear alkyl group having 10 to 40 carbon atoms is more preferred.
[0136]
[0137] In formula (2), R 2 is an alkyl group, and q is an integer of 10 to 12. 2 An alkyl group having 10 to 40 carbon atoms is preferred, and a linear alkyl group having 10 to 40 carbon atoms is more preferred.
[0138]
[0139] In formula (3), R 3 is an alkyl group, M 1 For NH 4 Or Na. R 3 An alkyl group having 10 to 40 carbon atoms is preferred, and a linear alkyl group having 10 to 40 carbon atoms is more preferred.
[0140]
[0141] In formula (4), R 4 is an alkyl group, M 2 For NH 4 Or Na. R 4 An alkyl group having 10 to 40 carbon atoms is preferred, and a linear alkyl group having 10 to 40 carbon atoms is more preferred.
[0142] In addition, the reactive surfactant plays an emulsifying role in the reaction system in the emulsion polymerization and has copolymerizability with the nonionic ethylenically unsaturated monomer (a1), the anionic ethylenically unsaturated monomer (a2), and the crosslinking agent (a3), but in the present embodiment, it is not regarded as a structural unit constituting the polymer (A).
[0143] From the viewpoints of stable progress of the polymerization reaction, dispersion stability of the synthetic raw materials and the generated polymer (A) in the aqueous medium, and adhesion of the conductive material to the substrate, the amount of the surfactant added is preferably 0.050 to 1.2 parts by mass relative to 100 parts by mass of the total of the nonionic ethylenically unsaturated monomer (a1), the anionic ethylenically unsaturated monomer (a2), and the crosslinking agent (a3). It is more preferably 0.10 parts by mass or more, and even more preferably 0.15 parts by mass or more. In addition, it is more preferably 1.0 parts by mass or less, and even more preferably 0.50 parts by mass or less.
[0144] Examples of other additives include chain transfer agents such as mercaptans, thioglycolic acid and esters thereof, and 3-mercaptopropionic acid and esters thereof.
[0145] The addition of other additives is optional, and they can be added within a range that does not hinder the effects of the present invention.
[0146] (Water-soluble cellulose derivative (B))
[0147] The electrode binder of the present embodiment also preferably contains the polymer (A) and further contains a water-soluble cellulose derivative (B).
[0148] The water-soluble cellulose derivative (B) plays a role in facilitating the dispersion of the conductive material in the electrode slurry.
[0149] As the water-soluble cellulose derivative (B), for example, celluloses such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose and their salts; polyvinyl alcohol; polyvinyl pyrrolidone, etc. can be mentioned. As the salt of cellulose, for example, ammonium salts, alkali metal salts, etc. can be mentioned. The water-soluble cellulose derivative (B) can be used alone or in combination of two or more. Among them, carboxymethyl cellulose and its salts are preferred.
[0150] When the water-soluble cellulose derivative (B) is included in the electrode binder, the content is preferably 1 to 50% by mass, more preferably 5% by mass or more, further preferably 10% by mass or more, and more preferably 40% by mass or less, further preferably 30% by mass or less, from the viewpoint of not hindering the action of the polymer (A) and obtaining good dispersibility of the conductive material.
[0151] The total content of the polymer (A) and the water-soluble cellulose derivative (B) in the electrode binder is preferably 80% by mass or more, more preferably 95% by mass or more, and may be 100% by mass.
[0152] [Electrode binder composition]
[0153] The electrode binder composition includes the electrode binder of the present embodiment and an aqueous medium, and the polymer (A) is dispersed in the aqueous medium.
[0154] The electrode binder composition can be produced by mixing the electrode binder and the aqueous medium. The mixing method is not particularly limited.
[0155] As the aqueous medium in the electrode binder composition, the same substance as the aqueous medium used in the synthesis method of the above-mentioned polymer (A) can be exemplified, and it can be the same as or different from the aqueous medium used in the synthesis method of the polymer (A). The aqueous medium used in the synthesis of the polymer (A) can include a substance that directly remains after the synthesis.
[0156] The aqueous medium is preferably water from the viewpoint of dispersion stability of the electrode binder in the electrode binder composition, reduction of environmental load, etc. A mixture of water and a hydrophilic solvent is also preferred as long as the dispersion stability is not impaired.
[0157] The content of the polymer (A) in the electrode binder composition can be appropriately adjusted by arbitrarily adding an aqueous medium when manufacturing the electrode slurry, but from the viewpoints of easy-to-handle viscosity, dispersion stability of the polymer (A), etc., it is preferably 10 to 80% by mass, more preferably 15% by mass or more, and further preferably 20% by mass or more. In addition, it is more preferably 70% by mass or less, and further preferably 60% by mass or less.
[0158] [Electrode slurry]
[0159] The electrode slurry of the present embodiment contains the electrode binder of the present embodiment described above, a conductive material, and an aqueous medium.
[0160] The electrode slurry can be produced by mixing an electrode binder, a conductive material, and an aqueous medium. The mixing method is not particularly limited, but in order to disperse the conductive material sufficiently and uniformly, kneading is preferably performed using, for example, a rotary mixer or the like.
[0161] The electrode slurry may contain other components in addition to the electrode binder, the conductive material and the aqueous medium within a range that does not hinder the effects of the present invention. Examples of other components include surfactants from the viewpoint of dispersion stability and the like.
[0162] In order to fully exert the effects of the present invention, the total content of the electrode binder, the conductive material and the aqueous medium in the electrode slurry is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 80% by mass or more, and may be 100% by mass.
[0163] The aqueous medium in the electrode slurry is the same as the description of the aqueous medium in the above-mentioned electrode binder composition.
[0164] As the conductive material, for example, carbon materials, metal materials, etc. can be mentioned. As the carbon material, for example, graphite, carbon black, porous carbon, etc. can be mentioned. The conductive material can be used alone or in combination of two or more. Among them, from the viewpoints of operability, the fixation of the enzyme, etc., preferably a carbon material, more preferably porous carbon.
[0165] Examples of porous carbon include mesoporous carbon, and more specifically, mesoporous carbon produced by a template method such as Ketjen black, carbon nanotubes, graphene, and MgO template carbon. Among these, MgO template carbon is preferably used from the viewpoint of good enzyme fixation.
[0166] From the viewpoint of allowing a sufficient amount of conductive material to adhere closely to the substrate, the content of the conductive material in the electrode slurry is preferably 40 to 85% by mass, more preferably 45% by mass or more, further preferably 50% by mass or more, and more preferably 80% by mass or less, further preferably 75% by mass or less.
[0167] The content of the electrode binder in the electrode slurry is preferably 10 to 200 parts by mass relative to 100 parts by mass of the conductive material, as a sufficient amount for the close adhesion of the conductive material to the substrate. It is more preferably 20 parts by mass or more, and further preferably 30 parts by mass or more. In addition, it is more preferably 150 parts by mass or less, further preferably 120 parts by mass or less, and further preferably 60 parts by mass or less.
[0168] From the viewpoints of the applicability of the electrode slurry to screen printing and the reduction of the amount used, the total content of the electrode binder and the conductive material in the electrode slurry is preferably 40 to 80% by mass, more preferably 45% by mass or more, further preferably 50% by mass or more, and more preferably 75% by mass or less, further preferably 70% by mass or less.
[0169] [Example]
[0170] Hereinafter, the present invention will be specifically described based on examples. The present invention is not limited to the following examples, and various modifications can be made within the scope of the present invention.
[0171] [Production of polymer (A)]
[0172] The methods for measuring various physical properties in the following synthesis examples are as follows.
[0173] <Glass transition temperature>
[0174] Differential scanning calorimetry (DSC) was measured using a differential scanning calorimeter ("EXSTAR DSC7020", manufactured by Hitachi HiTech Science & Technology Co., Ltd.; heating rate: 10°C / min, nitrogen atmosphere), and the peak top temperature of the temperature differential curve of the DSC was defined as the glass transition temperature.
[0175] <Median particle size D50>
[0176] The median particle size D50 (volume basis) was determined from a particle size distribution curve measured by a dynamic light scattering (DLS) method.
[0177] (Synthesis example 1)
[0178] In a reaction container equipped with a cooling tube, a thermometer, a stirrer and a dropping funnel, 60 parts by mass of ion exchange water was added and the temperature was raised to 75°C. A mixed solution containing a nonionic ethylenically unsaturated monomer (a1), an anionic ethylenically unsaturated monomer (a2), a crosslinking agent (a3) totaling 100 parts by mass, 0.20 parts by mass of Elemi Nol JS-20 (excluding the solvent), 0.20 parts by mass of HiTen Nol 08E, and 80 parts by mass of ion exchange water was added dropwise in the reaction container over 3 hours, and stirred and mixed. At the same time, a substance obtained by dissolving 0.40 parts by mass of potassium persulfate in 10 parts by mass of ion exchange water was added dropwise over 3 hours, stirred and mixed, and polymerized.
[0179] Two hours after the completion of the dropwise addition, the reaction product was neutralized with 0.90 parts by mass of 25% by mass ammonia water to obtain a dispersion of the polymer (A1) (content of the polymer (A1) 40% by mass).
[0180] [Table 1]
[0181] Table 1
[0182]
[0183] In addition, the details of the surfactants in Table 1 are as follows.
[0184] Eleminol JS-20: sodium alkyl allyl sulfosuccinate; "Eleminol (registered trademark) JS-20", manufactured by Sanyo Chemical Industries, Ltd.; anionic reactive surfactant; non-volatile content 38.5% by mass
[0185] · HI-TENOLE 08E: polyoxyethylene oleyl cetyl ether ammonium sulfate; "HI-TENOLE (registered trademark) 08E", manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; anionic surfactant
[0186] The glass transition temperature of the polymer (A1) was 15° C. and the median particle size D50 was 0.26 μm.
[0187] [Manufacturing of electrode slurry]
[0188] The raw materials used in the production of the electrode slurry are as follows.
[0189] Porous carbon powder: "Kunobel (registered trademark) MJ (3) 100-00", manufactured by Toyo Tanso Co., Ltd.; BET specific surface area 390 m 2 / g, total pore volume 0.91mL / g, micropore capacity 0.15mL / g, mesopore diameter 75nm, bulk density 0.06g / mL
[0190] Electrode binder composition (1): a dispersion of the polymer (A1) (electrode binder) prepared in Synthesis Example 1 (non-volatile content 40% by mass)
[0191] Electrode binder composition (2): "Kureha KF Polymer L#9305", manufactured by Kureha Co., Ltd.; 5 mass % NMP solution of PVDF ("Kureha KF Polymer L#9300": electrode binder)
[0192] Electrode binder composition (3): styrene / butadiene rubber (electrode binder) latex (non-volatile content 40% by mass)
[0193] Electrode binder composition (4): PTFE (electrode binder) aqueous dispersion (non-volatile content 60% by mass)
[0194] The porous carbon powder, the electrode binder composition, and the additive medium were mixed in the compositions shown in Table 2, and kneaded using a rotary mixer to produce electrode slurries 1 to 9, respectively.
[0195] As shown in Table 2, the dispersibility of the porous carbon powder in the obtained electrode slurries was good (○) for electrode slurries 1 to 8, and poor (×) for electrode slurry 9.
[0196] [Manufacturing of biofuel cells]
[0197] Biofuel cells were produced by the following methods using electrode slurries 1 to 9. The cases using electrode slurries 1 to 6 are examples, and the cases using electrode slurries 7 to 9 are comparative examples.
[0198] The following shows the details of the materials and raw materials used in the manufacture of the biofuel cell.
[0199] ·Base material (Japanese paper): Rice paper with water-repellent treatment; Izumo Japanese paper
[0200] ·Base material (oil-resistant and water-resistant paper): "Oil-resistant and water-resistant paper (3)", manufactured by Lintech Co., Ltd.
[0201] ·Carbon paste: "JELCON CH-8", manufactured by Jujo Micron Co., Ltd.
[0202] ·AzBTS: 2,2'-azinobis(3-ethylbenzothiazoline-6-sulfonate ammonium); manufactured by Tokyo Chemical Industry Co., Ltd.
[0203] ·TTF:Tetrathiafulvalene
[0204] ·GOD: Glucose oxidase; manufactured by Fujifilm Wako Junyao Co., Ltd.
[0205] Phosphate buffer: 1 mol / L phosphate buffer, pH 7.0
[0206] · BOD: Bilirubin oxidase; manufactured by Amano Enzyme Co., Ltd.
[0207] · Triton X-100: polyethylene glycol-tert-octylphenyl ether; "Triton (registered trademark) X-100"; manufactured by Rossu Diagnosis Technology Co., Ltd.; nonionic surfactant
[0208] The carbon paste was screen-printed on the substrate and dried at 120°C for 20 minutes to form a lead portion. The electrode paste with 0.04g of AzBTS added as a mediator was screen-printed three times on the lead portion, and then dried at 45°C for 30 minutes to form 32 electrodes of 20mm×5mm, which were then cleaned with UV ozone for 15 minutes. The electrode pattern was set to an electrode pattern in which 4 anodes and 4 cathodes were connected in series and 4 in parallel.
[0209] A saturated methanol solution of TTF was dripped as a mediator at a portion corresponding to the anode of the electrode, and further, 20 μL of a liquid (10 U / μL) in which GOD was dispersed in a phosphate buffer was dripped per anode.
[0210] In the portion corresponding to the cathode of the electrode, 20 μL of a liquid (10 U / μL) in which BOD was dispersed in a phosphate buffer solution having a concentration of 0.01% by mass of Triton X-100 was dropped per cathode.
[0211] Then, the electrode (pattern electrode) was dried under reduced pressure for 1 hour to prepare an enzyme electrode plate in which GOD was fixed to the anode and BOD was fixed to the cathode.
[0212] In addition, enzyme electrode plates using Japanese paper as a substrate were prepared using electrode slurries 1, 7, and 8, and enzyme electrode plates using oil-resistant and water-resistant paper were prepared using electrode slurries 1 to 6. Electrode slurry 9 had poor dispersibility, so a biofuel cell using it was not prepared (Comparative Example 3).
[0213] In addition, a phosphate buffer solution (1 mL / cm 2 ), and dried at 100° C. for 30 minutes to prepare a substrate containing glucose.
[0214] The glucose-containing substrate is placed on the enzyme electrode of the enzyme electrode plate to produce a biofuel cell.
[0215] [Output characteristics evaluation]
[0216] The output of each biofuel cell manufactured by the above method was measured by linear sweep voltammetry (measurement conditions: two-electrode method, sweep potential open circuit voltage 0V, sweep rate 1mV / s), and the maximum output was obtained. The liquid supply during the measurement was performed by dropping 1 mol / L phosphate buffer (pH 7.0).
[0217] Table 2 shows the measured values of the maximum output.
[0218] [Table 2]
[0219] Table 2
[0220]
[0221] As shown in Table 2, it was confirmed that the biofuel cell manufactured using electrode slurry 1 showed good output characteristics (Example 1). In addition, the biofuel cells manufactured using electrode slurries 2 to 6 also showed good output characteristics (Examples 2 to 6). On the other hand, the output characteristics of the biofuel cells manufactured using electrode slurries 7 and 8 were poor (Comparative Examples 1 and 2).
[0222] Based on the above, it can be said that the biofuel cell produced using the electrode slurry containing the aqueous electrode binder according to the present embodiment exhibits good output characteristics.
[0223] Explanation of symbols
[0224] 1. Substrate
[0225] 2 Anode
[0226] 3 Cathode
[0227] 4 Lead wire
[0228] 5 Covering sheet
[0229] 6 Skin
[0230] 10.20 Biofuel cells.
Claims
1. A biofuel cell that generates electricity through a redox reaction using an enzyme as a catalyst, An enzyme is immobilized on at least one of the anode and the cathode, The anode comprises a conductive material (1) and an electrode binder (1), The cathode comprises a conductive material (2) and an electrode binder (2), At least one of the electrode binder (1) and the electrode binder (2) comprises a polymer (A), The polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3). The crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
2. A biofuel cell that generates electricity through a redox reaction using an enzyme as a catalyst, At least one of the anode and the cathode comprises a conductive material and an electrode binder, and an enzyme is immobilized thereon. The electrode binder comprises a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), The crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
3. An electrode for a biofuel cell, comprising a conductive material and an electrode binder, The electrode binder comprises a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), The crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule. 4 . An enzyme electrode, comprising the electrode for a biofuel cell according to claim 3 to which an enzyme is immobilized.
5. An electrode slurry for a biofuel cell, comprising an electrode binder, a conductive material and an aqueous medium, The electrode binder comprises a polymer (A), wherein the polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), The crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule. 6 . The electrode slurry for a biofuel cell according to claim 5 , wherein the content of the electrode binder is 10 to 200 parts by mass based on 100 parts by mass of the conductive material.
Citation Information
Patent Citations
Preparation method of photofixation horse radish peroxidase electric pole and uses thereof
CN101140256A
Binder for lithium ion secondary battery electrode, slurry obtained using the binder for electrode, electrode obtained using the slurry, and lithium ion secondary battery using the electrode
CN102934269A
Lithium ion battery negative electrode aqueous adhesive and preparation method thereof
CN107325225A
Aqueous catalyst paste composition for fuel batteries, and fuel battery
JP2015028932A
Composition for forming enzyme battery positive electrode, positive electrode for enzyme battery, and enzyme battery