Ruthenium-based solid acid catalyst, preparation method thereof and application of ruthenium-based solid acid catalyst in preparation of ethanol through hydrogenation of carbon dioxide
Through the preparation and application of ruthenium-based solid acid catalyst, the problem of low selectivity and yield in the hydrogenation of carbon dioxide to ethanol is solved, and high selectivity is achieved to prepare ethanol and reduce by-product generation, and the catalyst cost is relatively low.
Patent Information
- Application Number
- CN202411191142.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-28
AI Technical Summary
At this stage, the single-pass selectivity and yield of carbon dioxide hydrogenation to produce ethanol is relatively low, and the existing catalysts are costly or scarce, which has the problem of greater competition for by-products.
The Ru-S2O82-/ZrO2-HZSM-5 catalyst was prepared by impregnation method using the preparation method of a ruthenium-based solid acid catalyst, and the catalyst was used in the liquid solid phase reaction to react carbon dioxide with hydrogen to prepare ethanol with high selectivity.
The high selective preparation of ethanol is achieved, reducing by-product generation, and the use of ruthenium-based catalysts is relatively economical, avoiding high cost and by-product competition in traditional methods.
Smart Images

Figure CN119076050A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of a ruthenium-based catalyst, in particular to a ruthenium-based solid acid catalyst and a preparation method thereof and application thereof in the hydrogenation of carbon dioxide to produce ethanol, and belongs to the field of petrochemical industry. Background Art
[0002] As a C1 resource, carbon dioxide has aroused great interest due to its advantages such as recyclability, low cost, low toxicity and high added value of conversion products. The current methods to reduce the concentration of carbon dioxide in the atmosphere include carbon capture, storage and utilization. Therefore, converting carbon dioxide into chemicals with higher added value, such as alcohols, is of great significance for reducing CO2 emissions and effectively alleviating the greenhouse effect. The products of carbon dioxide thermal catalytic conversion are very rich. Carbon dioxide can be directly catalytically converted with green hydrogen to produce gasoline, alcohols, olefins and aromatics. They can be used directly as fuel, or they can be used as chemical raw materials to enter the next reaction to produce higher value-added chemical products.
[0003] Ethanol is an important chemical raw material, widely used in the fields of medicine, chemical industry, food, and fuel industry, and has great application prospects. In the early days, ethanol could only be synthesized by fermentation, but this method is time-consuming and inefficient. Ethylene synthesis and coal chemical production of ethanol are also unable to be applied on a large scale due to their harsh production conditions, the need for instruments and equipment to be acid-resistant and high-pressure-resistant, and high production costs. Therefore, the thermal catalytic conversion of carbon dioxide to ethanol is considered to be one of the most promising ways at present.
[0004] In summary, the study of carbon dioxide hydrogenation to ethanol has the following research significance: vigorously develop renewable energy industry, reduce human dependence on fossil energy, and thus reduce carbon dioxide gas emissions. On the other hand, CO2 is an abundant "carbon resource" in nature, low-priced and widely available. If C1 resources can be recycled, it is also an important way to achieve energy conversion; at the same time, it can also reduce CO2 concentration and achieve harmonious coexistence between man and nature. As a clean energy that can be used directly, ethanol is considered to be one of the best substances to replace fossil fuels. Therefore, the preparation of ethanol by catalytic hydrogenation of CO2 has received worldwide attention and is one of the effective ways to alleviate the dual pressures of environment and resources.
[0005] There are two widely accepted reaction mechanisms: one is that CO2 is converted into CO by reverse water gas shift reaction, part of CO is hydrogenated to generate *CH3, CO is embedded in *CH3 to complete carbon chain growth, and further hydrogenated to generate ethanol. The role of the catalyst is crucial in this process. The binding force between CO and the active species on the catalyst needs to be strong enough to prevent CO from further dissociating into *C and *O. The second is to form a carboxylic acid intermediate through the adsorption and activation of CO2 molecules, which is further reduced to produce a formic acid intermediate *HCOO, and the surface intermediate (*CH3COO) formed by the bonding of *CHx and *HCOO is further hydrogenated to form ethanol. The key steps are the activation of carbon dioxide and CC coupling. However, due to the high thermodynamic stability of CO2 and the high energy barrier of C=O bond breaking, its conversion and utilization are difficult. Studies have shown that the use of catalytic hydrogenation can effectively reduce the activation energy barrier of CO2.
[0006] Cu-based catalysts make ethanol the only organic product of CO2 hydrogenation reaction. Under certain conditions, the single-pass yield of ethanol can reach 14%, and the space-time yield can reach 398 mg / (g cat ·h). Due to the synergistic effect between the highly dispersed Rh and high density of hydroxyl groups on TiO2 nanorods, the Rh-based nanorod catalyst loaded on TiO2 nanorods has an ethanol selectivity of 32% in the catalytic CO2 hydrogenation reaction. The hydroxyl groups can stabilize the formate and protonate methanol, making it easy for methanol to decompose into *CH x , then CO (generated by the reverse water gas shift reaction) is inserted into *CH x *CH3CO is formed in the reaction, and *CH3CO is hydrogenated to produce ethanol. It is found that the shortcomings of the current research are: the single-pass selectivity and yield of the ethanol product synthesized by CO2 hydrogenation are relatively low, and the formation of byproducts such as C1 still has great competition for ethanol. The modified non-precious metal catalysts (Cu, Co) have obvious cost advantages, but generally have low ethanol selectivity. In addition, due to the high price and scarcity of Pt, the development of Pt-free catalysts for the reaction is prompted. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a ruthenium-based solid acid catalyst
[0008] The second object of the present invention is to provide a ruthenium-based solid acid catalyst prepared by the above preparation method.
[0009] The third object of the present invention is to provide the use of the above-mentioned ruthenium-based solid acid catalyst in the hydrogenation of carbon dioxide to ethanol.
[0010] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0011] In a first aspect, the present invention provides a method for preparing a ruthenium-based solid acid catalyst, comprising the following steps:
[0012] (1) dissolving ammonium persulfate in methanol to prepare an ammonium persulfate methanol solution; after ultrasonication for 10-20 minutes, adding zirconium dioxide and HZSM-5 molecular sieve to the solution respectively, and then stirring at room temperature for 6-8 hours; the SiO2 / Al2O3 of the HZSM-5 molecular sieve is 50;
[0013] (2) The precipitate obtained in step (1) was filtered and dried, and then calcined at 550°C for 3h to obtain S2O8 2- / ZrO2-HZSM-5 support;
[0014] (3) S2O8 2- / ZrO2-HZSM-5 carrier was added to the ruthenium salt aqueous solution, ultrasonicated, and reduced by adding sodium borohydride solution. After stirring for 10 minutes, it was filtered and then vacuum dried to obtain the desired Ru-S2O8 2- / ZrO2-HZSM-5 catalyst, wherein the Ru loading amount is 1%.
[0015] Preferably, the mass ratio of the zirconium dioxide to the HZSM-5 molecular sieve is 0.5-1.5:1.5-0.5.
[0016] Preferably, the concentration of the ammonium persulfate methanol solution is 0.0024 g / mL.
[0017] Preferably, the ruthenium salt is ruthenium trichloride.
[0018] Preferably, the vacuum drying temperature is 110° C. and the time is 12 h.
[0019] In a second aspect, the present invention also provides a ruthenium-based solid acid catalyst prepared by the above preparation method.
[0020] The pore size of the ruthenium-based solid acid catalyst is mainly present in the form of micropores and mesopores, and the Ru metal is highly dispersed on the surface of the carrier.
[0021] In the third aspect, the present invention further provides a method for utilizing the aforementioned Ru-S2O8 2- / ZrO2-HZSM-5 catalyst to hydrogenate carbon dioxide to ethanol, is to Ru-S2O8 2- / ZrO2-HZSM-5 catalyst is used in liquid-solid phase reaction to hydrogenate carbon dioxide into ethanol;
[0022] When used for liquid-solid phase reaction: take 5-50 mg of catalyst and 10 mL of deionized water, and place them in a reactor with a volume of 50 mL; fill the reactor with 0.4-2.8 MPa of reaction gas, and the molar ratio of H2:CO2 in the reaction gas is 2.5-3.5; control the reaction temperature to 140-240°C, and the reaction time to 1-5 hours; after the reaction, the main product obtained is ethanol, and the by-product is methanol;
[0023] In the present invention, the reaction gas also contains a balance gas that does not participate in the reaction, and the balance gas is N2, He or Ar.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The impregnation preparation method of the present invention is simple and easy to implement, and avoids the influence of uncertain factors in the preparation process on the catalyst structure and performance. The active component selected for the catalyst is ruthenium, which is relatively cheap among precious metals, and the Ru-based metal catalyst is applied to the carbon dioxide hydrogenation to ethanol reaction for the first time.
[0026] 2. The method of the present invention changes the status quo of the existing ethanol preparation methods. Compared with the traditional grain fermentation method, ethylene hydration method and synthesis gas synthesis method, the highly selective preparation of ethanol through the hydrogenation reaction of CO2, an abundant and easily available carbon source, is undoubtedly green and very promising.
[0027] 3. The Ru metal catalyst is obtained by reduction with sodium borohydride. The method is simple and can be activated simultaneously with CO2 and H2, which is beneficial to improve the selectivity for ethanol. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the SEM image of the ruthenium-based solid acid catalyst prepared in Example 1-5.
[0029] Figure 2 N2 adsorption-desorption isotherms of the ruthenium-based solid acid catalyst prepared in Examples 1-5.
[0030] Figure 3 The pore size distribution curves of the ruthenium-based solid acid catalysts prepared in Examples 1-5.
[0031] Figure 4 The XRD spectrum of the ruthenium-based solid acid catalyst prepared in Example 1-5.
[0032] Figure 5 It is the N2 adsorption-desorption isotherm of the ruthenium-based solid acid catalyst prepared in Example 1 and Examples 6-7.
[0033] Figure 6The pore size distribution curves of the ruthenium-based solid acid catalysts prepared in Example 1 and Examples 6-7.
[0034] Figure 7 The XRD spectra of the ruthenium-based solid acid catalysts prepared in Example 1 and Examples 6-7.
[0035] Figure 8 These are SEM images of the ruthenium-based solid acid catalysts prepared in Example 1 and Examples 8-11.
[0036] Fig. 9 N2 adsorption-desorption isotherms of the ruthenium-based solid acid catalysts prepared in Example 1 and Examples 8-11.
[0037] Fig.10 This is the pore size distribution curve of the ruthenium-based solid acid catalyst prepared in Example 1 and Examples 8-11.
[0038] Fig.11 The XRD spectra of the ruthenium-based solid acid catalysts prepared in Example 1 and Examples 8-11.
[0039] Fig.12 The catalytic performance of the ruthenium-based solid acid catalyst prepared in Examples 1-5 in producing ethanol from CO2.
[0040] Fig.13 The ruthenium-based solid acid catalyst prepared in Example 1 and Examples 6-7 has catalytic performance in producing ethanol from CO2.
[0041] Fig.14 The catalytic performance of ruthenium-based solid acid catalysts prepared in Example 1 and Examples 8-11 in producing ethanol from CO2. DETAILED DESCRIPTION
[0042] The first aspect of the present invention provides a catalyst preparation method: preparing an ammonium persulfate solution, preparing a composite carrier by an impregnation method, and further drying, high-temperature calcination and loading Ru metal, reducing, and drying to obtain Ru-S2O8 2- / ZrO2-HZSM-5 catalyst.
[0043] The second aspect of the present invention provides a catalyst application: the prepared Ru-S2O8 2- / ZrO2-HZSM-5 catalyst is used for the directional synthesis of ethanol by hydrogenation of carbon dioxide. In the liquid-solid phase reaction, the catalyst and solvent are put into a high-pressure reactor, and a mixed reaction gas (CO2 and H2) of a certain pressure is filled in. At a certain reaction temperature, ethanol can be prepared with high selectivity.
[0044] By controlling the catalyst preparation conditions and reaction conditions, as well as optimizing a number of experimental parameters, Ru-S2O8 can be used to prepare ethanol with high selectivity.2- Control of the structure and catalytic performance of / ZrO2-HZSM-5 catalyst.
[0045] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. The methods described are conventional methods unless otherwise specified. The materials described can be obtained from public commercial channels unless otherwise specified.
[0046] Example 1
[0047] 1. 1%Ru-5%S2O8 2- Preparation of ZrO2-HZSM-5 catalyst:
[0048] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h;
[0049] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5 support;
[0050] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0051] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / ZrO2-HZSM-5 catalyst.
[0052] 2. 1%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5 catalyst:
[0053] The prepared 1%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 1%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst was placed in a 50mL high-pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 3.05%, 96.95%, and 475ug·g, respectively. cat -1 ·h -1 and 21675ug·g cat -1 ·h -1 .
[0054] Example 2
[0055] 1. 1%Ru-5%S2O8 2- Preparation of / 2ZrO2 catalyst:
[0056] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 2 g of zirconium dioxide and add it to the mixed solution, and stir at room temperature for 7 h;
[0057] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / 2ZrO2 carrier;
[0058] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0059] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / 2ZrO2 catalyst.
[0060] 2. 1%Ru-5%S2O8 2- / 2ZrO2 catalyst application:
[0061] The prepared 1%Ru-5%S2O8 2- / 2ZrO2 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20mg1%Ru-5%S2O8 2- / 2ZrO2 catalyst was placed in a 50mL high pressure reactor, and 10mL water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 80.59%, 19.41% and 650ug·g respectively. cat -1 ·h -1 and 650ug·g cat -1 ·h -1 .
[0062] Example 3
[0063] 1. 1%Ru-5%S2O8 2- Preparation of / 1.5ZrO2-0.5HZSM-5 catalyst:
[0064] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1.5 g of zirconium dioxide and 0.5 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h;
[0065] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / 1.5ZrO2-0.5HZSM-5 carrier;
[0066] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0067] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / 1.5ZrO2-0.5HZSM-5 catalyst.
[0068] 2. 1%Ru-5%S2O8 2- / Application of 1.5ZrO2-0.5HZSM-5 catalyst:
[0069] The prepared 1%Ru-5%S2O8 2- / 1.5ZrO2-0.5HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20mg 1%Ru-5%S2O8 2- / 1.5ZrO2-0.5HZSM-5 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 18.42%, 81.58% and 950ug·g respectively. cat -1 ·h -1 and 6050ug·g cat -1 ·h -1 .
[0070] Example 4
[0071] 1. 1%Ru-5%S2O8 2- Preparation of / 0.5ZrO2-1.5HZSM-5 catalyst:
[0072] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 0.5 g of zirconium dioxide and 1.5 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h;
[0073] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / 0.5ZrO2-1.5HZSM-5 carrier;
[0074] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0075] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / 0.5ZrO2-1.5HZSM-5 catalyst.
[0076] 2. 1%Ru-5%S2O8 2- / Application of 0.5ZrO2-1.5HZSM-5 catalyst:
[0077] The prepared 1%Ru-5%S2O8 2- / 0.5ZrO2-1.5HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20mg 1%Ru-5%S2O8 2- / 0.5ZrO2-1.5HZSM-5 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 8.72%, 91.28% and 1225ug·g respectively. cat -1 ·h -1 and 18425ug·g cat -1 ·h -1 .
[0078] Example 5
[0079] 1. 1%Ru-5%S2O8 2- / Preparation of 2HZSM-5 catalyst:
[0080] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 2 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add it to the mixed solution, and stir at room temperature for 7 h;
[0081] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / 2HZSM-5 carrier;
[0082] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0083] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / 2HZSM-5 catalyst.
[0084] 2. 1%Ru-5%S2O8 2- / Application of 2HZSM-5 catalyst:
[0085] The prepared 1%Ru-5%S2O8 2- / 2HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 1% Ru-5% S2O8 2- / 2HZSM-5 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 46.99%, 53.01% and 3900ug·g respectively. cat -1 ·h -1 and 6325ug·g cat -1 ·h -1 .
[0086] Example 6
[0087] 1. 1%Ru-5%S2O8 2- / Preparation of ZrO2-HZSM-5-2 catalyst:
[0088] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=25) and add them to the mixed solution, and stir at room temperature for 7 h;
[0089] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5-2 carrier;
[0090] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0091] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / ZrO2-HZSM-5-2 catalyst.
[0092] 2. 1%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5-2 catalyst:
[0093] The prepared 1%Ru-5%S2O8 2- / ZrO2-HZSM-5-2 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 1% Ru-5% S2O8 2- / ZrO2-HZSM-5-2 catalyst was placed in a 50mL high-pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 41.56%, 58.44% and 1175ug·g, respectively. cat -1 ·h -1 and 2375ug·g cat -1 ·h -1 .
[0094] Example 7
[0095] 1. 1%Ru-5%S2O8 2- Preparation of ZrO2-HZSM-5-3 catalyst:
[0096] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=80) and add them to the mixed solution, and stir at room temperature for 7 h;
[0097] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5-3 carrier;
[0098] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0099] (4) Take 0.0104g of ruthenium trichloride and dissolve it in 15mL of deionized water. After ultrasonication for 15min, add 0.5g of carrier to the solution. After ultrasonication for 15min, add 2mL of sodium borohydride solution for reduction. Continue stirring for 10min and filter. Then, vacuum dry at 110℃ for 12h to obtain the desired 1%Ru-5%S2O8. 2- / ZrO2-HZSM-5-3 catalyst;
[0100] 2. 1%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5-3 catalyst:
[0101] The prepared 1%Ru-5%S2O8 2- / ZrO2-HZSM-5-3 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 1% Ru-5% S2O8 2- / ZrO2-HZSM-5-3 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 52.79%, 47.21% and 875ug·g, respectively. cat -1 ·h -1 and 1125ug·g cat -1 ·h -1 .
[0102] Example 8
[0103] 1. 0.3%Ru-5%S2O8 2- Preparation of ZrO2-HZSM-5 catalyst:
[0104] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h.
[0105] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5 catalyst.
[0106] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0107] (4) 0.0031 g of ruthenium trichloride was dissolved in 15 mL of deionized water. After ultrasonication for 15 min, 0.5 g of the carrier was added to the solution. After ultrasonication for another 15 min, 1 mL of sodium borohydride solution was added for reduction. After stirring for 10 min, the mixture was filtered and then vacuum dried at 110 ° C for 12 h to obtain the desired 0.3% Ru-5% S2O8. 2- / ZrO2-HZSM-5 catalyst.
[0108] 2. 0.3%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5 catalyst:
[0109] The prepared 0.3%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 0.3%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 58.97%, 41.03% and 475ug·g, respectively. cat -1 ·h -1 and 475ug·g cat -1 ·h -1 .
[0110] Example 9
[0111] 1. 0.5%Ru-5%S2O8 2- Preparation of ZrO2-HZSM-5 catalyst:
[0112] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h.
[0113] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5 catalyst.
[0114] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0115] (4) 0.0052 g of ruthenium trichloride was dissolved in 15 mL of deionized water. After ultrasonication for 15 min, 0.5 g of the carrier was added to the solution. After ultrasonication for another 15 min, 1 mL of sodium borohydride solution was added for reduction. After stirring for 10 min, the mixture was filtered and then dried under vacuum at 110 °C for 12 h to obtain the desired 0.5% Ru-5% S2O8. 2- / ZrO2-HZSM-5 catalyst.
[0116] 2. 0.5%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5 catalyst:
[0117] The prepared 0.5%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 0.5%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 52.48%, 47.52% and 1575ug·g respectively. cat -1 ·h -1 and 2050ug·g cat -1 ·h -1 .
[0118] Example 10
[0119] 1. 3%Ru-5%S2O8 2- Preparation of ZrO2-HZSM-5 catalyst:
[0120] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h.
[0121] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5 catalyst.
[0122] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0123] (4) 0.0311 g of ruthenium trichloride was dissolved in 15 mL of deionized water. After ultrasonication for 15 min, 0.5 g of the carrier was added to the solution. After ultrasonication for another 15 min, 1 mL of sodium borohydride solution was added for reduction. After stirring for 10 min, the mixture was filtered and then dried under vacuum at 110 ° C for 12 h to obtain the desired 3% Ru-3% S2O8. 2- / ZrO2-HZSM-5 catalyst.
[0124] 2. 3%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5 catalyst:
[0125] The prepared 3%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 3%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst was placed in a 50mL high-pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 71.96%, 28.04% and 3125ug·g, respectively. cat -1 ·h -1 and 1750ug·g cat -1 ·h -1 .
[0126] Embodiment 11
[0127] 1. 5%Ru-5%S2O8 2- Preparation of ZrO2-HZSM-5 catalyst:
[0128] (1) Weigh 0.12 g of ammonium persulfate and dissolve it in 50 mL of methanol with stirring; after ultrasonic treatment for 15 min, weigh 1 g of zirconium dioxide and 1 g of HZSM-5 molecular sieve (SiO2 / Al2O3=50) and add them to the mixed solution, and stir at room temperature for 7 h.
[0129] (2) The obtained precipitate was filtered and dried at 110°C for 12 h, then calcined in a muffle furnace at 550°C for 3 h, and cooled to room temperature to obtain 5% S2O8 2- / ZrO2-HZSM-5 catalyst.
[0130] (3) dissolving 0.1 g of sodium borohydride in 10 mL of deionized water to prepare a 10 g / L sodium borohydride solution;
[0131] (4) 0.0518 g of ruthenium trichloride was dissolved in 15 mL of deionized water. After ultrasonication for 15 min, 0.5 g of the carrier was added to the solution. After ultrasonication for another 15 min, 1 mL of sodium borohydride solution was added for reduction. After stirring for 10 min, the mixture was filtered and then dried under vacuum at 110 ° C for 12 h to obtain the desired 5% Ru-3% S2O8. 2- / ZrO2-HZSM-5 catalyst.
[0132] 2. 5%Ru-5%S2O8 2- / Application of ZrO2-HZSM-5 catalyst:
[0133] The prepared 5%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst is used for liquid-solid phase reaction of CO2 hydrogenation. Weigh 20 mg 5%Ru-5%S2O8 2- / ZrO2-HZSM-5 catalyst was placed in a 50mL high pressure reactor, and 10mL of water was added as solvent. 2.0MPa of reaction gas (H2:CO2=3.0) was charged and reacted at 160℃ for 2h. The selectivity and yield of methanol and ethanol were 80.50%, 19.50% and 3375ug·g respectively. cat -1 ·h -1 and 1175ug·g cat -1 ·h -1 .
[0134] Table 1 Pore structure characteristics of samples
[0135]
[0136]
[0137] By comparing the SEM characterization results of the catalysts with different ZrO2-HZSM-5 ratios prepared in Examples 1 to 5 ( Figure 1 ) found that: ZrO2 presents an irregular honeycomb shape, HZSM-5 presents a regular plate shape, and Ru metal is evenly distributed on the surface. The catalyst N2 adsorption-desorption isotherm ( Figure 2 ) and pore size distribution curve ( Figure 3 ) and the pore structure characteristics of the samples (Table 1), it can be seen that the catalyst pore size mainly exists in micropores and mesopores. When ZrO2-HZSM-5 is 1, its mesopore distribution is more, and it also has the largest ethanol selectivity and ethanol yield ( Fig.12 ). Catalyst XRD characterization results ( Figure 4 ) shows mainly the characteristic peaks of ZrO2 and HZSM-5, and the diffraction peak of metallic Ru is very weak, which may be due to the high dispersion of Ru on the support.
[0138] By comparing the N2 adsorption-desorption isotherms of HZSM-5 catalysts with different silicon-aluminum ratios prepared in Example 1 and Example 6-7 ( Figure 5 ) and pore size distribution curve ( Figure 6 ) and the pore structure characteristics of the samples (Table 1), it can be seen that the catalyst pore size is mainly present in micropores and mesopores. When the Si-Al ratio is 50, the mesopores are more distributed, and it also has the largest ethanol selectivity and ethanol yield ( Fig.13 ). Catalyst XRD characterization results ( Figure 7 ) shows mainly the characteristic peaks of ZrO2 and HZSM-5. The diffraction peaks of HZSM-5 are slightly different. The metal Ru is highly dispersed and the diffraction peaks are weak.
[0139] By comparing the SEM characterization results of catalysts with different Ru metal loadings prepared in Example 1 and Examples 8-11 ( Figure 8 ) found that with the increase of loading, Ru metal agglomerates on the surface. Through the catalyst N2 adsorption-desorption isotherm ( Fig. 9 ) and pore size distribution curve ( Fig.10 ) and the pore structure characteristics of the samples (Table 1), it can be seen that the catalyst pore size mainly exists in micropores and mesopores. When the metal Ru loading is 1%, its mesopore distribution is more, and it also has the largest ethanol selectivity and ethanol yield ( Fig.14 ). Catalyst XRD characterization results ( Fig.11 ) shows that the metallic Ru is highly dispersed and its diffraction peak is difficult to observe.
[0140] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a ruthenium-based solid acid catalyst, characterized in that: The following steps are involved: (1) dissolving ammonium persulfate in methanol to prepare an ammonium persulfate methanol solution; after ultrasonication for 10 to 20 minutes, adding zirconium dioxide and HZSM-5 molecular sieve to the solution respectively, and then stirring at room temperature for 6 to 8 hours; the SiO2 / Al2O3 of the HZSM-5 molecular sieve is 50; (2) The precipitate obtained in step (1) was filtered and dried, and then calcined at 550°C for 3h to obtain S2O8 2- / ZrO2-HZSM-5 support; (3) S2O8 2- / ZrO2-HZSM-5 carrier was added to the ruthenium salt aqueous solution, ultrasonicated, and reduced by adding sodium borohydride solution. After stirring for 10 minutes, it was filtered and then vacuum dried to obtain the desired Ru-S2O8 2- / ZrO2-HZSM-5 catalyst, wherein the Ru loading amount is 1%.
2. The method for preparing a ruthenium-based solid acid catalyst according to claim 1, characterized in that: The mass ratio of the zirconium dioxide to the HZSM-5 molecular sieve is 0.5-1.5:1.5-0.
5.
3. The method for preparing a ruthenium-based solid acid catalyst according to claim 1, characterized in that: The concentration of the ammonium persulfate methanol solution is 0.0024 g / mL.
4. The method for preparing a ruthenium-based solid acid catalyst according to claim 1, characterized in that: The ruthenium salt is ruthenium trichloride.
5. The method for preparing a ruthenium-based solid acid catalyst according to claim 1, characterized in that: The vacuum drying was carried out at a temperature of 110° C. and for a period of 12 h.
6. A ruthenium-based solid acid catalyst prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the catalyst according to claim 6 in producing ethanol by hydrogenation of carbon dioxide.
8. The use according to claim 7, characterized in that: The following steps are involved: A ruthenium-based solid acid catalyst and a solvent are placed in a reaction kettle; 0.4-2.8 MPa of reaction gas is charged into the reaction kettle, and the molar ratio of H2:CO2 in the reaction gas is 2.5-3.5; the reaction temperature is controlled to be 140-240°C, and the reaction time is 1-5 hours.
9. The use according to claim 8, characterized in that: The solvent is water.
10. The use according to claim 8, characterized in that: The pressure of the reaction gas is 2 MPa, the reaction temperature is 160° C., and the reaction time is 2 h.
Citation Information
Patent Citations
Catalyst for hydrolysis of cellulose and / or reduction of hydrolysis product thereof, and method for producing sugar alcohol from cellulose
CA2644074A1
Preparation of high-activity ruthenium catalyst and application of high-activity ruthenium catalyst in room-temperature catalytic hydrogenation
CN110947379A
Preparation method and application of high-activity HZSM-5 supported solid superacid catalyst
CN116786155A
Preparation method and application of high-activity peroxypersulfate type solid superacid catalyst
CN118122343A
Cited By
Ruthenium on low acidity zirconia support
WO2026047336A1