Preparation method and detection application of magnetic nanometer enrichment material
By using superparamagnetic ferrooxide cores to coat covalent organic skeleton shells in magnetic solid-phase extraction materials, magnetic nano-enriched materials with high adsorption capacity and selectivity are prepared, and the existing technology is solved The problem of insufficient adsorption capacity and selectivity in the medium has achieved efficient enrichment and purification of macrolide drugs, and is suitable for trace detection of complex samples.
Patent Information
- Application Number
- CN202411206404.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing magnetic solid-phase extraction materials have shortcomings in adsorption capacity, adsorption rate and selectivity, making it difficult to efficiently enrich and purify macrolide drugs in complex samples, especially in trace detection in foods.
Magnetic nano-enriched material prepared by superparamagnetic ferrooxide core coated with covalent organic framework shell, which has a porous and ordered crystal structure, rich boric acid groups, large specific surface area, high adsorption capacity, The adsorption rate is fast and can be reused. It is functionally modified by aldehyde amine condensation and thiol-ene click reaction to form Fe3O4@Tp-PaV@MPBA material.
It realizes efficient selective enrichment and purification of macrolide compounds, is suitable for trace detection in complex samples, the material can be reused more than 8 times, and is suitable for industrial production.
Smart Images

Figure BDA0005019152290000021 
Figure BDA0005019152290000101 
Figure BDA0005019152290000102
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemistry, and in particular to a preparation method and detection application of boric acid functionalized magnetic nano-enriched materials. Background Art
[0002] Magnetic Solid Phase Extraction (MSPE) refers to a solid phase extraction technique that uses magnetic or magnetizable materials as adsorbents. It is simple, fast, efficient, and has high enrichment multiples. It is widely used in sample enrichment and purification. The core factor affecting the efficiency of MSPE enrichment and purification is the selection and preparation of adsorbents. At present, a large number of new materials have been developed at home and abroad for use as MSPE adsorbents, including carbon-based nanomaterials, metal organic frameworks, polydopamine derivatives, etc. However, the above materials face a series of technical difficulties such as low adsorption capacity, slow adsorption rate, and poor selectivity.
[0003] Covalent Organic Framework (COF) is a type of crystalline organic porous material formed by covalent bond connection. It has the characteristics of low density, large specific surface area, and adjustable pore size. It can provide excellent skeleton structure and good mass transfer rate. Boron affinity is a type of specific adsorption, that is, the boric acid group can form cyclic esters with cis-dihydroxy substances under alkaline conditions, and the cyclic esters can be dissociated under acidic conditions. Boric acid modification of the material can greatly improve its selectivity. Therefore, the combination of covalent organic framework and boric acid functionalization modification is expected to greatly improve the adsorption capacity, adsorption rate and selectivity of magnetic solid phase extraction materials.
[0004] Macrolides (MALs) are widely used to treat animal diseases and promote animal growth. They are easily left in animal-derived foods and enter the dining table through the production, processing and consumption chains, thus posing safety risks. Long-term exposure to macrolides can cause allergic reactions, damage to the cochlear nerve, and even serious damage to the liver and kidneys. Detection is an important means to prevent the risk of MALs. However, due to the complex food matrix and the low content of macrolides, the enrichment and purification of target compounds are the key to trace detection.
[0005] Therefore, new adsorbent materials for efficient enrichment and purification of MALs need further research. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one purpose of the present invention is to provide a magnetic nano-enrichment material, which has a porous ordered crystal structure and a large specific surface area, a large adsorption capacity, a fast adsorption rate, a high adsorption selectivity, and can be reused. It can selectively and efficiently enrich and purify macrolide drugs in complex samples, which is conducive to the trace detection of macrolide substances in complex food samples.
[0007] According to one aspect of the present invention, the present invention provides a magnetic nano-enriched material. According to an embodiment of the present invention, the magnetic nano-enriched material comprises: a core body, the core body is composed of superparamagnetic ferroferric oxide; and a shell, the shell is coated on at least part of the surface of the core body, and the shell is composed of a repeating unit shown in Formula I.
[0008]
[0009] According to the nano-enrichment material of the embodiment of the present invention, the shell has a porous ordered crystal structure and abundant boric acid groups, and has a large specific surface area and adsorption capacity, a fast adsorption rate, and high adsorption selectivity for compounds containing cis-dihydroxy structures, such as macrolide compounds. In addition, the nano-enrichment material according to the embodiment of the present invention has good dispersibility in water, strong magnetism, and is reusable. It is suitable for complex samples, such as selective and efficient enrichment and purification of macrolide drugs in food, especially trace detection of macrolide substances in complex samples.
[0010] In addition, the magnetic nano-enriched material according to the above embodiment of the present invention may also have the following additional technical features:
[0011] According to an embodiment of the present invention, the average particle size of the core is 150-250 nm, and the shell is a porous mesh structure.
[0012] According to an embodiment of the present invention, the average adsorption pore diameter of the shell is 3-5 nm, and the thickness is 40-60 nm.
[0013] According to an embodiment of the present invention, the specific surface area of the magnetic nano-enriched material is 120-180 m 2 / g.
[0014] According to an embodiment of the present invention, the magnetic strength of the magnetic nano-enriched material is 35-45emu / g.
[0015] According to an embodiment of the present invention, the magnetic nano-enriched material can be reused more than 8 times.
[0016] According to an embodiment of the present invention, the magnetic nano-enriched material has crystal diffraction peaks at 2θ of 4.7°, 30.2°, 35.4°, 43.1°, 53.8°, 57.2° and 62.8° in X-ray powder diffraction data.
[0017] According to another aspect of the present invention, the present invention provides a method for preparing the aforementioned magnetic nano-enriched material. According to an embodiment of the present invention, the method comprises: providing aminated ferroferric oxide magnetic nanoparticles; contacting the aminated ferroferric oxide magnetic nanoparticles with an aldehyde monomer, and premixing in a first solvent to obtain a premixed solution; contacting the premixed solution with the amino monomer to perform an aldehyde-amine condensation reaction to obtain an enriched material intermediate; and contacting the enriched material intermediate with 4-mercaptophenylboronic acid (4-MPBA), and performing a thiol-ene click reaction in a second solvent to functionalize and modify the enriched material intermediate to obtain the magnetic nano-enriched material.
[0018] The magnetic nano-enriched material prepared by the preparation method of the embodiment of the present invention has the advantages of large specific surface area, large adsorption capacity, fast adsorption rate, and high adsorption selectivity for compounds containing cis-dihydroxy structures, such as macrolide compounds. In addition, the preparation method has simple and efficient steps, mild reaction conditions, and is suitable for industrial production.
[0019] According to an embodiment of the present invention, the method for preparing the amino-iron tetroxide magnetic nanoparticles includes: dispersing ferric chloride hexahydrate in ethylene glycol and performing a first ultrasonic treatment to obtain a first mixed solution; contacting the first mixed solution with anhydrous sodium acetate and performing a first stirring to obtain a second mixed solution; contacting the second mixed solution with 1,6-hexanediamine and performing a second stirring to obtain a third mixed solution; and heating the second mixed solution in a reactor to obtain the amino-iron tetroxide magnetic nanoparticles.
[0020] According to an embodiment of the present invention, the mass ratio of ferric chloride hexahydrate, anhydrous sodium acetate and 1,6-hexanediamine is 1:(1-3):(5-7), preferably, the mass ratio is 1:2:6.5.
[0021] According to an embodiment of the present invention, the temperature of the heating treatment is 180-220° C., preferably 200° C., and the time is 6-8 hours, preferably 7 hours.
[0022] According to an embodiment of the present invention, the amino monomer is 1,4-diamino-2,5-divinylbenzene (PaV), and the aldehyde monomer is trialdehyde phloroglucinol (Tp).
[0023] According to an embodiment of the present invention, the mass ratio of the aldehyde monomer, the amino monomer and the amino-treated ferroferric oxide magnetic nanoparticles is 1:(0.5-1.5):(2-4), preferably, the mass ratio is 1:1.14:2.86.
[0024] According to an embodiment of the present invention, the initiator of the thiol-ene click reaction is azobisisobutyronitrile (AIBN).
[0025] According to an embodiment of the present invention, the mass ratio of the initiator, 4-mercaptophenylboric acid and the enrichment material intermediate is 1:(10-15):(10-15), preferably, 1:12:13.3.
[0026] According to an embodiment of the present invention, the reaction temperature of the thiol-ene click reaction is 50-70° C., preferably 65° C., and the reaction time is optionally 10-16 hours, preferably 14 hours.
[0027] According to an embodiment of the present invention, the first solvent is a mixed solution of 1,4-dioxane and mesitylene, and the volume ratio of 1,4-dioxane to mesitylene is 1:(0.9-1.1).
[0028] According to an embodiment of the present invention, the second solvent is an ethanol-water solution, wherein the volume ratio of ethanol to water is 1:(2-5), preferably, 1:3.
[0029] According to an embodiment of the present invention, the catalyst for the aldehyde-amine condensation reaction is acetic acid.
[0030] According to an embodiment of the present invention, the volume ratio of the acetic acid to the first solvent is 1:(25-35), preferably, 1:28.
[0031] According to an embodiment of the present invention, the reaction time of the aldehyde-amine condensation reaction is 48-84 hours, preferably, the reaction time is 72 hours.
[0032] According to another aspect of the present invention, the present invention provides a method for adsorbing macrolide compounds. According to an embodiment of the present invention, the method is carried out using the aforementioned magnetic nano-enrichment material. Thus, since the aforementioned magnetic nano-enrichment material has the advantages of large specific surface area, large adsorption capacity, fast adsorption rate, and high adsorption selectivity for compounds containing cis-dihydroxy structures, such as macrolide compounds, the method for adsorbing macrolide compounds in the embodiment of the present invention has a fast adsorption rate for macrolide compounds, a large adsorption amount, and a short time to reach adsorption equilibrium. The method is suitable for complex samples, such as selective and efficient enrichment and purification of macrolide drugs in food, especially trace detection of macrolide substances in complex samples.
[0033] According to an embodiment of the present invention, the macrolide compound is at least one selected from toramectin (TUL), spiramycin (SPI), azithromycin (AZI), gaminomycin (GAM), tylosin (TYL), clarithromycin (CLA) and roxithromycin (ROX).
[0034] According to an embodiment of the present invention, the adsorption capacity of the magnetic nano-enriched material is 18-45 mg / g.
[0035] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0037] Figure 1 The scanning electron microscope and transmission electron microscope schematic diagrams of the magnetic nano-enriched material according to one embodiment of the present invention are shown, wherein (A) the scanning electron microscope image of Fe3O4-NH2, (B) the scanning electron microscope image of Fe3O4@Tp-PaV, (C) the scanning electron microscope image of Fe3O4@Tp-PaV@MPBA, (D) the transmission electron microscope image of Fe3O4-NH2, (E) the transmission electron microscope image of Fe3O4@Tp-PaV, and (F) the transmission electron microscope image of Fe3O4@Tp-PaV@MPBA;
[0038] Figure 2 The X-ray diffraction patterns of the magnetic nano-enriched materials according to one embodiment of the present invention are shown, wherein (A) is a conventional X-ray diffraction pattern, wherein (a) Fe3O4-NH2, (b) Fe3O4@Tp-PaV, (c) Fe3O4@Tp-PaV@MPBA; (B) is a small-angle X-ray diffraction pattern of Fe3O4@Tp-PaV@MPBA;
[0039] Figure 3 shows infrared spectra of magnetic nano-enriched materials according to one embodiment of the present invention, including (a) Fe3O4-NH2, (b) Fe3O4@Tp-PaV and (c) Fe3O4@Tp-PaV@MPBA;
[0040] Figure 4 shows X-ray photoelectron spectra of magnetic nano-enriched materials according to one embodiment of the present invention, including (a) Fe3O4-NH2, (b) Fe3O4@Tp-PaV and (c) Fe3O4@Tp-PaV@MPBA;
[0041] Figure 5shows the hysteresis loop diagram of the magnetic nano-enriched material according to one embodiment of the present invention, wherein (a) Fe3O4-NH2 and (b) Fe3O4@Tp-PaV@MPBA;
[0042] Figure 6 A schematic diagram showing the characterization results of the pore size distribution and specific surface area of the nitrogen adsorption and desorption isotherm experimental line of the magnetic nano-enriched material according to an embodiment of the present invention, wherein (A) is a nitrogen isotherm adsorption and desorption curve diagram of Fe3O4-NH2 and Fe3O4@Tp-PaV@MPBA; (B) is a pore size distribution diagram of Fe3O4@Tp-PaV@MPBA;
[0043] Figure 7 The figure shows the static and dynamic adsorption test results of 7 macrolides by the magnetic nano-enrichment material according to one embodiment of the present invention, wherein (A) is an adsorption isotherm curve and (B) is an adsorption kinetic curve;
[0044] Figure 8 A schematic diagram showing the recovery rates of Fe3O4@Tp-PaV@MPBA and Fe3O4@Tp-PaV for the adsorption of 7 macrolides according to an embodiment of the present invention is shown;
[0045] Fig. 9 A schematic diagram showing the number of times Fe3O4@Tp-PaV@MPBA can be reused according to one embodiment of the present invention. DETAILED DESCRIPTION
[0046] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0047] In the description of the present invention, the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and do not require that the present invention must be constructed and operated in a specific orientation. Therefore, they should not be understood as limitations on the present invention.
[0048] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.
[0049] According to one aspect of the present invention, the present invention provides a magnetic nano-enriched material. According to the nano-enriched material of the embodiment of the present invention, the shell has a porous ordered crystal structure and abundant boric acid groups, and has a large specific surface area. In some embodiments, the specific surface area can reach 155.72 m 2 / g; large adsorption capacity, in some embodiments, the adsorption capacity is 19-37mg / g; fast adsorption rate, in some embodiments, 2mL 25mg / L macrolide can reach adsorption equilibrium in 10min; high adsorption selectivity for compounds containing cis-dihydroxy structures, such as macrolide compounds. In addition, the nano-enrichment material according to the embodiment of the present invention has good dispersibility in water, strong magnetism, and can be reused, which is suitable for complex samples, such as selective and efficient enrichment and purification of macrolide drugs in food, especially trace detection of macrolide substances in complex samples.
[0050] According to an embodiment of the present invention, the magnetic nano-enriched material includes: a core body, which is composed of superparamagnetic ferroferric oxide; and a shell, which covers at least a portion of the surface of the core body, and the shell is composed of a repeating unit shown in Formula I.
[0051] According to an embodiment of the present invention, the average particle size of the core is 150-250 nm, and the shell is a porous mesh structure. Therefore, the specific surface area of the magnetic nano-enriched material is large.
[0052] According to an embodiment of the present invention, the average adsorption pore size of the shell is 3-5nm, preferably, the average adsorption pore size is 3.92-4.50nm, and the thickness is 40-60nm. Thus, the greater the shell thickness, the more the number of layers between the surface shell material repeating unit (Formula I), the greater the adsorption capacity, the better the adsorption effect of macrolides, and, when the average adsorption pore size is 3-5nm, it is suitable for the adsorption of adsorption pores and macrolide compounds, and the adsorption pores have a confined effect on the macromolecular matrix with a particle size greater than 4.50nm, and when the average adsorption pore size is 3.92-4.50nm, the anti-matrix interference ability of the magnetic nano-enriched material adsorption can be further improved.
[0053] According to an embodiment of the present invention, the specific surface area of the magnetic nano-enriched material is 120-180 m 2 / g. Therefore, the specific surface area is large and the adsorption capacity is large.
[0054] According to an embodiment of the present invention, the magnetic intensity of the magnetic nano-enriched material is 35-45emu / g. Thus, under the condition of this magnetic intensity, the magnetic nano-enriched material can produce a strong reaction to the external magnetic field, providing a basis for the rapid implementation of magnetic solid phase extraction. Thereby achieving rapid separation of the magnetic nano-enriched material and the sample matrix, shortening the operation time, and at the same time, the magnetic nano-enriched material has a shorter analyte diffusion distance in the sample solution, thereby improving the adsorption efficiency.
[0055] According to an embodiment of the present invention, the magnetic nano-enriched material can be reused more than 8 times, thereby having a large number of reuse times and a low use cost.
[0056] According to an embodiment of the present invention, the magnetic nano-enriched material has crystal diffraction peaks at 2θ of 4.7°, 30.2°, 35.4°, 43.1°, 53.8°, 57.2° and 62.8° in X-ray powder diffraction data.
[0057] According to another aspect of the present invention, the present invention provides a method for preparing the aforementioned magnetic nano-enriched material. According to an embodiment of the present invention, the method comprises: providing aminated ferroferric oxide magnetic nanoparticles; contacting the aminated ferroferric oxide magnetic nanoparticles with an aldehyde monomer, and premixing in a first solvent to obtain a premixed solution; contacting the premixed solution with the amino monomer to perform an aldehyde-amine condensation reaction to obtain an enriched material intermediate; and contacting the enriched material intermediate with 4-mercaptophenylboronic acid (4-MPBA), and performing a thiol-ene click reaction in a second solvent to functionalize and modify the enriched material intermediate to obtain the magnetic nano-enriched material.
[0058] The magnetic nano-enriched material prepared by the preparation method of the embodiment of the present invention has the advantages of large specific surface area, large adsorption capacity, fast adsorption rate, and high adsorption selectivity for compounds containing cis-dihydroxy structures, such as macrolide compounds. In addition, the preparation method has simple and efficient steps, mild reaction conditions, and is suitable for industrial production.
[0059] According to an embodiment of the present invention, the method for preparing the amino-iron tetroxide magnetic nanoparticles includes: dispersing ferric chloride hexahydrate in ethylene glycol and performing a first ultrasonic treatment to obtain a first mixed solution; contacting the first mixed solution with anhydrous sodium acetate and performing a first stirring to obtain a second mixed solution; contacting the second mixed solution with 1,6-hexanediamine and performing a second stirring to obtain a third mixed solution; and heating the second mixed solution in a reactor to obtain the amino-iron tetroxide magnetic nanoparticles.
[0060] According to an embodiment of the present invention, the mass ratio of ferric chloride hexahydrate, anhydrous sodium acetate and 1,6-hexanediamine is 1:(1-3):(5-7), preferably, the mass ratio is 1:2:6.5. Therefore, this ratio is conducive to promoting amino functionalization modification of the Fe3O4 surface;
[0061] According to an embodiment of the present invention, the temperature of the heating treatment is 180-220° C., preferably 200° C., and the time is 6-8 hours, preferably 7 hours. Therefore, under this condition, the Fe3O4-NH2 is completely crystallized and the yield is high.
[0062] According to an embodiment of the present invention, the amino monomer is 1,4-diamino-2,5-divinylbenzene (PaV), and the aldehyde monomer is trialdehyde phloroglucinol (Tp). Wherein, PaV is a C2-symmetric amino monomer, and Tp is a C3-symmetric aldehyde monomer. Thus, by selecting these two symmetry axis monomers, a covalent organic framework material with a good hexagonal unit cell structure can be generated through an aldehyde-amine condensation reaction; at the same time, the carbon-carbon double bond provided by PaV provides a reaction site for subsequent boric acid functionalization, and the hydroxyl group provided by Tp can enhance the hydrophilicity of the material, which is beneficial to the subsequent adsorption of MALs in the aqueous matrix.
[0063] According to an embodiment of the present invention, the mass ratio of the aldehyde monomer, the amino monomer and the amino-ferroferric oxide magnetic nanoparticles is 1: (0.5-1.5): (2-4), preferably, the mass ratio is 1: 1.14: 2.86. The covalent organic framework material formed under this ratio has a good core-shell structure, a large shell thickness, a large adsorption capacity, and a high yield.
[0064] According to an embodiment of the present invention, the initiator of the thiol-ene click reaction is azobisisobutyronitrile (AIBN), thereby having high catalytic efficiency for the thiol-ene click reaction.
[0065] According to an embodiment of the present invention, the mass ratio of the initiator, 4-mercaptophenylboronic acid and the enrichment material intermediate is 1:(10-15):(10-15), preferably 1:12:13.3. Therefore, the click chemistry reaction rate is appropriate and the reaction yield is high under this ratio.
[0066] According to an embodiment of the present invention, the reaction temperature of the thiol-ene click reaction is 50-70° C., preferably 65° C., and the reaction time is 10-16 hours, preferably 14 hours. Thus, the temperature reaction efficiency is high, and the reaction time is conducive to the full progress of the thiol-ene click reaction.
[0067] According to an embodiment of the present invention, the first solvent is a mixed solution of 1,4-dioxane and mesitylene, and the volume ratio of 1,4-dioxane to mesitylene is 1:(0.9-1.1). Thus, Tp and PaV have high solubility in the first solvent, which is conducive to full contact of the reaction system.
[0068] According to an embodiment of the present invention, the second solvent is an ethanol aqueous solution, wherein the volume ratio of ethanol to water is 1: (2-5), preferably 1: 3. Under this ratio, the enrichment material intermediate and 4-mercaptophenylboric acid can be evenly dispersed in the solvent, thereby ensuring sufficient contact of the reaction system and improving the reaction efficiency.
[0069] According to an embodiment of the present invention, the catalyst for the aldehyde-amine condensation reaction is acetic acid, thereby achieving high catalytic efficiency.
[0070] According to an embodiment of the present invention, the volume ratio of the acetic acid to the first solvent is 1: (25-35), preferably 1: 28. This ratio is conducive to uniform dispersion of the COF monomer of the organic framework polymer material, thereby ensuring full contact of the reaction system and improving the reaction efficiency and yield.
[0071] According to an embodiment of the present invention, the reaction time of the aldehyde-amine condensation reaction is 48-84 hours, preferably 72 hours, which is conducive to the full reaction of the amino monomer and the aldehyde monomer, and promotes the growth of COF material crystals.
[0072] According to another aspect of the present invention, the present invention provides a method for adsorbing macrolide compounds. According to an embodiment of the present invention, the method is carried out using the aforementioned magnetic nano-enrichment material. Thus, since the aforementioned magnetic nano-enrichment material has the advantages of large specific surface area, large adsorption capacity, fast adsorption rate, and high adsorption selectivity for compounds containing cis-dihydroxy structures, such as macrolide compounds, the method for adsorbing macrolide compounds in the embodiment of the present invention has a fast adsorption rate for macrolide compounds, a large adsorption amount, and a short time to reach adsorption equilibrium. The method is suitable for complex samples, such as selective and efficient enrichment and purification of macrolide drugs in food, especially trace detection of macrolide substances in complex samples.
[0073] According to an embodiment of the present invention, the macrolide compound is at least one selected from toramectin (TUL), spiramycin (SPI), azithromycin (AZI), gaminomycin (GAM), tylosin (TYL), clarithromycin (CLA) and roxithromycin (ROX).
[0074] According to an embodiment of the present invention, the adsorption capacity of the magnetic nano-enrichment material is 18-45 mg / g, preferably 25-45 mg / g, and more preferably 19-37 mg / g. Therefore, the magnetic nano-enrichment material has a large adsorption capacity and is particularly suitable for the enrichment and purification of macrolides in complex samples.
[0075] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and should not be construed as limiting the present invention.
[0076] The scheme of the present invention will be explained below in conjunction with the examples. Those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. Where specific techniques or conditions are not specified in the examples, the techniques or conditions described in the literature in the art (e.g., reference to "Molecular Cloning Experiment Guide" by J. Sambrook, etc., translated by Huang Peitang, etc., 3rd edition, Science Press) or in accordance with the product instructions are performed. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be purchased commercially, such as those that can be purchased from Illumina.
[0077] Example 1
[0078] According to the method for preparing a magnetic nano-enriched material in an embodiment of the present invention, an aminated ferroferric oxide magnetic nano-enriched material (Fe3O4-NH2) is first prepared, and then trialdehyde phloroglucinol (Tp) and 1,4-diamino-2,5-divinylbenzene (PaV) are used as functional monomers to coat a covalent organic framework (COF) shell on the surface of Fe3O4-NH2 to obtain Fe3O4@Tp-PaV, and finally 4-mercaptophenylboronic acid (4-MPBA) is used for functional modification to obtain Fe3O4@Tp-PaV@MPBA. The specific preparation process is as follows:
[0079] 1. Preparation of Fe3O4-NH2: It was prepared by hydrothermal method. First, 2.0g of ferric chloride hexahydrate was dispersed in 60mL of ethylene glycol, ultrasonicated for 30min, and then 4.0g of anhydrous sodium acetate was added in sequence, and magnetic stirring was performed for 30min to obtain a yellow suspension; then 13g of 1,6-hexanediamine was added, and magnetic stirring was performed for 1h, and then the mixture was transferred to a polytetrafluoroethylene-lined reactor, and the mixture was placed in a muffle furnace at 200℃ for 7 hours to separate the black solid, and the Fe3O4-NH2 was obtained after washing with water and ethanol alternately for 3 times and drying.
[0080] 2. Preparation of Fe3O4@Tp-PaV: 480.0 mg of the above Fe3O4-NH2 and 168.0 mg of Tp were taken in turn, dispersed in 90 mL of 1,4-dioxane / mesitylene (v / v=1:1) solution, ultrasonicated for 30 min, and mechanically stirred in a 110°C oil bath for premixing for 1 h, then 192.0 mg of PaV was added, and finally 3.2 mL of acetic acid was added dropwise to the reaction system using a separatory funnel, and mechanically stirred in a 110°C oil bath for 72 h, with nitrogen protection during the reaction process. After the reaction, magnetic separation was performed, and Fe3O4@Tp-PaV was obtained after alternating washing with water and ethanol for 3 times and drying.
[0081] 3. Preparation of Fe3O4@Tp-PaV@MPBA: 200.0 mg of the above Fe3O4@Tp-PaV and 180.0 mg of 4-MPBA were dispersed in 100 mL of anhydrous ethanol / ultrapure water (v / v=1:3) in turn, ultrasonicated for 30 min, and then 15 mg of azobisisobutyronitrile (AIBN) was slowly added, and mechanically stirred in a 65°C water bath for 14 h. After the reaction, magnetic separation was performed, and the boric acid functionalized magnetic covalent organic framework nano-enriched material Fe3O4@Tp-PaV@MPBA was obtained by alternating washing with water and ethanol for 3 times and drying.
[0082] Example 2
[0083] Detailed characterization experiments were conducted on Fe3O4@Tp-PaV@MPBA prepared in Example 1 and the precursor materials Fe3O4@Tp-PaV and Fe3O4@Tp-PaV@MPBA to demonstrate the successful preparation of the magnetic nano-enriched material and its excellent physical and chemical properties, as follows:
[0084] 1. Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) were used to characterize the morphology of Fe3O4-NH2, Fe3O4@Tp-PaV and Fe3O4@Tp-PaV@MPBA. Figure 1 As shown in the SEM image, the prepared Fe3O4-NH2( Figure 1 (A))、Fe3O4@Tp-PaV( Figure 1 (B)) and Fe3O4@Tp-PaV@MPBA( Figure 1 (C)) has a regular spherical structure and is evenly dispersed; the Fe3O4-NH2 core particle size is about 200nm. After modification, the surface of the sphere becomes smooth, confirming the successful coating of the COF shell; Fe3O4-NH2( Figure 1 (D)) and Fe3O4@Tp-PaV( Figure 1The TEM image of (E) further proves that the COF shell is successfully wrapped on the Fe3O4 surface. The prepared Fe3O4@Tp-PaV@MPBA presents a typical core-shell structure with a shell thickness of about 50nm ( Figure 1 (F)).
[0085] 2. The crystal structures of Fe3O4-NH2, Fe3O4@Tp-PaV and Fe3O4@Tp-PaV@MPBA were analyzed by powder XRD diffraction experiment. The results are as follows: Figure 2 As shown. Figure 2 (A) It can be seen that the diffraction peaks at 2θ of 30.2°, 35.4°, 43.1°, 53.8°, 57.2° and 62.8° can be observed in the XRD spectra of Fe3O4-NH2, Fe3O4@Tp-PaV and Fe3O4@Tp-PaV@MPBA, which are in good agreement with the crystal plane indices (220), (311), (400), (422), (511) and (440) of Fe3O4, proving the successful preparation of Fe3O4-NH2 and that Fe3O4-NH2 still maintains its original crystal structure after gradual modification; Figure 2 (B) shows the small-angle diffraction peak of Fe3O4@Tp-PaV at 4.7°, which is consistent with the crystal plane index (100) of the COF material, confirming that the material has a COF shell with a better crystal structure after modification.
[0086] 3. Fourier transform infrared spectroscopy (FT-IR) was used to characterize the surface functional groups of Fe3O4-NH2, Fe3O4@Tp-PaV and Fe3O4@Tp-PaV@MPBA. Figure 3 a) 581cm –1 and 1610cm –1 There are absorption peaks at all locations, which are attributed to the stretching vibration of Fe-O-Fe and the bending vibration of NH bond, respectively, confirming the successful preparation of Fe3O4-NH2; in the infrared spectrum of Fe3O4@Tp-PaV ( Figure 3 b), respectively at 1271cm -1 and 1590cm -1 The stretching vibration absorption peaks belonging to C=C bond and CN bond were observed at , confirming the successful coating of COF; in the infrared spectrum of Fe3O4@Tp-PaV@MPBA ( Figure 3 c) 1091cm can be observed -1 and 1382cm -1 Two characteristic absorption peaks, which originated from the stretching vibration of CS bond and BO, respectively, confirmed the successful modification of MPBA.
[0087] 4. X-ray photoelectron spectroscopy (XPS) was used to analyze the surface elements of Fe3O4-NH2, Fe3O4@Tp-PaV and Fe3O4@Tp-PaV@MPBA. Figure 4 a As can be seen, the peaks at 711, 532, and 398 eV are attributed to the binding energies of Fe2p, O1s, and N1s, respectively, confirming the successful preparation of Fe3O4-NH2; Figure 4 The peak response at 398 eV was significantly enhanced in b, which was due to the successful coating of the COF shell on the surface of the magnetic core; Figure 4 In c, two peaks at 190 and 163 eV were observed, which were attributed to the binding energies of B1s and S2p, respectively, confirming that MPBA was successfully modified on the COF surface.
[0088] 5. The magnetic properties of Fe3O4-NH2 and Fe3O4@Tp-PaV@MPBA were analyzed using a vibrating sample magnetometer (VSM). Figure 5 As shown in the figure, the coercivity and remanence of the hysteresis curves of Fe3O4-NH2 and Fe3O4@Tp-PaV@MPBA are almost zero, indicating that they both exhibit superparamagnetism. COF encapsulation and subsequent boration modification lead to a decrease in the saturation magnetization of Fe3O4-NH2, but it can still reach 40emu / g, which is sufficient to meet the requirements for separating Fe3O4@Tp-PaV@MPBA from the sample matrix solution. Figure 5 As can be seen from the inset, the prepared Fe3O4@Tp-PaV@MPBA is well dispersed in water and can be quickly separated from the sample matrix solution within 15s under the action of an external magnet.
[0089] 6. The pore size distribution and specific surface area of Fe3O4-NH2 and Fe3O4@Tp-PaV@MPBA were characterized by nitrogen adsorption and desorption isotherms. Figure 6 As shown in (A), Fe3O4@Tp-PaV@MPBA exhibits a typical type IV nitrogen adsorption-desorption isotherm, and its average pore size is approximately 3.92 nm ( Figure 6 (B)), indicating that Fe3O4@Tp-PaV@MPBA has mesoporous structure characteristics. Further calculations show that the specific surface area of Fe3O4@Tp-PaV@MPBA is 155.72m 2 / g, significantly higher than the specific surface area of Fe3O4-NH2 (11.59m 2 / g, proving that the specific surface area of the modified material is greatly improved, which helps to improve the adsorption capacity and efficiency of the material, and has good prospects for its use in the adsorption of macrolides.
[0090] Example 3
[0091] Static and dynamic adsorption experiments were used to study the feasibility of Fe3O4@Tp-PaV@MPBA prepared in Example 1 to adsorb 7 representative macrolide drugs (tolamectin (TUL), spiramycin (SPI), azithromycin (AZI), gaminomycin (GAM), tylosin (TYL), clarithromycin (CLA), roxithromycin (ROX)) with 14-16 rings in complex samples, as follows:
[0092] 1. Static adsorption test
[0093] 2 mL of standard solution of each target with a concentration gradient of 1 mg / L, 2 mg / L, 5 mg / L, 10 mg / L, 15 mg / L, 20 mg / L and 25 mg / L was prepared, and the pH was adjusted to 8. Then 1 mg of Fe3O4@Tp-PaV@MPBA was added and vortexed for 90 min to fully adsorb the target.
[0094] 1.1 Calculation of maximum adsorption capacity
[0095] The maximum adsorption capacity of Fe3O4@Tp-PaV@MPBA for each MALs was calculated by the following formula (1).
[0096] Q=(C0-C e )V / m Formula (1)
[0097] Where, Q is the maximum adsorption capacity (mg / g), C0 is the initial concentration of the adsorption solution (mg / L), and C e is the target concentration (mg / L) when adsorption equilibrium is reached, m is the mass of Fe3O4@Tp-PaV@MPBA (mg), and V is the volume of the adsorption solution (mL).
[0098] Depend on Figure 7 (A) It can be seen that as the solution concentration increases, the adsorption capacity of the magnetic nano-enriched material for each MALs increases, and it approaches saturation when the solution concentration increases to 20 mg / L. According to formula (1), the saturated adsorption capacity of Fe3O4@Tp-PaV@MPBA for TUL, SPI, AZI, GAM, TYL, CLA and ROX are 36.85, 26.84, 33.99, 34.82, 28.47, 19.45 and 28.07 mg / g, respectively. The large adsorption capacity for MALs can be attributed to the large specific surface area and abundant boric acid group adsorption sites of the magnetic nano-enriched material.
[0099] 1.2 Study on adsorption isotherm model
[0100] The adsorption behavior of Fe3O4@Tp-PaV@MPBA on seven MALs was further studied by Langmuir and Freundlich adsorption isotherm models. The Langmuir adsorption isotherm model describes the monolayer adsorption of the target on the outer surface of the adsorbent, and the linear form of its equation is shown in Equation (2).
[0101]
[0102] Among them, C e (mg / L) is the concentration of the target solution at equilibrium; Q e (mg / g) and Q s (mg / g) are the equilibrium adsorption capacity and saturated adsorption capacity, respectively; K L (L / mg) is the Langmuir constant.
[0103] The Freundlich adsorption isotherm model describes multilayer adsorption based on heterogeneous surfaces, and the linear form of its equation is shown in equation (3).
[0104]
[0105] Among them, K F (mg / g) and n are the Freundlich constant and the binding energy constant of Fe3O4@Tp-PaV@MPBA adsorption on 7 MALs, respectively.
[0106] The static adsorption test data were fitted to the Langmuir and Freundlich adsorption isotherm models, and the model-related parameters were calculated. The results are shown in Table 1. It can be seen from the table that the linear fitting coefficients (R 2 )(0.9746-0.9957) are greater than the R of the Freundlich model. 2 (0.7127-0.9052), indicating that the adsorption of Fe3O4@Tp-PaV@MPBA on MALs is more consistent with the characteristics of monolayer adsorption.
[0107] Table 1 Fitting parameters of the adsorption isotherm model of seven macrolide drugs
[0108]
[0109] 2. Dynamic adsorption test
[0110] 2 mL of single-label solution of each MALs (25 mg / L) was prepared, the pH was adjusted to 8, and 1 mg of Fe3O4@Tp-PaV@MPBA was added thereto, and vortexed for different adsorption times (2 min, 5 min, 10 min, 20 min, 30 min, 60 min and 90 min). Figure 7 (B) shows the results of MALs adsorption at different adsorption times. As can be seen from the figure, all MALs can reach adsorption equilibrium in about 10 minutes, confirming that the material has a fast adsorption rate and high efficiency.
[0111] The adsorption kinetics pseudo-first-order and pseudo-second-order models were further used to study the adsorption of MALs by nano-enriched materials.
[0112] The pseudo-first-order model of adsorption kinetics often describes physical adsorption. The adsorption process is only related to the concentration of the target substance and is controlled by the diffusion step. The linear expression of the model is shown in Equation (4).
[0113] In(Q e -Q t )=In Q e -k1t Formula (4)
[0114] The adsorption kinetics pseudo-second-order model is controlled by chemical adsorption. The adsorption process involves electron transfer or sharing between the adsorbent and the adsorbate. The linear expression of the model is shown in Eq. (5).
[0115]
[0116] Among them, Q e (mg g -1 ) and Qt(mg g -1 ) are the adsorption capacity at equilibrium and the adsorption amount at time t, respectively; K1 and K2 are the reaction rate constants of pseudo-first-order and pseudo-second-order reactions, respectively.
[0117] The obtained data were fitted with pseudo-first-order and pseudo-second-order adsorption kinetics models, and the model-related parameters were calculated. The results are shown in Table 2. It can be seen from the table that the R 2 (0.9962-0.9999) are all greater than the pseudo-first-order adsorption kinetics R 2 (0.9115-0.9948), and the theoretical adsorption amount Qe,cal calculated by the quasi-second-order model is close to the saturated adsorption amount Qe obtained in the experiment, indicating that the adsorption of MALs by Fe3O4@Tp-PaV@MPBA is more in line with the kinetic quasi-second-order model and belongs to the chemical adsorption characteristics, which is consistent with the results of the static adsorption test.
[0118] Table 2 Fitting parameters of the adsorption kinetic model of seven macrolide drugs
[0119]
[0120] Example 4
[0121] The adsorption mechanism of Fe3O4@Tp-PaV@MPBA prepared in Example 1 was studied, and the specific experiment is as follows:
[0122] The Fe3O4@Tp-PaV@MPBA and Fe3O4@Tp-PaV prepared in Example 1 were used for the adsorption of seven macrolide drugs, and the recovery rates of each target were calculated. The results are shown in Figure 8 As shown. Figure 8 It can be seen that the recovery rates of Fe3O4@Tp-PaV@MPBA for 7 macrolides are all greater than 80%, which is significantly higher than that of Fe3O4@Tp-PaV; except for toramectin (TUL), the recovery rates of Fe3O4@Tp-PaV for other macrolides are all lower than 30%. The above results show that this material is not based on non-covalent forces (hydrogen bonding, π-π interactions, etc.) on COF, but mainly based on boron affinity to adsorb macrolides, and has high selectivity.
[0123] Example 5
[0124] The reusability of Fe3O4@Tp-PaV@MPBA prepared in Example 1 was studied, and the specific experiment is as follows:
[0125] Prepare 2mL of aqueous solution containing 100μg / kg mixed standard of 7 macrolide drugs, adjust pH to 8, disperse 4mg Fe3O4@Tp-PaV@MPBA in it, vortex extract, magnetically separate nano-enriched materials, rinse twice with pure water, then add 2mL water / acetonitrile (v / v=4:1) containing 1% formic acid to the nano-enriched materials, vortex elute the target, take the supernatant through the membrane, and detect on the machine. The above nano-enriched materials were washed several times with water / acetonitrile (v / v=4:1) containing 1% formic acid, and dried for standby use; repeat the above experiment a total of 8 times.
[0126] Calculate the recovery rate of macrolides under different times of use of this material. The results are as follows Fig. 9 After being reused 8 times, the recovery rate was not significantly different from that before (P ≥ 0.05), indicating that the magnetic nano-enrichment material can be reused at least 8 times and has good reusability.
[0127] Examples 3-5 have conducted a detailed study on the adsorption isotherm model, adsorption kinetics, and adsorption mechanism of the magnetic nano-enriched material. The results show that Fe3O4@Tp-PaV@MPBA exhibits similar adsorption processes for 7 typical MALs. The adsorption of Fe3O4@Tp-PaV@MPBA on 7 typical MALs conforms to the kinetic pseudo-secondary model and the Langmuir adsorption isotherm model. This phenomenon can be explained as follows: there is a boron affinity between Fe3O4@Tp-PaV@MPBA (containing boronic acid groups) and MALs (containing cis-dihydroxyl groups), which is the dominant adsorption effect, and the boron affinity is accompanied by electron transfer (boron-oxygen bond formation), thus causing monolayer chemical adsorption.
[0128] In summary, the magnetic nano-enrichment material prepared in the embodiment of the present invention has strong magnetism, good dispersibility in water, large specific surface area, large adsorption capacity, fast adsorption rate, high selectivity, and reusability, and is particularly suitable for the efficient enrichment and purification of MALs in complex samples.
[0129] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0130] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A magnetic nano-enriched material, characterized in that: include: A core body, wherein the core body is composed of superparamagnetic ferroferric oxide; as well as A shell is coated on at least a portion of the surface of the core, and the shell is composed of the repeating unit shown in Formula I.
2. The magnetic nano-enriched material according to claim 1, characterized in that: The average particle size of the core is 150-250nm, and the shell is a porous mesh structure. Optionally, the shell has an average adsorption pore size of 3-5 nm and a thickness of 40-60 nm. Optionally, the specific surface area of the magnetic nano-enriched material is 120-180 m 2 / g.
3. The magnetic nano-enriched material according to claim 1, characterized in that: The magnetic strength of the magnetic nano-enriched material is 35-45emu / g, Optionally, the magnetic nano-enriched material can be reused more than 8 times.
4. The magnetic nano-enriched material according to claim 1, characterized in that: In X-ray powder diffraction data, the magnetic nano-enriched material has crystal diffraction peaks at 2θ of 4.7°, 30.2°, 35.4°, 43.1°, 53.8°, 57.2° and 62.8°.
5. A method for preparing the magnetic nano-enriched material according to any one of claims 1 to 4, characterized in that: include: Providing amino-ferroferric oxide magnetic nanoparticles; The aminated ferroferric oxide magnetic nanoparticles are contacted with an aldehyde monomer and pre-mixed in a first solvent to obtain a pre-mixed solution; contacting the premixed solution with the amino monomer to perform an aldehyde-amine condensation reaction to obtain an enriched material intermediate; as well as The enrichment material intermediate is contacted with 4-mercaptophenylboronic acid (4-MPBA), and a thiol-ene click reaction is carried out in a second solvent to functionally modify the enrichment material intermediate, so as to obtain the magnetic nano-enrichment material.
6. The method according to claim 5, characterized in that The method for preparing the amino-ferroferric oxide magnetic nanoparticles comprises: Dispersing ferric chloride hexahydrate in ethylene glycol and performing a first ultrasonic treatment to obtain a first mixed solution; contacting the first mixed solution with anhydrous sodium acetate and performing a first stirring to obtain a second mixed solution; contacting the second mixed solution with 1,6-hexanediamine and performing a second stirring to obtain a third mixed solution; and The second mixed solution is heated in a reaction kettle to obtain the amino-ferroferric oxide magnetic nanoparticles. Optionally, the mass ratio of ferric chloride hexahydrate, anhydrous sodium acetate and 1,6-hexanediamine is 1:(1-3):(5-7), preferably, the mass ratio is 1:2:6.5, Optionally, the heating treatment is carried out at a temperature of 180-220° C., preferably 200° C., and for a time of 6-8 hours, preferably 7 hours.
7. The method according to claim 5, characterized in that The amino monomer is 1,4-diamino-2,5-divinylbenzene (PaV), the aldehyde monomer is trialdehyde phloroglucinol (Tp), Optionally, the mass ratio of the aldehyde monomer, the amino monomer and the amino-containing ferroferric oxide magnetic nanoparticles is 1:(0.5-1.5):(2-4), preferably, the mass ratio is 1:1.14:2.
86. Optionally, the initiator of the thiol-ene click reaction is azobisisobutyronitrile (AIBN), Optionally, the mass ratio of the initiator, 4-mercaptophenylboronic acid and the enrichment material intermediate is 1:(10-15):(10-15), preferably, 1:12:13.
3. Optionally, the reaction temperature of the thiol-ene click reaction is 50-70°C, preferably 65°C, and the reaction time is 10-16 hours, preferably 14 hours.
8. The method according to claim 5, characterized in that The first solvent is a mixed solution of 1,4-dioxane and mesitylene, and the volume ratio of 1,4-dioxane to mesitylene is 1:(0.9-1.1), Optionally, the second solvent is an ethanol aqueous solution, wherein the volume ratio of ethanol to water is 1:(2-5), preferably 1:
3. Optionally, the catalyst for the aldehyde-amine condensation reaction is acetic acid, Optionally, the volume ratio of the acetic acid to the first solvent is 1:(25-35), preferably, 1:
28. Optionally, the reaction time of the aldehyde amine condensation reaction is 48-84 hours, preferably, the reaction time is 72 hours.
9. A method for adsorbing macrolide compounds, characterized in that: The method is carried out using the magnetic nano-enriched material according to any one of claims 1 to 4.
10. The method according to claim 9, characterized in that The macrolide compound is at least one selected from toramectin (TUL), spiramycin (SPI), azithromycin (AZI), gamithromycin (GAM), tylosin (TYL), clarithromycin (CLA) and roxithromycin (ROX); Optionally, the adsorption capacity of the magnetic nano-enriched material is 18-45 mg / g.