Catalyst and synthesis method thereof, and preparation method for synthesizing 1, 1, 2, 3-tetrachloropropene intermediate product

M@KIT-6 catalyst was prepared by supporting the active metal on the KIT-6 molecular sieve and carrying out appropriate heat treatment, which solved the problem of excessive chlorination and polychlorinated recombinant in the production of 1,1,2,3-tetrachloropropylene , improves product selectivity and production efficiency, and is suitable for industrial applications.

CN119076044APending Publication Date: 2024-12-06JIANGSU YANGNONG CHEMICAL GROUP CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411194931.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, there is an excessive chlorination reaction in the production process of 1,1,2,3-tetrachloropropylene, which leads to the generation of polychlorinated recombinant impurities, affecting the selectivity and cost of the product.

Method used

A M@KIT-6 catalyst was prepared by using KIT-6 molecular sieve as catalyst support and treatment with heating reflux, active metal loading and inert atmosphere to control the chlorination reaction and inhibit the generation of excessive chlorination and polychlorination recombinant.

Benefits of technology

It improves the selectivity of the target product, reduces the generation of polychlorinated recombinants, is suitable for industrial production, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016897900000101
    Figure BDA0005016897900000101
  • Figure BDA0005016897900000111
    Figure BDA0005016897900000111
Patent Text Reader

Abstract

The invention provides a catalyst, a synthesis method thereof and a preparation method for synthesizing an intermediate product of 1, 1, 2, 3-tetrachloropropene. The synthesis method of the catalyst comprises the following steps: S1) mixing a KIT-6 molecular sieve with a first dispersing solvent and a reactant in sequence, and carrying out heating reflux to obtain a to-be-loaded KIT-6 molecular sieve; s2) mixing a to-be-loaded KIT-6 molecular sieve and the dispersion liquid of the active metal, and performing first heating in a first atmosphere to obtain a KIT-6 molecular sieve loaded with the active metal; and S3) carrying out second heating on the active metal-loaded KIT-6 molecular sieve in a second atmosphere to obtain the catalyst. The problem that a synthesis method of the catalyst in the prior art is not suitable for industrial enlarged production can be solved, and the catalyst is suitable for the field of industrial catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of industrial catalysis, and in particular to a catalyst and a synthesis method thereof, and a preparation method for synthesizing a 1,1,2,3-tetrachloropropene intermediate. Background Art

[0002] 1,1,2,3-Tetrachloropropene is an important precursor of the new green and environmentally friendly refrigerants HFO-1234yf (2,3,3,3-tetrafluoropropene) and HFO-1234ze (E) (trans-1,3,3,3-tetrafluoropropene). As the fourth generation of new environmentally friendly refrigerants, HFO-1234yf and HFO-1234ze (E) have the characteristics of low ODP (Ozone Depletion Potential, ozone depletion index) and low GWP (Global Warming Potential, greenhouse effect index), and are considered to be the most promising alternatives to the new generation of refrigerants. In addition, 1,1,2,3-tetrachloropropene can also be used to synthesize the chemical herbicide wild barley chlorpyrifos and the pesticide chlormequat, which has broad application prospects.

[0003] At present, the production of 1,1,2,3-tetrachloropropene mainly uses ethylene + carbon tetrachloride or trichloropropane as raw materials, and the tetrachloropropene product is obtained through multi-step chlorination, HCl removal, distillation, and water removal. The process route is long, a large amount of waste salt is produced as a by-product, and there is also great environmental pressure. Using chloropropylene / dichloropropylene as raw materials through multi-step chlorination and HCl removal reactions can effectively reduce the production cost of 1,1,2,3-tetrachloropropene, but there is a problem of over-chlorination, which causes the product to contain a variety of heavy component impurities, affecting the product yield and product quality of the process. Therefore, controlling the chlorination process is one of the research focuses of the product synthesis route.

[0004] Patent application CN1566063A reports a method for selectively chlorinating acetic acid to produce monochloroacetic acid. In the technical solution of the patent application, a mother liquor containing monochloroacetic acid and a chlorine inhibitor are used to inhibit over-chlorination and reduce the generation of dichloroacetic acid. However, the addition of the mother liquor and the chlorine inhibitor with complex components leads to heavy components in the final product. Therefore, the prior art lacks a synthesis method that can avoid the generation of polychlorinated heavy component impurities due to over-chlorination and has high selectivity for the target product, which can be applied to industrial scale-up production. Summary of the invention

[0005] The main purpose of the present invention is to provide a catalyst and a synthesis method thereof and a preparation method for synthesizing a 1,1,2,3-tetrachloropropene intermediate product, so as to solve the problem that the synthesis method of the catalyst in the prior art is not suitable for industrial scale-up production.

[0006] In order to achieve the above-mentioned purpose, according to the first aspect of the present invention, a method for synthesizing a catalyst is provided, which comprises: S1) mixing a KIT-6 molecular sieve with a first dispersing solvent and a reactant in sequence, and heating and refluxing the mixture to obtain a KIT-6 molecular sieve to be loaded; S2) mixing the KIT-6 molecular sieve to be loaded and a dispersion of an active metal, and performing a first heating under a first atmosphere to obtain a KIT-6 molecular sieve loaded with an active metal; S3) performing a second heating on the KIT-6 molecular sieve loaded with an active metal under a second atmosphere to obtain a catalyst.

[0007] Further, in S1), the reactant includes one or more of hexamethyldioxysilane, trimethylchlorosilane, methoxytrimethylsilane or trimethylamine; preferably, the first dispersing solvent includes methanol and / or ethanol; preferably, the heating reflux temperature is 20-80°C, and the time is 2-24h; preferably, the mass ratio of the reactant to the KIT-6 molecular sieve is 1.5-10:1; preferably, after heating reflux, the KIT-6 molecular sieve obtained after heating reflux is subjected to a first washing and a first drying; preferably, the first drying time is 20-80°C, and the time is 6-24h.

[0008] Further, in S2), the active metal includes one or more of Zn, Ca or Mg; preferably, the active metal is Zn.

[0009] Further, S2) includes: S2-1) mixing, stirring and solid-liquid separation of the KIT-6 molecular sieve to be loaded and the dispersion of the active metal in sequence to obtain a wet powder of the KIT-6 molecular sieve loaded with the active metal; S2-2) performing a second drying on the wet powder of the KIT-6 molecular sieve loaded with the active metal, and then performing a first heating under a first atmosphere to obtain a KIT-6 molecular sieve loaded with the active metal; the first atmosphere is hydrogen; preferably, the stirring time is 2-10h; preferably, the first heating temperature is 20-600°C and the time is 2-48h; preferably, the second drying temperature is 20-80°C and the time is 6-24h.

[0010] Further, in S2-1), the method for synthesizing the active metal dispersion comprises: mixing the active metal precursor in a second dispersing solvent to obtain the active metal dispersion; preferably, the active metal precursor comprises: one or more of sulfates, nitrates, perchlorates or tetrafluoroborates containing active metal elements; preferably, the active metal precursor comprises one or more of ZnSO4, Zn(NO3)2, Zn(ClO4)2 or Zn(BF4)2; more preferably, the active metal precursor is Zn(NO3)2; preferably, the second dispersing solvent comprises deionized water.

[0011] Further, in S3), the second atmosphere includes an inert gas; preferably, the inert gas includes one or more of nitrogen, argon or helium; preferably, the second heating temperature is 50-1000°C, and the time is 1-24h; preferably, the loading amount of the active metal in the catalyst is 0.1wt%-5wt%; preferably, the loading includes loading the active metal in the pores of the KIT-6 molecular sieve.

[0012] In order to achieve the above object, according to a second aspect of the present invention, a catalyst is provided, which is a catalyst synthesized by any of the above-mentioned catalyst synthesis methods.

[0013] In order to achieve the above object, according to the third aspect of the present invention, there is provided a method for preparing an intermediate product for synthesizing 1,1,2,3-tetrachloropropene, the method comprising: mixing a catalyst synthesized by any of the above catalyst synthesis methods, or the above catalyst, with a raw material, and introducing chlorine gas to carry out a chlorination reaction to obtain an intermediate product for synthesizing 1,1,2,3-tetrachloropropene; the raw material comprises chlorinated olefins; and the intermediate product for synthesizing 1,1,2,3-tetrachloropropene comprises chlorinated propanes.

[0014] Further, the chlorinated propane includes one or more of 1,1,2,3-tetrachloropropane, 1,2,2,3-tetrachloropropane or 1,2,3-trichloropropane; preferably, the chlorinated olefin includes one or more of 1,3-dichloropropene, 3-chloropropene, 2,3-dichloropropene, 1,2,3-trichloropropene, 2,3-trichloropropene, 1,1,3-trichloropropene or 2,3,3-trichloropropene.

[0015] Furthermore, the amount of catalyst added is 0.1wt%-10wt% of the raw material mass; preferably, the molar ratio of chlorine to raw material is 0.1-2:1.

[0016] According to a fourth aspect of the present invention, there is provided a catalyst synthesized by the synthesis method of any one of the above catalysts, or use of the above catalyst in synthesizing chlorine-containing compounds.

[0017] By applying the technical solution of the present invention, the KIT-6 molecular sieve is sequentially mixed with the first dispersing solvent and the reactant, and then heated under reflux. After the pretreatment is completed, the KIT-6 molecular sieve to be loaded is obtained. The KIT-6 molecular sieve to be loaded and the dispersion of the active metal are first heated under the first atmosphere to obtain the KIT-6 molecular sieve with the active metal loaded inside the pores. The molecular sieve is second heated under the second atmosphere to obtain the catalyst of the present application. When the catalyst of the present application is used to synthesize the polychlorinated target product, the chlorination reaction process can be effectively controlled, the occurrence of over-chlorination can be prevented, the generation of polychlorinated heavy components can be suppressed, the selectivity of the target product can be improved, and the catalyst is suitable for industrial scale-up production. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] Terminology explanation:

[0020] Target product selectivity: The ratio of the target product to all other possible products produced during the reaction reflects the specificity of the reaction.

[0021] Polychlorinated heavy components: refers to components containing 5 or 6 chlorine atoms produced during the synthesis of chlorine-containing compounds.

[0022] As mentioned in the background technology, in the prior art, the synthesis route of 1,1,2,3-tetrachloropropene has the situation of over-chlorination, which leads to the generation of polychlorinated heavy components and low selectivity of the target product. To solve this defect, the occurrence of over-chlorination reaction can be regulated by changing the properties of the raw materials or adding chlorine inhibitors, but this method will introduce other impurities and the selectivity of the target product is still low. Therefore, in the present application, the inventor attempts to develop a new catalyst and apply it to the intermediate product in the production process of synthesizing 1,1,2,3-tetrachloropropene. This catalyst can avoid the occurrence of over-chlorination reaction, improve the selectivity of the target product, and is suitable for industrialized scale-up production, so a series of protection schemes of the present application are proposed.

[0023] In a first typical embodiment of the present application, a method for synthesizing a catalyst is provided, the method comprising: S1) mixing a KIT-6 molecular sieve with a first dispersing solvent and a reactant in sequence, and heating and refluxing the mixture to obtain a KIT-6 molecular sieve to be loaded; S2) mixing the KIT-6 molecular sieve to be loaded and a dispersion of an active metal, and performing a first heating under a first atmosphere to obtain a KIT-6 molecular sieve loaded with an active metal; S3) performing a second heating on the KIT-6 molecular sieve loaded with an active metal under a second atmosphere to obtain a catalyst.

[0024] In the prior art, when preparing the intermediate product of synthesizing 1,1,2,3-tetrachloropropene, due to the occurrence of over-chlorination reaction, various polychlorinated heavy components are easily generated, resulting in low selectivity of the target product. Usually, the generation of polychlorinated heavy components is reduced by selecting the substrate or adding a chlorine inhibitor to control the chlorination reaction. However, this is often accompanied by the complication of the reaction system components and the generation of other heavy component impurities. The selectivity of the target product is also affected, thereby affecting the subsequent synthesis of 1,1,2,3-tetrachloropropene.

[0025] KIT-6 molecular sieve is a mesoporous silica molecular sieve with a three-dimensional interconnected double-helix pore structure. The pore size can be adjusted, and it can maintain structural stability at higher temperatures. It can load various active metals and is suitable as a catalyst carrier.

[0026] In the present application, a new catalyst suitable for selective chlorination to prepare trichloro and tetrachloro products (a product containing 3 to 4 chlorine atoms) is synthesized, which is an M@KIT-6 catalyst, wherein M represents an active metal, including one or more of Zn, Ca, and Mg; the catalyst in the present application is mixed with a raw material to be chlorinated, and after a proper amount of chlorine is introduced, the chlorine and the M@KIT-6 catalyst are in-situ chlorinated to produce an MCl@KIT-6 catalyst, and then the raw material to be chlorinated is continued to be chlorinated without changing the amount of chlorine. The catalyst of the present application can inhibit the occurrence of over-chlorination reaction, prevent the generation of polychlorinated heavy components (pentachloro and hexachloro products), and improve the selectivity of the target product.

[0027] When synthesizing the catalyst in this application, the KIT-6 molecular sieve is first surface pretreated to passivate the outer surface so that the active metal can be selectively loaded in the pores of the molecular sieve, rather than loaded on the surface of the molecular sieve. When the active metal is selectively loaded in the pores of the KIT-6 molecular sieve, compared with loading on its surface, it has the advantage that the active component is not easy to lose and does not grow up excessively. The application uses a second atmosphere to treat the catalyst, and the active component particle size grows appropriately, adjusts the particle size of the active component, controls the ability of the catalyst to activate chlorine, and makes the catalytic activity not too strong to cause side reactions to occur, therefore, the target product selectivity of the catalyst of the application is high, and the yield of the product can be further improved. Compared with the catalyst in the prior art, it is more suitable for industrial amplification production of high chlorine product synthesis.

[0028] In a preferred embodiment, in S1), the reactant includes one or more of hexamethyldioxysilane, trimethylchlorosilane, methoxytrimethylsilane or trimethylamine; preferably, the first dispersing solvent includes methanol and / or ethanol; preferably, when the first dispersing solvent contains methanol and ethanol, the volume ratio of methanol to ethanol is: (1-99); (99-1), including but not limited to 1:99, 10:90, 30:70, 20:80, 40:60, 50:50, 60:40, 70:30, 80:2010:90 or 99:1; preferably, the heating reflux temperature is 20-80°C, including but not limited to 20°C, 30°C, 40°C, 50°C, 60°C, 70°C or 80°C, and the time is 2-24h, including but not limited to 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h; preferably, the mass ratio of the reactant to the KIT-6 molecular sieve is 1.5-10:1, including but not limited to 1.5:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1; preferably, after heating and reflux, the KIT-6 molecular sieve obtained after heating and reflux is subjected to a first washing and a first drying; preferably, the first drying time is 20-80°C, including but not limited to 20°C, 30°C, 40°C, 50°C, 60°C, 70°C or 80°C, and the time is 6-24h, including but not limited to 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h.

[0029] S1 of the present application) is a step for pre-treating KIT-6 molecular sieve, the purpose of which is to enable subsequent active metals to be loaded in the pores of the molecular sieve rather than on the surface. Using the reaction treatment agent in the present application, the KIT-6 molecular sieve is heated to reflux for 2-24h in the temperature range of 20-80°C, and the mass ratio of the reaction treatment agent and the KIT-6 molecular sieve is controlled, and the KIT-6 molecular sieve is subjected to surface passivation treatment, and the hydrophilicity / hydrophobicity of the molecular sieve surface can be appropriately changed, so that the active metals of the subsequent steps can be attached to the pores of the molecular sieve. Compared with being attached to the surface, the active metal attached to the pores is not easy to be lost in the reaction, which is conducive to the catalyst to remain active during the reaction, and further improves the efficiency of catalysis.

[0030] In a preferred embodiment, in S2), the active metal includes one or more of Zn, Ca or Mg; preferably, the active metal is Zn.

[0031] In a preferred embodiment, S2) includes: S2-1) mixing, stirring and solid-liquid separation of the KIT-6 molecular sieve to be loaded and the dispersion of the active metal in sequence to obtain a wet powder of the KIT-6 molecular sieve loaded with the active metal; S2-2) after the wet powder of the KIT-6 molecular sieve loaded with the active metal is subjected to a second drying, a first heating is performed under a first atmosphere to obtain a KIT-6 molecular sieve loaded with the active metal; preferably, the stirring time is 2-10h, including but not limited to 2, 3, 4, 5, 6, 7, 8, 9 or 10h; the first atmosphere is hydrogen; preferably, the first heating temperature is 20-600°C, including but not limited to 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 150°C, , 200℃, 250℃, 300℃, 400℃, 500℃ or 600℃, and the time is 2-48h, including but not limited to 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 30, 36, 40, 45 or 48h; more preferably, the temperature of the first heating is 150-400℃; preferably, the temperature of the second drying is 20-80℃, including but not limited to 20℃, 30℃, 40℃, 50℃, 60℃, 70℃ or 80℃; the time is 6-24h, including but not limited to 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h.

[0032] In the present application, the KIT-6 molecular sieve is first pretreated (S1 step) and surface passivated to obtain the KIT-6 molecular sieve to be loaded. The KIT-6 molecular sieve to be loaded is mixed with a dispersion of an active metal, and stirring allows the active metal to be loaded into the pores of the KIT-6 molecular sieve. At this time, what is loaded in the pores is an oxide containing an active metal, and a reduction reaction occurs under the heating of hydrogen, so that the active metal on the pores is reduced, and the loading of the active metal is achieved, and the KIT-6 molecular sieve loaded with active metal components in the pores of the molecular sieve can be obtained. The present application promotes the occurrence of the reduction reaction by controlling the temperature of the above-mentioned first heating, while maintaining a certain substrate conversion rate, and improving the selectivity of the target product.

[0033] In a preferred embodiment, in S2-1), the method for synthesizing the active metal dispersion comprises: mixing the active metal precursor in a second dispersing solvent to obtain the active metal dispersion; preferably, the active metal precursor comprises: one or more of sulfates, nitrates, perchlorates or tetrafluoroborates containing active metal elements; preferably, the active metal precursor comprises one or more of ZnSO4, Zn(NO3)2, Zn(ClO4)2 or Zn(BF4)2; more preferably, the active metal precursor is Zn(NO3)2; the second dispersing solvent comprises deionized water.

[0034] In a preferred embodiment, in S3), the second atmosphere comprises an inert gas; preferably, the inert gas comprises one or more of nitrogen, argon or helium; preferably, the second heating temperature is 50-1000°C, including but not limited to 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 150°C, 200°C, 250°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C or 1000°C, and the time is 1-24h, including but not limited to 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24h; more preferably, the temperature of the second heating is 100-600°C; preferably, the loading amount of the active metal in the catalyst is 0.1wt%-5wt%, including but not limited to 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%; preferably, the loading includes the active metal loading in the pores of the KIT-6 molecular sieve.

[0035] In this application, the size of the metal particles attached to the inside of the KIT-6 molecular sieve pores belongs to the nanometer level, and the melting point of the active metal particles of nanometer level size is much lower than the melting point of the bulk metal under the conventional size. The present application can further regulate the particle size of the active metal particles by performing a second heat treatment on the KIT-6 molecular sieve loaded with active metal under an inert gas. The present application can control the size of the active metal nanoparticles by controlling the temperature range and atmosphere of the second heat treatment, thereby regulating the particle size of the metal particles, so that it will not excessively affect the catalyst capacity, and the catalyst activates the ability of chlorine gas. Moderate regulation. If the temperature of the heating treatment is too high at this time, the size of the metal particles will be too large, affecting the efficiency of the catalytic reaction; and if the temperature is too low, the size of the metal particles will be too small, and too small a size will easily lead to uncontrollable reactions; and too large or too small a size will affect the stability of the catalyst.

[0036] By controlling the temperature range of the second heating, the present application further realizes that when the catalyst participates in the chlorination reaction, the depth of the chlorination reaction can be controlled, thereby avoiding excessive chlorination reaction and the generation of polychlorinated heavy components, improving the selectivity of the reaction target product, further improving the yield of the product, and being more suitable for industrial scale-up production.

[0037] In a second typical embodiment of the present application, a catalyst is provided. The catalyst is a catalyst synthesized by any of the above-mentioned catalyst synthesis methods.

[0038] In a third typical embodiment of the present application, a method for preparing an intermediate product for synthesizing 1,1,2,3-tetrachloropropene is provided, the preparation method comprising: mixing a catalyst synthesized by any of the above catalyst synthesis methods, or the above catalyst, with a raw material, and introducing chlorine gas for chlorination reaction to obtain an intermediate product for synthesizing 1,1,2,3-tetrachloropropene; the raw material comprises chlorinated olefins; and the intermediate product for synthesizing 1,1,2,3-tetrachloropropene comprises chlorinated propanes.

[0039] In a preferred embodiment, the chlorinated propane includes one or more of 1,1,2,3-tetrachloropropane, 1,2,2,3-tetrachloropropane or 1,2,3-trichloropropane; preferably, the chlorinated olefin includes 1,3-dichloropropene, 3-chloropropene, 2,3-dichloropropene, 1,2,3-trichloropropene, 2,3-trichloropropene, 1,1,3-trichloropropene, 2,3,3-trichloropropene.

[0040] In a preferred embodiment, the amount of the catalyst added is 0.1wt%-10wt% of the raw material mass, including but not limited to 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%; preferably, the molar ratio of chlorine to the raw material is 0.1-2:1, including but not limited to 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or 2:1.

[0041] The catalyst of the present application is mixed with the raw material in proportion, and after an appropriate amount of chlorine is introduced, the chlorine enters the catalyst pores, and an in-situ chlorination reaction occurs with the active metal loaded on the catalyst to obtain the MCl@KIT-6 catalyst, and then the raw material is continued to be chlorinated without changing the amount of chlorine. When in-situ chlorination occurs, the presence of the substrate changes the surface chemical environment during chlorination, promotes the chlorination process to move in a direction that is conducive to interaction with the substrate, and is conducive to improving the performance of the catalyst. When the catalyst of the present application is used in the preparation of chlorine-containing products, it can prevent the occurrence of excessive chlorination reactions, inhibit the generation of polychlorinated heavy components, and improve the selectivity of the target product. The present application further improves the reaction efficiency by controlling the mass range of the catalyst and the raw material, as well as the molar ratio of the chlorine introduced to the raw material, further improves the yield, reduces the processing cost of the discarded polychlorinated heavy components, and is more suitable for the synthesis of industrialized 1,1,2,3-tetrachloropropylene intermediates, which is conducive to the industrialized amplification of 1,1,2,3-tetrachloropropylene.

[0042] In a fourth typical embodiment of the present application, a method for synthesizing any one of the above catalysts, or use of the above catalysts in the synthesis of chlorine-containing compounds is provided.

[0043] The application of the synthesis of the above-mentioned chlorine-containing compounds is preferably the application of the synthesis of polychlorinated compounds that need to react with chlorine. In the synthesis process of such polychlorinated compounds in the prior art, an over-chlorination reaction usually occurs with chlorine, resulting in the generation of a variety of polychlorinated heavy components. When the catalyst synthesized by the synthesis method of any of the above-mentioned catalysts in this application or the above-mentioned catalyst is applied to the synthesis of such polychlorinated compounds, the chlorination depth can be controlled by controlling the ability of the catalyst to activate chlorine, which is beneficial to reduce the polychlorinated heavy components generated by over-chlorination in the production process, further improve the product yield, reduce the post-processing cost of the product, and improve the economic benefits of the overall process.

[0044] The beneficial effects of the present application will be further explained in detail below in conjunction with specific examples. Unless otherwise specified, the reagents used in the examples of the present application are all conventional commercially available products.

[0045] Example 1

[0046] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent containing methanol / ethanol (volume ratio of 10:90), add 1g of hexamethyldioxysilane, heat and reflux at 50°C for 6h, then wash with ethanol, and dry in a vacuum oven at 50°C for 12h to obtain the KIT-6 molecular sieve to be loaded.

[0047] 2. Disperse 1g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 4h, centrifuge, and dry at 30℃ for 12h. Then, reduce with hydrogen at 200℃ (first heating) for 6h to obtain KIT-6 molecular sieve loaded with active metal, wherein the loading amount of Zn is 0.8wt%.

[0048] 3. Treat the KIT-6 molecular sieve loaded with active metals with nitrogen at 150° C. (second heating) for 2 h to obtain a catalyst.

[0049] Chlorination performance verification:

[0050] 80g of catalyst and 1kg of 1,3-dichloropropene (substrate) were loaded into a kettle reactor. After the system was replaced with nitrogen three times and leak tested, chlorine was introduced at a chlorine to substrate molar ratio of 0.2:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,1,2,3-tetrachloropropane.

[0051] Example 2

[0052] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent of methanol / ethanol (volume ratio of 30:70), add 2g of trimethylsilyl chloride, heat and reflux at 60°C for 4h. Then wash with ethanol and dry in a vacuum oven at 40°C for 8h to obtain the KIT-6 molecular sieve to be loaded.

[0053] 2. Disperse 0.8 g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 6 hours, centrifuge, and dry at 40°C for 8 hours. Then reduce with hydrogen at 150°C for 7 hours to obtain the KIT-6 molecular sieve loaded with active metals, wherein the loading amount of Zn is 0.6 wt%.

[0054] 3. Treat the KIT-6 molecular sieve loaded with active metals with argon at 200° C. for 1.5 h to obtain a catalyst.

[0055] Chlorination performance verification:

[0056] 80g of the above catalyst and 1kg of 3-chloropropene (substrate) were loaded into a kettle reactor. After the system was replaced with nitrogen three times and leak tested, chlorine was introduced at a chlorine to substrate molar ratio of 0.4:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,2,3-trichloropropane.

[0057] Example 3

[0058] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent of methanol / ethanol (volume ratio of 20:80), add 1.8g of methoxytrimethylsilane, heat and reflux at 70°C for 4h. Then wash with ethanol and dry in a vacuum oven at 60°C for 8h to obtain the KIT-6 molecular sieve to be loaded.

[0059] 2. Disperse 1.2 g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 7 hours, centrifuge, and dry at 40°C for 8 hours. Then reduce with hydrogen at 250°C for 4 hours to obtain the KIT-6 molecular sieve loaded with active metals, wherein the loading amount of Zn is 1.1 wt%.

[0060] 3. Treat the KIT-6 molecular sieve loaded with active metals with helium at 250° C. for 1.2 h to obtain a catalyst.

[0061] Chlorination performance verification:

[0062] 80g of the above catalyst and 1kg of 2,3-dichloropropene (substrate) were loaded into a kettle reactor. After three treatments with nitrogen replacement system and leak testing, chlorine was introduced at a chlorine to substrate molar ratio of 0.6:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,2,2,3-tetrachloropropane.

[0063] Example 4

[0064] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent of methanol / ethanol (volume ratio of 30:70), add 2g of trimethylsilyl chloride, heat and reflux at 60°C for 4h. Then wash with ethanol and dry in a vacuum oven at 40°C for 8h to obtain the KIT-6 molecular sieve to be loaded.

[0065] 2. Disperse 0.8 g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 6 hours, centrifuge, and dry at 40°C for 8 hours. Then reduce with hydrogen at 150°C for 7 hours to obtain the KIT-6 molecular sieve loaded with active metals, wherein the loading amount of Zn is 0.7 wt%.

[0066] 3. Treat the KIT-6 molecular sieve loaded with active metals with nitrogen at 600°C for 1.5 hours to obtain a catalyst.

[0067] Chlorination performance verification:

[0068] 80g of the above catalyst and 1kg of 3-chloropropene (substrate) were loaded into a kettle reactor. After the system was replaced with nitrogen three times and leak tested, chlorine was introduced at a chlorine to substrate molar ratio of 0.4:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,2,3-trichloropropane.

[0069] Example 5

[0070] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent of methanol / ethanol (volume ratio of 20:80), add 1.8g of methoxytrimethylsilane, heat and reflux at 70°C for 4h. Then wash with ethanol and dry in a vacuum oven at 60°C for 8h to obtain the KIT-6 molecular sieve to be loaded.

[0071] 2. Disperse 1.2 g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 7 hours, centrifuge, and dry at 40°C for 8 hours. Then reduce with hydrogen at 250°C for 4 hours to obtain the KIT-6 molecular sieve loaded with active metals, wherein the loading amount of Zn is 1.1 wt%.

[0072] 3. Treat the KIT-6 molecular sieve loaded with active metals with nitrogen at 50° C. for 1.2 h to obtain a catalyst.

[0073] Chlorination performance verification:

[0074] 80g of the above catalyst and 1kg of 2,3-dichloropropene (substrate) were loaded into a kettle reactor. After three treatments with nitrogen replacement system and leak testing, chlorine was introduced at a chlorine to substrate molar ratio of 0.6:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,2,2,3-tetrachloropropane.

[0075] Example 6

[0076] The difference from Example 1 is that the temperature of the first heating in step 2 is 400° C., and the remaining steps and chlorination performance verification are consistent with the steps of Example 1.

[0077] Example 7

[0078] The difference from Example 1 is that the temperature of the second heating in step 3 is 100° C., and the remaining steps and chlorination performance verification are consistent with the steps of Example 1.

[0079] Example 8

[0080] The difference from Example 1 is that the temperature of the first heating in step 2 is 20° C., and the remaining steps and chlorination performance verification are consistent with the steps of Example 1.

[0081] Example 9

[0082] The difference from Example 1 is that the temperature of the first heating in step 2 is 600° C., and the remaining steps and chlorination performance verification are consistent with the steps of Example 1.

[0083] Example 10

[0084] The difference from Example 1 is that the temperature of the second heating in step 3 is 1000° C., and the remaining steps and chlorination performance verification are consistent with the steps of Example 1.

[0085] Comparative Example 1

[0086] 1. Take 100g KIT-6 molecular sieve and 1.2g Zn(NO3)2 dispersed in deionized water, mix the two, stir for 7h, centrifuge and dry at 40℃ for 8h. Then reduce with hydrogen at 250℃ for 4h and treat with nitrogen at 250℃ for 1.2h to obtain the catalyst.

[0087] Chlorination performance verification:

[0088] 80g of the above catalyst and 1kg of 1,3-dichloropropene (substrate) were loaded into a kettle reactor. After three treatments with nitrogen replacement system and leak testing, chlorine was introduced at a chlorine to substrate molar ratio of 0.6:1, a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to obtain the product 1,1,2,3-tetrachloropropane.

[0089] Comparative Example 2

[0090] 1 kg of 1,3-dichloropropene (substrate) was loaded into a kettle reactor. After the system was replaced with nitrogen three times and leak tested, chlorine was introduced at a molar ratio of chlorine to substrate of 1:1, with a chlorine flow rate of 60 L / min, a reaction temperature of 25°C, a pressure of 0.1 MPa, and a reaction time of 6 h to obtain the product 1,1,2,3-tetrachloropropane.

[0091] Comparative Example 3

[0092] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent of methanol / ethanol (volume ratio of 10:90), add 1g of hexamethyldioxysilane, heat and reflux at 50°C for 6h. Then wash with ethanol and dry in a vacuum oven at 50°C for 12h to obtain the KIT-6 molecular sieve to be loaded.

[0093] 2. Disperse 1g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 4h, centrifuge, and dry at 30℃ for 12h. Then reduce with hydrogen at 200℃ for 6h to obtain KIT-6 molecular sieve loaded with active metals, with a Zn loading of 0.9wt%.

[0094] 3. Treat the KIT-6 molecular sieve loaded with active metals with nitrogen at 150°C for 2 h and with chlorine at room temperature for 8 h to obtain a catalyst.

[0095] Chlorination performance verification:

[0096] 80g of the above catalyst and 1kg of 1,3-dichloropropene (substrate) were loaded into a kettle reactor. After the system was replaced with nitrogen three times and leak tested, chlorine was introduced at a molar ratio of chlorine to substrate of 0.8:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,1,2,3-tetrachloropropane.

[0097] Comparative Example 4

[0098] 1. Take 100g of KIT-6 molecular sieve, disperse it in 500mL of the first dispersing solvent containing methanol / ethanol (volume ratio of 10:90), add 1g of hexamethyldioxysilane, heat and reflux at 50°C for 6h, then wash with ethanol, and dry in a vacuum oven at 50°C for 12h to obtain the KIT-6 molecular sieve to be loaded.

[0099] 2. Disperse 1g Zn(NO3)2 in deionized water, then add the KIT-6 molecular sieve to be loaded, stir for 4h, centrifuge and dry at 30°C for 12h. Then reduce with hydrogen at 200°C for 6h to obtain KIT-6 molecular sieve loaded with active metal, which is used as the catalyst in this comparative example, wherein the loading amount of Zn is 0.8wt%.

[0100] Chlorination performance verification:

[0101] 80g of catalyst and 1kg of 1,3-dichloropropene (substrate) were loaded into a kettle reactor. After the system was replaced with nitrogen three times and leak tested, chlorine was introduced at a chlorine to substrate molar ratio of 0.3:1, with a chlorine flow rate of 60L / min, a reaction temperature of 25°C, a pressure of 0.1MPa, and a reaction time of 6h to generate the product 1,1,2,3-tetrachloropropane.

[0102] The substrate conversion rate and chromatographic analysis were performed on Examples 1 to 10 and Comparative Examples 1 to 4. The substrate conversion rate and the selectivity of the target product are shown in Table 1.

[0103] Table 1

[0104]

[0105]

[0106] As can be seen from Table 1, the use of the catalyst of the present application can effectively control the chlorination reaction, avoiding the problems of excessive by-products and low selectivity of the target product caused by over-chlorination reaction.

[0107] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: by passivating the surface of KIT-6 molecular sieve, the loading of active metal in the pores of KIT-6 molecular sieve is achieved; and by adopting appropriate heat treatment regulation, including regulating the size of active metal nanoparticles in atmosphere, temperature and treatment time, the ability to activate chlorine is controlled; and by in-situ chlorination of active metal in the presence of substrate, the surface chemical environment is improved. Through the combined effect of the above treatments, the catalyst prepared can achieve the inhibition of over-chlorination when used in the preparation of the intermediate product of synthesizing 1,1,2,3-tetrachloropropene, reduce the generation of polychlorinated heavy components or other by-products, and improve the selectivity of the target product. In addition, the reaction conditions are mild, the synthesis method is simple, and the cost is lower than that of the prior art, which can further improve the yield of the target product and is more suitable for industrial scale-up production.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for synthesizing a catalyst, characterized in that: The synthesis method comprises: S1) mixing the KIT-6 molecular sieve with the first dispersing solvent and the reactant in sequence, and heating and refluxing to obtain the KIT-6 molecular sieve to be loaded; S2) mixing the KIT-6 molecular sieve to be loaded and the dispersion of the active metal, and performing a first heating under a first atmosphere to obtain the KIT-6 molecular sieve loaded with the active metal; S3) subjecting the KIT-6 molecular sieve loaded with active metal to a second heating under a second atmosphere to obtain the catalyst.

2. The synthesis method according to claim 1, characterized in that In the S1), the reactant includes one or more of hexamethyldioxysilane, trimethylchlorosilane, methoxytrimethylsilane or trimethylamine; Preferably, the first dispersing solvent comprises methanol and / or ethanol; Preferably, the heating reflux temperature is 20-80°C and the time is 2-24h; Preferably, the mass ratio of the reactant to the KIT-6 molecular sieve is 1.5-10:1; Preferably, after the heating and reflux, the KIT-6 molecular sieve obtained after the heating and reflux is subjected to a first washing and a first drying; Preferably, the first drying time is 20-80°C and the time is 6-24h.

3. The synthesis method according to claim 1, characterized in that In said S2), said active metal comprises one or more of Zn, Ca or Mg; Preferably, the active metal is Zn.

4. The synthesis method according to claim 1, characterized in that The S2) includes: S2-1) sequentially mixing, stirring and solid-liquid separation of the KIT-6 molecular sieve to be loaded and the dispersion of the active metal to obtain a wet powder of the KIT-6 molecular sieve loaded with the active metal; S2-2) performing a second drying on the wet powder of the KIT-6 molecular sieve loaded with active metals, and then performing the first heating under the first atmosphere to obtain the KIT-6 molecular sieve loaded with active metals; The first atmosphere is hydrogen; Preferably, the stirring time is 2-10 h; preferably, the first heating temperature is 20-600° C., and the time is 2-48 h; preferably, the second drying temperature is 20-80° C., and the time is 6-24 h.

5. The synthesis method according to claim 4, characterized in that In S2-1), the method for synthesizing the active metal dispersion includes: mixing the active metal precursor in a second dispersion solvent to obtain the active metal dispersion; Preferably, the precursor of the active metal includes: one or more of sulfates, nitrates, perchlorates or tetrafluoroborates containing active metal elements; Preferably, the precursor of the active metal includes one or more of ZnSO4, Zn(NO3)2, Zn(ClO4)2 or Zn(BF4)2; More preferably, the precursor of the active metal is Zn(NO3)2; Preferably, the second dispersing solvent comprises deionized water.

6. The synthesis method according to claim 1, characterized in that In said S3), said second atmosphere comprises an inert gas; Preferably, the inert gas comprises one or more of nitrogen, argon or helium; Preferably, the second heating temperature is 50-1000°C, and the time is 1-24h; preferably, the loading amount of the active metal in the catalyst is 0.1wt%-5wt%; Preferably, the loading includes loading the active metal in the pores of the KIT-6 molecular sieve.

7. A catalyst, characterized in that The catalyst is a catalyst synthesized by the method for synthesizing a catalyst according to any one of claims 1 to 6.

8. A method for preparing an intermediate product for synthesizing 1,1,2,3-tetrachloropropene, characterized in that: The preparation method comprises: The catalyst synthesized by the method for synthesizing the catalyst according to any one of claims 1 to 6, or the catalyst according to claim 7, is mixed with a raw material, and chlorine gas is introduced to carry out a chlorination reaction to obtain the intermediate product for synthesizing 1,1,2,3-tetrachloropropene; The raw materials include chlorinated olefins; The intermediate product of synthesizing 1,1,2,3-tetrachloropropene includes chloropropane.

9. The preparation method according to claim 8, characterized in that: The chloropropane includes one or more of 1,1,2,3-tetrachloropropane, 1,2,2,3-tetrachloropropane or 1,2,3-trichloropropane; Preferably, the chlorinated olefins include one or more of 1,3-dichloropropene, 3-chloropropene, 2,3-dichloropropene, 1,2,3-trichloropropene, 2,3-trichloropropene, 1,1,3-trichloropropene or 2,3,3-trichloropropene.

10. The preparation method according to claim 8, characterized in that: The amount of the catalyst added is 0.1wt%-10wt% of the raw material mass; Preferably, the molar ratio of the chlorine gas to the raw material is 0.1-2:

1.

11. A catalyst synthesized by the method for synthesizing a catalyst according to any one of claims 1 to 6, or use of the catalyst according to claim 7 in synthesizing chlorine-containing compounds.