SO3 adsorbent as well as preparation method and application thereof

By loading alcohol amine-modified graphene oxide and carbon nanotubes on activated carbon, an efficient SO3 adsorbent is formed, which solves the problem of high-concentration SO3 flue gas treatment, and achieves efficient and stable SO3 removal effect, which is suitable for coal burning Industrial application of power plants.

CN119075916AActive Publication Date: 2024-12-06XIAMEN SIYAN NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411373394.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the concentration of high concentration SO3 in flue gas, resulting in corrosion and pollution to coal-fired power plant equipment. The ultra-low emission transformation increases the SO2/SO3 conversion rate, further exacerbating the challenge of SO3 emission control.

Method used

Using SO3 adsorbents including activated carbon and alcohol amine-loaded graphene oxide and carbon nanotubes, the olefin carbon mixture is uniformly loaded on the activated carbon through ultrasonic treatment and solid-liquid separation to form an efficient SO3 adsorbent, using hydrogen bonds. Combining with van der Waals can improve the adsorption capacity of SO3.

Benefits of technology

It achieves efficient removal of high-concentration SO3 flue gas, maintains long-term adsorption efficiency, avoids powder loss and pore blockage of adsorbents, and meets the needs of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068133600000141
    Figure BDA0005068133600000141
  • Figure BDA0005068133600000151
    Figure BDA0005068133600000151
Patent Text Reader

Abstract

The invention belongs to the field of flue gas treatment, and provides an SO3 adsorbent and a preparation method and application thereof. The SO3 adsorbent comprises activated carbon and an olefinic carbon mixture loaded on the activated carbon, and the olefinic carbon mixture comprises alcohol amine modified graphene oxide and carbon nanotubes. The SO3 adsorbent can effectively remove SO3 in flue gas, and is especially suitable for treating flue gas with high-concentration SO3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of flue gas treatment, and specifically provides a SO3 adsorbent and a preparation method and application thereof. Background Art

[0002] As a power plant pollutant, SO3 emissions not only damage boiler equipment, but also threaten the ecological environment and even life safety. Therefore, SO3 emission control has received more and more attention. High-temperature combustion in the furnace and selective catalytic reduction (SCR) catalytic oxidation of part of SO2 are the main reasons for the generation of SO3. When burning high-sulfur coal, the SO3 concentration in the flue gas at the SCR outlet can reach 100mg / m 3 Even higher. Although the electrostatic precipitator, wet electrostatic precipitator and other devices in the power plant can effectively remove SO3 to avoid discharge into the atmosphere, the high concentration of SO3 and H2SO4 vapor in the flue will cause serious damage to the equipment, causing blockage of the SCR catalyst and air preheater, deactivation of the SCR catalyst, corrosion of downstream pipelines and equipment, and even corrosion of concrete and plastic parts in the plant. Therefore, reducing the concentration of SO3 in the flue gas is also of great significance to the stable operation of the coal-fired system. With the implementation of ultra-low emission transformation of thermal power plants, SO2, NOx and smoke emissions have been effectively controlled, and the control of SO3 emissions, an unconventional pollutant, will become the focus of the next stage of atmospheric pollutant control.

[0003] In addition, since the ultra-low emission transformation of coal-fired power plants generally adds a spare layer of adsorbent, the increase in SO2 / SO3 conversion rate increases the concentration of SO3 downstream of denitrification, resulting in the corresponding SO3 or NH4HSO4 (generated by the reaction of escaped NH3 in the flue gas with SO3) causing corrosion and blockage problems and post-emission pollution problems. This also brings new challenges to the control of SO3 pollutants in coal-fired power plants. Summary of the invention

[0004] In view of the above problems existing in the prior art, the purpose of the present application is to provide a SO3 adsorbent and its preparation method and application. The SO3 adsorbent of the present application can effectively remove SO3 from flue gas, and is particularly suitable for treating flue gas with high concentration of SO3.

[0005] In a first aspect, the present application provides a SO3 adsorbent, comprising activated carbon and an olefin-carbon mixture supported thereon, wherein the olefin-carbon mixture comprises amine-modified graphene oxide and carbon nanotubes.

[0006] In the SO3 adsorbent provided in the present application, the activated carbon has a developed pore structure. Using activated carbon as a carrier is beneficial to reducing the cost of the adsorbent and realizing the industrial production and application of the adsorbent. Loading amine-modified graphene oxide and carbon nanotubes on activated carbon can significantly improve the adsorption capacity of activated carbon for SO3; wherein, the hydroxyl group (-OH) on the surface of amine-modified graphene oxide can form hydrogen bonds with SO3, and the alkaline amine has a strong affinity for acidic SO3, and the carbon nanotubes have a more uniform structure at the atomic scale, which can provide the adsorbent with clear adsorption sites and stronger van der Waals binding energy, and improve the bonding strength between amine-modified graphene oxide and activated carbon, avoiding the "powdering" phenomenon of the adsorbent caused by flue gas flow, so that the SO3 adsorbent maintains a high SO3 removal efficiency in long-term flue gas treatment.

[0007] In some embodiments of the present application, the alcoholamine-modified graphene oxide is at least one of monoethanolamine-modified graphene oxide, diethanolamine-modified graphene oxide and triethanolamine-modified graphene oxide.

[0008] Furthermore, the graphene oxide modified by alcoholamine is graphene oxide modified by diethanolamine. In this case, the adsorbent has stronger alkalinity, which can further improve the adsorption efficiency of SO3.

[0009] In some embodiments of the present application, the iodine value of the activated carbon is not less than 800 mg / g, and the specific surface area is 500 to 1500 m 2 / g, particle size is 3 to 9 mm.

[0010] In some embodiments of the present application, the mass ratio of the activated carbon to the olefin-carbon mixture is 100:(0.2-2). Thus, the adsorbent can maintain a relatively high adsorption capacity for SO3: if the loading amount of the olefin-carbon mixture is too low, the ability to improve the adsorption capacity of the activated carbon is limited, while if the loading amount is too high, the pores of the activated carbon may be blocked.

[0011] Furthermore, the mass ratio of the activated carbon to the olefin-carbon mixture is 100:(0.3-1).

[0012] In some embodiments of the present application, the mass ratio of the amine-modified graphene oxide to the carbon nanotubes is (1-4): 1. In this case, the adsorbent "powdering" caused by too low a carbon nanotube content can be avoided as much as possible, and the reduction in removal efficiency caused by too much carbon nanotube content can be suppressed.

[0013] Furthermore, the mass ratio of the amine-modified graphene oxide to the carbon nanotubes is (1.5-3):1.

[0014] In a second aspect, the present application provides a method for preparing the SO3 adsorbent described in the first aspect of the present application, the method comprising:

[0015] (1) uniformly dispersing graphene oxide and carbon nanotubes in a solvent to obtain an olefin-carbon dispersion;

[0016] (2) mixing the graphene-carbon dispersion with an activator and performing a first ultrasonic treatment to activate the graphene oxide and the carbon nanotubes to obtain a reaction solution;

[0017] (3) mixing the reaction solution, alcoholamine and activated carbon and subjecting the mixture to a second ultrasonic treatment, so that the alcoholamine modifies the activated graphene oxide to form alcoholamine-modified graphene oxide, thereby obtaining a mixed solution;

[0018] (4) The mixed liquid is subjected to solid-liquid separation, washing and drying to obtain a SO3 adsorbent.

[0019] The method provided by the present application can promote the uniform dispersion of the olefin-carbon mixture and load it to the inner surface of the activated carbon pores, thereby obtaining an adsorbent in which the olefin-carbon mixture is evenly distributed on the carrier activated carbon. Specifically, compared with directly modifying the activated carbon by impregnating the graphene oxide and carbon nanotubes modified with alcohol amines, the present application first disperses the graphene oxide and carbon nanotubes in a solvent and performs activation treatment together, and then performs alcohol amination modification of the graphene oxide in situ in the presence of activated carbon. This method can improve the uniformity of the loading of the olefin-carbon mixture on the activated carbon, and avoid the blockage of the activated carbon pores caused by the direct addition of the poorly water-soluble alcohol amine-modified graphene oxide and carbon nanotubes.

[0020] In some embodiments of the present application, in step (1), the oxygen content of the graphene oxide is 35-45%.

[0021] In some embodiments of the present application, in step (1), the carbon nanotube has a diameter of 2 to 4 nm, a length of not less than 500 μm, and a specific surface area of ​​not less than 450 m 2 / g.

[0022] In some embodiments of the present application, in step (1), the solid content of the olefin-carbon dispersion is 1 to 5 mg / mL, and the solvent is water.

[0023] In some embodiments of the present application, in step (2), the activator is potassium hydroxide, and the amount of potassium hydroxide used is 2 to 3 g relative to 1 L of the olefin-carbon dispersion.

[0024] In some embodiments of the present application, the temperature of the first ultrasonic treatment is 20 to 40° C., and the treatment time is 10 to 60 min.

[0025] In some embodiments of the present application, in step (3), the alcoholamine is at least one of monoethanolamine, diethanolamine and triethanolamine, preferably diethanolamine.

[0026] In some embodiments of the present application, in step (3), the temperature of the second ultrasonic treatment is 70 to 90° C., and the treatment time is 2 to 6 hours.

[0027] In some embodiments of the present application, in step (3), relative to 1 L of the olefin-carbon dispersion, the amount of the activated carbon used is 0.1 to 0.3 kg, and the amount of the alcoholamine used is 60 to 110 mL.

[0028] In some embodiments of the present application, in step (4), the solid-liquid separation method includes screen filtration, and the solvent used for washing is water.

[0029] In some embodiments of the present application, in step (4), the drying temperature is 100 to 300° C., and the drying time is 2 to 12 hours.

[0030] In a third aspect, the present application provides the application of the SO3 adsorbent described in the first aspect of the present application in removing SO3 from flue gas.

[0031] In some embodiments of the present application, the application includes: introducing the flue gas to be treated into a fixed bed device filled with the SO3 adsorbent, so that the flue gas to be treated contacts with the SO3 adsorbent to obtain desulfurized flue gas.

[0032] Furthermore, the SO3 adsorbent concentration in the flue gas to be treated is not less than 100 mg / m 3 .

[0033] Furthermore, relative to 1 kg of the SO3 adsorbent, the amount of the flue gas to be treated is 100 to 600 m 3 , the temperature of the flue gas to be treated is 60-200°C.

[0034] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. DETAILED DESCRIPTION

[0035] The following describes the implementation of the present application in detail. The implementation described below is exemplary and is only used to explain the present application, and cannot be understood as limiting the present application.

[0036] The "range" disclosed in the present application is defined in the form of a lower limit and / or an upper limit, and a given range is defined by selecting a lower limit and / or an upper limit. The range defined in this way can be inclusive or exclusive of end values, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form an unclearly recorded range, and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, each separately disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0037] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0038] Traditional SO3 adsorbents are divided into alkaline adsorbents (NaHSO3, NaCO3, natural alkali, etc.), activated carbon, etc. Alkaline adsorbents are only effective for adsorbing low concentrations of SO3, and their removal efficiency for SO3 is relatively low. Activated carbon is usually used for the adsorption of SO2. Although it also has a certain adsorption capacity for SO3, its adsorption efficiency is too low. Related technologies mention the use of metal halides and alkali metal hydroxides to modify activated carbon to improve its adsorption capacity for SO3. However, the initial concentration of SO3 in the flue gas treated by the modified activated carbon obtained by this method is not higher than 50 mg / m 3 Moreover, the removal efficiency of SO3 decreased significantly after 10 minutes of adsorption treatment, and it cannot be effectively used in the treatment process of high-concentration SO3 flue gas.

[0039] Accordingly, the first aspect of the present application provides a SO3 adsorbent, comprising activated carbon and an olefin-carbon mixture supported thereon, wherein the olefin-carbon mixture comprises amine-modified graphene oxide and carbon nanotubes.

[0040] According to the present application, the activated carbon can be selected from various activated carbons for exhaust gas adsorption, such as wood activated carbon, coconut shell activated carbon or coal activated carbon, and the shape of the activated carbon can be granular or columnar, and the particle size of the activated carbon can usually be 1 to 10 mm. It should be understood that the particle size of the columnar activated carbon refers to the diameter (φ) of the column.

[0041] In some embodiments, the iodine value of the activated carbon is not less than 800 mg / g, for example ≥800 mg / g, ≥900 mg / g, ≥1000 mg / g, etc., and can be further selected from 800 to 1200 mg / g, such as between 800 and 900 mg / g, between 1000 and 1100 mg / g, etc.; the specific surface area of ​​the activated carbon can be 500 to 1500 m2 / g, for example 600m 2 / g、700m 2 / g、900m 2 / g, 950m 2 / g、1000m 2 / g、1200m 2 / g, etc.; the particle size of the activated carbon is 3-9 mm, such as 3 mm, 4 mm, 5 mm, 5.5 mm, 7 mm, etc. Thus, the adsorbent can meet industrial application requirements while improving the adsorption effect on SO3.

[0042] As a preferred example, the activated carbon is a columnar coal-based activated carbon. In addition, the columnar coal-based activated carbon can be obtained commercially, for example, the columnar coal-based activated carbon selected from Ningxia Tingyuan Guomu Energy Technology Co., Ltd. has a diameter of 3 to 9 mm and a specific surface area of ​​780 to 1100 m 2 / g series of columnar coal-based activated carbon.

[0043] According to the present application, the olefin-carbon mixture is specifically loaded on the surface of the pore structure of the activated carbon, which can effectively improve the adsorption capacity of SO3. Among them, the graphene oxide modified by alcoholamine can be a product formed by the ring-opening reaction between the amino group and the amine group in the alcoholamine and the epoxy group provided by the graphene oxide, which realizes the immobilization of the alcoholamine on the graphene oxide and introduces hydroxyl groups (-OH), and the introduction of carbon nanotubes not only provides more adsorption sites, but also improves the bonding strength between the activated carbon and the graphene oxide modified by alcoholamine.

[0044] In some embodiments, the alcoholamine-modified graphene oxide is at least one of monoethanolamine-modified graphene oxide, diethanolamine-modified graphene oxide and triethanolamine-modified graphene oxide. Preferably, the alcoholamine-modified graphene oxide is diethanolamine-modified graphene oxide.

[0045] In addition, the alcoholamine-modified graphene oxide can be synthesized by reacting alcoholamine and activated graphene oxide in the presence of water at high temperature (eg, 70-90° C.), and the specific method is as described in the second aspect of the present application and will not be repeated here.

[0046] According to some embodiments, the mass ratio of the activated carbon to the olefin-carbon mixture is 100:(0.2-2), such as 100:0.3, 100:0.4, 100:0.5, 100:0.7, 100:1, 100:1.5, etc. Preferably, the mass ratio of the activated carbon to the olefin-carbon mixture is 100:(0.3-1).

[0047] In some embodiments, in the olefin-carbon mixture, the mass ratio of the alcoholamine-modified graphene oxide to the carbon nanotube is (1-4):1, such as 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 4:1, etc. Preferably, the mass ratio of the alcoholamine-modified graphene oxide to the carbon nanotube is (1.5-3):1.

[0048] In the present application, the component content can be calculated based on the feed amount of each component in the adsorbent, wherein the amount of amine-modified graphite oxide is calculated as graphene oxide.

[0049] The second aspect of the present application provides a method for preparing the SO3 adsorbent described in the first aspect of the present application, the method comprising:

[0050] (1) dispersing graphene oxide (GO) and carbon nanotubes (CNTs) uniformly in a solvent to obtain an olefin-carbon dispersion;

[0051] (2) mixing the graphene-carbon dispersion with an activator and performing a first ultrasonic treatment to activate the graphene oxide and the carbon nanotubes to obtain a reaction solution;

[0052] (3) mixing the reaction solution, alcoholamine and activated carbon and subjecting the mixture to a second ultrasonic treatment, so that the alcoholamine modifies the activated graphene oxide to form alcoholamine-modified graphene oxide, thereby obtaining a mixed solution;

[0053] (4) The mixed liquid is subjected to solid-liquid separation, washing and drying to obtain a SO3 adsorbent.

[0054] According to the present application, in step (1), in order to improve the mixing and stability of the carbon dispersion, it is preferred to use a high-pressure homogenizer to disperse the graphene oxide and carbon nanotubes in a solvent, and the dispersion can be carried out at room temperature. As some examples, the operating pressure of the high-pressure homogenizer is not less than 100MPa, such as 100MPa, 120MPa. In addition, the number of homogenization and dispersion can be 2 to 5 times, such as 2 times, 3 times, 4 times, etc., and the possibility of solid particles agglomerating can be reduced by multiple homogenization and dispersion, and nanoscale (D 50 <1μm) olefin-carbon dispersion.

[0055] In step (1), the graphene oxide used as a raw material not only has a high specific surface area, but also contains a large number of oxygen-containing functional groups (such as epoxy groups, carboxyl groups, etc.), which provide reaction sites for graphene oxide, which is conducive to the amine modification of graphene oxide. According to some embodiments, the oxygen content of the graphene oxide is 35-45%, for example, 35%, 38%, 40%, 41%, 42%, 45%, etc. The oxygen content can be measured according to X-ray photoelectron spectroscopy (XPS).

[0056] In step (1), the graphene oxide can be prepared, for example, by methods well known in the art, such as the Hummers method.

[0057] In some embodiments, the carbon nanotubes used as raw materials may have a diameter of 2 to 4 nm, a length of not less than 500 μm, and a specific surface area of ​​not less than 450 m 2 / g. Thus, the bonding strength between the olefin-carbon mixture and the activated carbon can be further improved.

[0058] In some embodiments, the solid content of the carbon-olefin dispersion (ie, the total content of GO and CNTs) may be 1 to 5 mg / mL, such as 1 mg / mL, 2 mg / mL, 3 mg / mL, and the like.

[0059] In some embodiments, in the olefin-carbon dispersion, the mass ratio of the graphene oxide to the carbon nanotubes is (1-4):1, such as 1:1, 2:1, 2.5:1, 3:1, 4:1, etc. Preferably, the mass ratio of the graphene oxide to the carbon nanotubes is (1.5-3):1.

[0060] According to the present application, in step (2), the chemical activity of the surface of the carbon material (GO, CNTs) can be increased by activation treatment, prompting the carbon material to generate a large number of micropores and mesopores, further increasing the specific surface area of ​​the carbon material.

[0061] In some embodiments, the activator is potassium hydroxide (KOH), and the amount of potassium hydroxide used is 2 to 3 g, such as 2.1 g, 2.2 g, 2.3 g, 2.2 g, 2.4 g, 2.8 g, etc., relative to 1 L of the olefin-carbon dispersion.

[0062] In some embodiments, the temperature of the first ultrasonic treatment can be 20-40°C, such as 25°C, 28°C, 30°C, etc.; the time of the first ultrasonic treatment can be 10-60 min, such as 20 min, 30 min, 35 min, 50 min, 60 min, etc.

[0063] As some examples, the frequency of the first ultrasonic treatment may be 30-50 kHz, for example 40 kHz.

[0064] According to the present application, in step (3), the second ultrasonic treatment can, on the one hand, allow the alcoholamine to react with graphene oxide to form alcoholamine-modified graphene oxide, and on the other hand, achieve uniform loading of the olefin-carbon mixture on the activated carbon. The activated carbon is as described in the first aspect of the present application.

[0065] In some embodiments, relative to 1L of the olefin-carbon dispersion, the amount of the activated carbon may be 0.1-0.3kg, for example, 0.12kg, 0.14kg, 0.15kg, 0.2kg, 0.22kg, 0.23kg, 0.25kg, 0.28kg, etc.

[0066] In some embodiments, the mass ratio of the activated carbon to the olefin-carbon mixture (ie, a mixture of GO and CNTs) in the olefin-carbon dispersion may be 100:(0.2-2), preferably 100:(0.3-1).

[0067] In some embodiments, the temperature of the second ultrasonic treatment is 70 to 90°C, such as 80°C, 90°C, etc.; the time of the second ultrasonic treatment is 2 to 6 hours, such as 3 hours, 4 hours, 5 hours, 6 hours, etc. High-temperature ultrasound can not only achieve the modification of GO by alcoholamine, but also promote the good dispersion and attachment of carbon materials to the inner surface of activated carbon pores, thereby improving its adsorption capacity. In addition, the frequency of the second ultrasonic treatment can be 30 to 50kHz, such as 40kHz. The ultrasonic treatment reaction system can be carried out in a closed or semi-closed space, so as to reduce solvent volatilization and achieve high-temperature reflux to improve the modification effect.

[0068] In step (3), the alcoholamine may be at least one of monoethanolamine (MEA), diethanolamine (DEA) and triethanolamine (TEA), preferably diethanolamine.

[0069] In some embodiments, relative to 1 L of the olefin-carbon dispersion, the amount of the alcoholamine used is 60-110 mL, for example, 60 mL, 75 mL, 80 mL, 85 mL, 90 mL, 100 mL, 105 mL, 108 mL, etc.

[0070] According to the present application, a high-purity solid SO3 adsorbent can be obtained through the post-treatment process of step (4).

[0071] In some embodiments, the solid-liquid separation method includes screen filtration, and the solvent used for washing is water. Unreacted raw materials (such as activators and alcohol amines) can be removed by washing, and the washing method may include, for example, washing the solid product with water until the pH of the washing liquid is 8 to 10.

[0072] In step (4), the drying may be, for example, high temperature oven drying, spray drying, freeze drying, etc., preferably oven drying.

[0073] In some embodiments, the drying temperature is 100-300°C, such as 150°C, 180°C, 200°C, 250°C, etc., and the drying time can be 2-12h, such as 4h, 5h, 6h, 8h, 10h, etc.

[0074] The third aspect of the present application provides the use of the SO3 adsorbent described in the first aspect of the present application in removing SO3 from flue gas.

[0075] In some embodiments, the method should include: introducing the flue gas to be treated into a fixed bed device filled with the SO3 adsorbent, so that the flue gas to be treated contacts the SO3 adsorbent to obtain desulfurized flue gas. The SO3 adsorbent is filled into a fixed bed to realize industrial treatment of flue gas, and the treatment process is simple.

[0076] According to the present application, the flue gas to be treated may be flue gas with a low concentration of SO3 (for example, a SO3 concentration not higher than 50 mg / m 3 ), or flue gas with high concentration of SO3. In particular, when the flue gas with high concentration of SO3 is continuously treated, the adsorbent can maintain a high desulfurization efficiency for a long time. As some examples, the SO3 concentration in the flue gas to be treated is not less than 100 mg / m 3 , and further can be 100 to 1000 mg / m 3 , for example 500mg / m 3 , 550mg / m 3 , 600mg / m 3 , 800mg / m 3 wait.

[0077] As some examples, the flue gas with high SO 3 concentration may be the flue gas at the SCR outlet when high-sulfur coal is burned.

[0078] In some embodiments, the amount of the flue gas to be treated is 100-600 m3 relative to 1 kg of the SO3 adsorbent. 3 The temperature of the flue gas to be treated is 60-200°C, such as 70°C, 80°C, 100°C, 150°C, 170°C, etc. In addition, the flow rate of the flue gas can be 1-5m 3 / min, for example 1m 3 / min、2m 3 / min、3m 3 / min, etc.

[0079] The following describes embodiments of the present application. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application.

[0080] In the following examples and comparative examples,

[0081] Carbon nanotubes were purchased from Jiangsu Tiannai Technology Co., Ltd. with a brand name of FT-2000.

[0082] The activated carbon was coal-based columnar activated carbon purchased from Ningxia Tingyuan Guomu Energy Technology Co., Ltd. (iodine value ≥ 1000 mg / g, specific surface area 1000 m 2 / g, diameter is 3mm).

[0083] Preparation Example 1

[0084] This preparation example is used to illustrate the preparation method of graphene oxide used in the following examples and comparative examples.

[0085] Graphene oxide was prepared by the Hummers method: 460 mL of concentrated sulfuric acid (H2SO4, concentration of 98 wt%) was added to a beaker, and the mixture was stirred in an ice bath. After the temperature cooled to 0°C, 20 g of graphite and 10 g of sodium nitrate (NaNO3) were slowly added to the concentrated sulfuric acid, and stirred vigorously for 50 min to mix evenly. A total of 60 g of potassium permanganate (KMnO4) was added in batches (5 g was added every 10 min). After the addition of KMnO4 was completed, the reaction was moved to a water bath, and the reaction was controlled at 32-37°C and stirred continuously. Stir for 30 minutes; then add 1000mL of water, raise the temperature to 98°C, continue stirring at this temperature for 15 minutes, then slowly add warm water to dilute the reaction solution to 3000mL, then pour 370mL of hydrogen peroxide (H2O2, 5wt%) to reduce the excess KMnO4 in the solution, filter, and wash the resulting precipitate with dilute hydrochloric acid and water to obtain graphite oxide, then add water to the graphite oxide, control the solid content to 1g / L, and ultrasonically treat for 60 minutes to obtain a dispersion of graphene oxide, which is freeze-dried to obtain graphene oxide. XPS test shows that the oxygen content of graphene oxide is 40%.

[0086] Example 1

[0087] Graphene oxide and carbon nanotubes were mixed in a mass ratio of 2:1, diluted with water, and dispersed at high speed using a high-pressure homogenizer at room temperature. The operating pressure was controlled at 100 MPa and the homogenization times were 3 times to obtain a 2 mg / mL graphene-carbon dispersion.

[0088] 6.5L of olefin-carbon dispersion was placed in a tank ultrasonic machine, 15.5g of potassium hydroxide was added, and ultrasonic treatment was performed at 25°C and 40kHz for 30min to activate GO and CNTs to obtain a reaction solution; 500mL of MEA and 1.5kg of activated carbon were added to the reaction solution, the temperature was raised to 80°C, and ultrasonic reaction was continued at 40kHz for 3h to form MEA-modified GO (GO-MEA), and a mixed solution containing olefin-carbon (GO-MEA+CNTs) modified activated carbon was obtained; the mixed solution was filtered through a sieve and washed with water in turn, and the crude product was placed in an oven and dried at 180°C for 6h to obtain a SO3 adsorbent, which was recorded as A-1.

[0089] Example 2

[0090] Graphene oxide and carbon nanotubes were mixed in a mass ratio of 2:1, diluted with water, and dispersed at high speed at room temperature using a high-pressure homogenizer, with the operating pressure controlled at 100 MPa and the homogenization times being 3 times to obtain a 2 mg / mL graphene-carbon dispersion;

[0091] 7L of olefin-carbon dispersion was placed in a tank ultrasonic machine, 20g of potassium hydroxide was added, and ultrasonic treatment was performed at 25°C and 40kHz for 60min to activate GO and CNTs to obtain a reaction solution; 600mL of DEA and 2kg of activated carbon were added to the reaction solution, the temperature was raised to 80°C, and at this temperature, ultrasonic reaction was performed at 40kHz for 3h to form DEA-modified GO (GO-DEA), and a mixed solution containing olefin-carbon (GO-DEA+CNTs) modified activated carbon was obtained; the mixed solution was filtered through a sieve and washed with water in turn, and the crude product was placed in an oven and dried at 270°C for 6h to obtain a SO3 adsorbent, which was recorded as A-2.

[0092] Example 3

[0093] Graphene oxide and carbon nanotubes were mixed in a mass ratio of 2:1, diluted with water, and dispersed at high speed using a high-pressure homogenizer at room temperature, with the operating pressure controlled at 100 MPa and the homogenization times being 3 times to obtain a 1 mg / mL graphene-carbon dispersion;

[0094] 6.5L of olefin-carbon dispersion was placed in a tank-type ultrasonic machine, 18g of potassium hydroxide was added, and ultrasonic treatment was performed at 25°C and 40kHz for 40min to activate GO and CNTs to obtain a reaction solution; 700mL of TEA and 1.5kg of activated carbon were added to the reaction solution, the temperature was raised to 85°C, and at this temperature, ultrasonic reaction was continued at 40kHz for 5h to form TEA-modified GO (GO-TEA), and a mixed solution containing olefin-carbon (GO-DEA+CNTs) modified activated carbon was obtained; the mixed solution was filtered through a sieve and washed with water in turn, and the crude product was placed in an oven and dried at 200°C for 8h to obtain a SO3 adsorbent, which was recorded as A-3.

[0095] Embodiments 4 to 6

[0096] The SO3 adsorbent was prepared according to the method of Example 1, except that when preparing the olefin-carbon dispersion, the mass ratio of GO and CNTs was adjusted to 1.5:1, 3:1 and 1:1. The prepared SO3 adsorbents were respectively recorded as A-4, A-5 and A-6.

[0097] Example 7

[0098] A SO3 adsorbent was prepared according to the method of Example 1, except that the amount of activated carbon was adjusted to 0.8 kg. The prepared adsorbent was recorded as A-7.

[0099] Comparative Example 1

[0100] The activated carbon was used as a comparative sample and the adsorbent was recorded as DA-1.

[0101] Comparative Example 2

[0102] The SO3 adsorbent was prepared according to the method of Example 1, except that MEA was not added. The specific operation was as follows:

[0103] 6.5L of olefin-carbon dispersion was placed in a tank ultrasonic machine, 15.5g of potassium hydroxide was added, and ultrasonic treatment was performed at 25°C and 40kHz for 30min to activate GO and CNTs to obtain a reaction solution; 1.5kg of activated carbon was added to the reaction solution, the temperature was raised to 80°C, and ultrasonic treatment was continued at this temperature and 40kHz for 3h to obtain a mixed solution containing olefin-carbon (GO+CNTs) modified activated carbon; the mixed solution was filtered through a sieve and washed with water in turn, and the crude product was placed in an oven and dried at 180°C for 6h to obtain a SO3 adsorbent, recorded as DA-2.

[0104] Comparative Example 3

[0105] The SO3 adsorbent was prepared according to the method of Example 1, except that no carbon nanotubes were added. The specific operation was as follows:

[0106] GO was diluted with water and dispersed at high speed using a high-pressure homogenizer at room temperature. The operating pressure was controlled at 100 MPa and the homogenization times were 3 times to obtain a 2 mg / mL GO dispersion.

[0107] 6.5L GO dispersion was placed in a tank ultrasonic machine, 15.5g potassium hydroxide was added, and ultrasonic treatment was performed at 25°C and 40kHz for 30min to activate GO to obtain a reaction solution; 500mL MEA (510g, 8.3mol) and 1.5kg activated carbon were added to the reaction solution, the temperature was raised to 80°C, and at this temperature, ultrasonic reaction was continued at 40kHz for 3h to form GO-MEA, and a mixed solution containing GO-MEA modified activated carbon was obtained; the mixed solution was filtered through a sieve and washed with water in turn, and the crude product was placed in an oven and dried at 180°C for 6h to obtain a SO3 adsorbent, recorded as DA-3.

[0108] In the above examples and comparative examples, the main raw materials used and their amounts are shown in Table 1.

[0109] Table 1

[0110]

[0111] Note: The loading amount in Examples 1-7 and Comparative Example 2 refers to the mass percentage of the total amount of GO and CNTs used in the activated carbon; Comparative Example 3 refers to the mass percentage of the amount of GO-MEA used in the activated carbon.

[0112] Test Case

[0113] The following test examples are used to illustrate the treatment effects of the adsorbents A-1 to A-7 and DA-1 to DA-3 of the above embodiments and comparative examples on high-concentration flue gas. The flue gas at the outlet of the SCR when a power plant burns high-sulfur coal is used as the flue gas to be treated. After cooling in the scrubber, the main components of the flue gas are shown in Table 2:

[0114] Table 2

[0115] project <![CDATA[Concentration (mg / m 3 )]]> <![CDATA[SO3]]> 537.665 <![CDATA[SO2]]> 42.734 <![CDATA[N2]]> 857661.7 <![CDATA[O2]]> 113511.8 water vapor 32367.433

[0116] Test method: Take 1kg of adsorbent and load it into the desulfurization tank equipment to form a fixed bed. The 80℃ flue gas to be treated is introduced from the bottom of the equipment. The flue gas flow rate is controlled to be 2m 3 / min, the flue gas introduction time is 240min, during which the flue gas at the outlet of the collection equipment is collected through a gas collection bag at regular intervals, and the SO3 concentration in the flue gas at the outlet (also known as SO3 penetration concentration) is tested using a SO3 desktop detector, and the desulfurization efficiency is calculated according to the following formula:

[0117] Desulfurization efficiency = [(C0-C t ) / C0]×100%, where

[0118] C0 is the initial concentration of SO3 in the flue gas, in mg / m 3

[0119] C t It is the SO3 penetration concentration at a certain time, in mg / m 3 ,

[0120] The test results are shown in Table 3.

[0121] Table 3

[0122]

[0123] Combined with Table 3, by comparing Examples 1-7 with Comparative Examples 1-3, it can be seen that when the adsorbents A-1 to A-7 prepared in Examples 1-7 are used to treat flue gas with high SO3 concentration, the initial desulfurization efficiency after 30 minutes of treatment is above 80%, and after 4 hours of desulfurization treatment, the adsorbent can still maintain a desulfurization efficiency of more than 65%; while when the adsorbents DA-1 to DA-3 of Comparative Examples 1-3 are used to treat high-concentration flue gas, the initial desulfurization efficiency after 30 minutes of treatment is low, and after 4 hours of flue gas treatment, the desulfurization efficiency decreases significantly, indicating that its SO3 adsorption capacity for flue gas with high SO3 concentration is limited.

[0124] It can be seen from Comparative Example 1 that the adsorption capacity of activated carbon as a SO3 adsorbent is limited. During the entire 4h adsorption treatment, the desulfurization efficiency of high-concentration flue gas does not exceed 56%; it can be seen from Comparative Examples 2-3 that although the initial desulfurization efficiency of flue gas can be improved by modifying the activated carbon with carbon nanotubes and amine-modified graphene oxide, the desulfurization efficiency will decrease significantly with the extension of time, and it is impossible to achieve long-term and efficient treatment of SO3 in high-concentration SO3 flue gas.

[0125] In summary, after the activated carbon is modified by an olefin-carbon mixture including amine-modified graphene oxide and carbon nanotubes, the obtained adsorbent has a high SO3 adsorption efficiency, and the adsorbent can maintain a high adsorption activity for a long time when continuously treating high-concentration SO3 flue gas, and has high stability.

[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A SO 3 Adsorbent, It is characterized in that The SO 3 The adsorbent comprises activated carbon and an olefin-carbon mixture loaded thereon, wherein the olefin-carbon mixture comprises alcoholamine-modified graphene oxide and carbon nanotubes.

2. The SO according to claim 1 3 Adsorbent, It is characterized in that The alcoholamine-modified graphene oxide is at least one of monoethanolamine-modified graphene oxide, diethanolamine-modified graphene oxide and triethanolamine-modified graphene oxide, preferably diethanolamine-modified graphene oxide; Preferably, the iodine value of the activated carbon is not less than 800 mg / g, and the specific surface area is 500 to 1500 m 2 / g, particle size is 3 to 9 mm.

3. SO according to claim 1 or 2 3 Adsorbent, It is characterized in that The mass ratio of the activated carbon to the olefin-carbon mixture is 100:(0.2-2), preferably 100:(0.3-1); In the olefin-carbon mixture, the mass ratio of the alcoholamine-modified graphene oxide to the carbon nanotube is (1-4):1, preferably (1.5-3):

1.

4. A method for preparing the SO according to any one of claims 1 to 3 3 Adsorbent method, It is characterized in that The method includes: (1) uniformly dispersing graphene oxide and carbon nanotubes in a solvent to obtain an olefin-carbon dispersion; (2) mixing the graphene-carbon dispersion with an activator and performing a first ultrasonic treatment to activate the graphene oxide and the carbon nanotubes to obtain a reaction solution; (3) mixing the reaction solution, alcoholamine and activated carbon and subjecting the mixture to a second ultrasonic treatment, so that the alcoholamine modifies the activated graphene oxide to form alcoholamine-modified graphene oxide, thereby obtaining a mixed solution; (4) subjecting the mixed solution to solid-liquid separation, washing and drying to obtain SO 3 Adsorbent.

5. The method according to claim 4, It is characterized in that In step (1), the solid content of the olefin-carbon dispersion is 1 to 5 mg / mL, and the solvent is water; Preferably, the oxygen content of the graphene oxide is 35-45%; Preferably, the carbon nanotubes have a diameter of 2-4 nm, a length of not less than 500 μm, and a specific surface area of ​​not less than 450 m 2 / g.

6. The method according to claim 4 or 5, It is characterized in that In step (2), the activator is potassium hydroxide, and the amount of potassium hydroxide used is 2 to 3 g relative to 1 L of the olefin-carbon dispersion; Preferably, the temperature of the first ultrasonic treatment is 20-40° C., and the treatment time is 10-60 min.

7. The method according to any one of claims 4 to 6, It is characterized in that In step (3), the alcoholamine is at least one of monoethanolamine, diethanolamine and triethanolamine, preferably diethanolamine; Preferably, relative to 1L of the olefin-carbon dispersion, the amount of the activated carbon is 0.1-0.3kg, and the amount of the alcoholamine is 60-110mL; Preferably, the temperature of the second ultrasonic treatment is 70-90° C., and the treatment time is 2-6 hours.

8. The method according to any one of claims 4 to 7, Its special feature is that In step (4), the solid-liquid separation method includes screen filtration, and the solvent used for washing is water; Preferably, the drying temperature is 100-300° C., and the drying time is 2-12 hours.

9. The SO according to any one of claims 1 to 3 3 Adsorbents for removing SO from flue gas 3 application.

10. The use according to claim 9, It is characterized in that The application includes: filling the SO 3 In the fixed bed device of the adsorbent, the flue gas to be treated is introduced so that the flue gas to be treated is mixed with the SO 3 The adsorbent is contacted to obtain the desulfurized flue gas; Preferably, the SO in the flue gas to be treated 3 Adsorbent concentration is not less than 100mg / m 3 ; Preferably, relative to 1 kg of the SO 3 The amount of the flue gas to be treated is 100-600m 3 , the temperature of the flue gas to be treated is 60-200°C.

Citation Information

Patent Citations

  • Adsorbing agent for capturing CO2 in flue gas, and preparation method thereof

    CN102658085A

  • Preparation method of low cost graphene / CNTs aerogel for adsorption of heavy metal ions

    CN108905981A

  • Carbon nanotube / graphene / activated carbon composite electrode material and preparation method and application thereof

    CN110797202A

  • Preparation method and application of graphene oxide improved activated carbon

    CN113750967A

  • Nitrogen-doped graphene-carbon nanotube composite catalyst and preparation method thereof

    CN113769774A