Metal additive manufacturing keyhole eliminating method based on interlayer self-healing

Through the interlayer self-healing method, keyhole defects in metal additive manufacturing are controlled and eliminated, and the problem of keyhole defects affecting the forming quality is solved, and efficient keyhole removal and material forming quality improvement are achieved.

CN119076975AActive Publication Date: 2024-12-06NORTHWESTERN POLYTECHNICAL UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411303967.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

Keyhole defects often occur in metal additive manufacturing, resulting in the impact of forming quality and service performance. The existing technology is costly and has limited spatial and temporal resolution, making it difficult to effectively control and eliminate these defects.

Method used

Using interlayer self-healing method, through single-channel and multi-channel forming experiments, self-healing criteria and forming parameters design, the autonomous control and complete elimination of keyholes is achieved, including obtaining the keyhole defect distance and melt pool position. Adjust the multi-forming parameters and combine post-treatment surface cutting to ensure that the sample has no internal keyholes.

Benefits of technology

It greatly improves the forming quality of metal additive manufacturing, shortens production cycles, reduces trial and error costs, provides a wider process window, increases the success rate of material preparation of different parameters, and achieves effective elimination of keyhole defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076975A_ABST
    Figure CN119076975A_ABST
Patent Text Reader

Abstract

The invention discloses a metal additive manufacturing keyhole eliminating method based on interlayer self-healing, which comprises the following steps: step 1, carrying out a single-channel forming experiment under multi-parameter combination, and judging a keyhole defect generation position; 2, on the basis of the experimental parameters in the step 1, multiple forming experiments under multi-parameter combination are conducted, and self-healing conditions of multiple formed keyholes are provided according to the keyhole defect self-healing condition; 3, aiming at genetic keyhole defects, providing a corresponding keyhole self-healing active control strategy through forming parameter design, and obtaining an additive sample without an internal keyhole; and 4, carrying out post-treatment on the sample obtained in the step 3 to completely eliminate the keyhole. By means of the interlayer self-healing metal additive manufacturing keyhole eliminating method, appropriate printing parameters can be rapidly obtained to prepare a compact sample without keyhole defects inside, and a theoretical basis is expected to be provided for active control over technological conditions in the online detection process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention belongs to the technical field of additive manufacturing metal materials, and in particular relates to a method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing. Background technology:

[0002] Metal additive manufacturing technology achieves near-net-shape formation of material integration through computer-aided layer-by-layer construction. It has the advantages of short production cycle and high material utilization rate. It has been widely used in many fields such as aerospace, biomedicine, etc., such as aircraft engine fuel nozzles, blades, and bearing seats, and has broad development prospects. However, the thermodynamic and kinetic behaviors of the melt pool in the metal additive manufacturing process are complex and involve many forming process parameters. Improper selection of process parameters can easily lead to the generation of keyhole defects inside metal additive components, thereby affecting the forming quality and service performance of the components.

[0003] Due to the layer-by-layer forming characteristics of additive manufacturing, if the keyhole defects caused by inappropriate process parameters in a single forming pass are not controlled in time, as the forming passes increase, the defects will remain inside the sample. At present, synchrotron radiation X-ray imaging technology can observe the forming morphology of the additive manufacturing process layer by layer, but the cost is high and the temporal and spatial resolution is limited. Under this premise, it is urgent to propose a low-cost keyhole defect control method for the additive manufacturing process, and realize the active elimination of keyhole defects by optimizing the process parameters. Summary of the invention:

[0004] In order to solve the problem of keyhole defects existing inside metal additively manufactured components, the present invention proposes a method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing. The method proposes a self-healing criterion for keyhole defects through single-pass forming and multi-pass forming experiments, actively controls the self-healing of genetic keyholes through forming parameter design, obtains a sample without internal keyholes, and achieves complete elimination of the keyhole through post-processing.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows: The present invention provides a method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing, the method comprising the following steps: Step 1: subjecting metal powder to a single-pass additive forming process under a multi-parameter combination to obtain a single-pass forming specimen, and obtaining a vertical distance between the bottom of the keyhole defect of the single-pass forming specimen and the bottom of the molten pool; Step 2: Based on the forming process parameters in step 1, a multi-pass additive forming process is performed under a multi-parameter combination to obtain a multi-pass forming sample, and the vertical distance from the bottom of the deepest molten pool of the forming layer at the junction of the two adjacent molten pools at the lowest relative to the forming plane and the powder bed thickness are obtained; Step 3: according to the vertical distance between the bottom of the keyhole defect and the bottom of the molten pool, the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer, and the thickness of the powder bed, the self-healing conditions of the multi-channel formed keyholes are obtained; Step 4: According to the self-healing condition of the multi-pass forming keyhole, the multi-pass forming parameters are adjusted so that the keyhole of the multi-pass forming sample can self-heal during the forming process, and finally an additive sample without an internal keyhole is obtained; Step 5: Post-process the additive sample obtained in step 4 to completely eliminate the keyhole.

[0006] As a further illustration of the present invention, the metal includes at least one of a titanium alloy, an aluminum alloy, and an intermetallic compound.

[0007] As a further illustration of the present invention, in step 1, the parameter selection of the single-pass additive manufacturing includes powder particle size, laser power, scanning rate, powder bed thickness and heat source type; As a further illustration of the present invention, the heat source is one of a laser, a plasma beam, and an electron beam.

[0008] As a further illustration of the present invention, in step 1, the method for obtaining the vertical distance between the bottom of the keyhole defect of the single-pass forming sample and the bottom of the molten pool is: Performing metallographic or scanning electron microscopy characterization on the single-pass formed sample to obtain the locations of the molten pool and keyhole defects of the single-pass formed sample; According to the positions of the molten pool and the keyhole defect of the single-pass forming sample, the vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is obtained.

[0009] As a further explanation of the present invention, in step 2, based on the forming process parameters in step 1, a multi-pass additive forming process under a multi-parameter combination is performed to obtain a multi-pass forming sample, specifically: On the basis of maintaining the single-pass forming parameter selection of step 1, the scanning spacing and scanning strategy are coupled to perform a multi-pass additive forming process to obtain a multi-pass forming specimen.

[0010] As a further explanation of the present invention, in step 2, the method for obtaining the vertical distance from the bottom of the deepest molten pool of the forming layer to the junction of the two adjacent molten pools at the lowest relative to the forming plane is: Performing metallographic or scanning electron microscopy characterization on the multi-pass formed sample to obtain the molten pool position of the multi-pass formed sample; According to the molten pool position of the multi-pass forming sample, the vertical distance between the junction of the two adjacent molten pools lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer is obtained.

[0011] As a further explanation of the present invention, in step 3, the method for determining the self-healing condition of the multi-channel formed keyhole is specifically: The vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is ≥ the vertical distance between the junction of the two adjacent molten pools with respect to the lowest forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed layer, and the keyhole defect is in a self-healing mode; The vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is ≤ the vertical distance between the junction of the two adjacent molten pools lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed. The keyhole defect is a genetic mode.

[0012] As a further illustration of the present invention, in step 4, when the keyhole defect meets the conditions of the self-healing mode, the multi-pass forming parameters of step 2 are maintained to select a multi-pass additive forming process, so that the keyhole of the multi-pass formed sample can self-heal during the forming process, and finally an additive sample without an internal keyhole is obtained.

[0013] As a further illustration of the present invention, in step 4, when the keyhole defect meets the condition of the inheritance mode, the multi-pass forming parameters are adjusted to perform the multi-pass additive forming process until the keyhole defect of the multi-pass formed sample meets the self-healing mode, and the multi-pass forming parameters that meet the self-healing mode are maintained to select the multi-pass additive forming process, so that the keyhole of the multi-pass formed sample can self-heal during the forming process, and finally an additive sample without an internal keyhole is obtained; The multi-pass forming parameters include scanning spacing and scanning strategy.

[0014] As a further illustration of the present invention, in step 5, the post-processing of the additive sample is surface cutting.

[0015] Compared with the prior art, the present invention has the following beneficial technical effects: The present invention greatly expands the window of metal additive manufacturing, improves the quality of material forming, greatly shortens the production cycle, and reduces the cost of trial and error. The present invention transfers the internal keyhole defects to the surface through the interlayer self-healing keyhole elimination method, and obtains a keyhole-free specimen through subsequent surface cutting. This method provides a wider process window and increases the success rate of material preparation with different parameters. Description of the drawings:

[0016] Figure 1 This is a diagram of the mechanism of keyhole defect generation in the present invention; Figure 2 This is a diagram of the keyhole self-healing control mechanism in the present invention; Figure 3 Schematic diagram of surface cutting process of a sample without an internal keyhole in Examples 1 and 2 of the present invention; Figure 4This is a scanning electron microscope image of TC4 laser powder bed melting single-pass forming in Example 1 of the present invention; Figure 5 This is a scanning electron microscope image of TC4 laser powder bed fusion single-layer multi-pass forming in Example 1 of the present invention; Figure 6 This is a scanning electron microscope image of TC4 laser powder bed fusion multi-layer single-pass forming in Example 1 of the present invention; Figure 7 This is a scanning electron microscope image of AlSi10Mg laser powder bed melting single layer multi-pass forming in Example 2 of the present invention;

[0017] Figure 8 This is a flow chart of the keyhole elimination method of metal additive manufacturing based on interlayer self-healing of the present invention. Specific implementation method:

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The embodiment of the present invention provides a method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing, comprising the following steps: Step 1: The metal powder is subjected to a single-pass additive forming process under a multi-parameter combination to obtain a single-pass forming specimen, and the vertical distance between the bottom of the keyhole defect of the single-pass forming specimen and the bottom of the molten pool is obtained. The process specifically includes: (a) Modeling: Use 3D modeling software to design a single-pass forming model, then slice the model layer by layer and generate the corresponding engineering files.

[0020] (b) Powder drying: The metal powder raw materials are screened and the screened powder is placed in a drying box for drying.

[0021] (c) Install the substrate and scraper: Select a metal substrate with a clean and flat surface that is the same or similar to the printing material. Fix the substrate and install the scraper.

[0022] (d) Gas washing: Close the equipment, introduce high-purity argon gas, control the oxygen content in the forming chamber below 50ppm, and start printing.

[0023] (e) Characterization: After printing, the substrate is removed and the single-pass formed sample is characterized by metallography or scanning electron microscopy to obtain information such as the molten pool depth, width, and keyhole defect location.

[0024] like Figure 1As shown in the figure, during the laser additive manufacturing process, the recoil pressure caused by metal vaporization acts on the surface of the melt to form a steam cavity. This cavity is in an unstable fluctuation with the intrinsic oscillation of the laser input frequency and the occurrence of melt flow, splashing and other phenomena. If the sharp bottom of the steam cavity vibrates and collapses, it will entrain the metal vapor and remain at the bottom of the molten pool. If it does not overflow in time before solidification, it will be trapped in the molten pool to form a keyhole defect.

[0025] The metal in step 1 includes at least one of titanium alloy, aluminum alloy, and intermetallic compound, preferably one of AlSi10Mg and TC4. The parameter selection of single-pass additive manufacturing includes powder particle size, laser power, scanning rate, powder bed thickness and heat source type. Preferably, the powder particle size is between 15 and 53 μm and conforms to the normal distribution, the laser power is 50 to 500 W, the scanning rate is 20 to 1600 mm / s, and the powder bed thickness is 40 to 90 μm. Preferably, the heat source is one of laser, plasma beam, and electron beam.

[0026] Step 2: Based on the forming process parameters of step 1 (coupling the scanning spacing and scanning strategy on the basis of maintaining the single-pass forming parameter selection of step 1), a multi-pass additive forming process under a multi-parameter combination is performed to obtain a multi-pass forming sample, and the vertical distance from the bottom of the deepest molten pool of the forming layer at the junction of the two adjacent molten pools at the lowest relative to the forming plane and the powder bed thickness are obtained. The process specifically includes: (a) Modeling: Use 3D modeling software to design a multi-pass forming model, then slice the model layer by layer and generate the corresponding engineering files.

[0027] (b) Powder drying: The metal powder raw materials are screened and the screened powder is placed in a drying box for drying.

[0028] (c) Install the substrate and scraper: Select a metal substrate with a clean and flat surface that is the same or similar to the printing material. Fix the substrate and install the scraper.

[0029] (d) Gas washing: Close the equipment, introduce high-purity argon gas, control the oxygen content in the forming chamber below 50ppm, and start printing.

[0030] (e) Characterization: After printing, the substrate is removed and the multi-pass formed sample is characterized by metallography or scanning electron microscopy to obtain the molten pool position information of the multi-pass formed sample (the vertical distance from the junction of the two adjacent molten pools at the lowest level of the forming plane to the bottom of the deepest molten pool of the forming layer) and to determine the self-healing of the keyhole defect.

[0031] Step 3: According to the vertical distance between the bottom of the keyhole defect and the bottom of the molten pool, the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer, and the thickness of the powder bed, the self-healing conditions of the multi-pass formed keyholes are obtained; Figure 2 As shown in the figure, the keyhole self-healing judgment condition is proposed based on the relationship between the distance between the keyhole defect and the bottom of the molten pool, the distance between the junction of the molten pool and the bottom of the molten pool, and the thickness of the powder bed.

[0032] The above-mentioned method for determining the self-healing condition of the multi-channel formed keyhole is specifically as follows: The vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is ≥ the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed. The keyhole defect is in self-healing mode. The vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is ≤ the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed. The keyhole defect is a genetic mode.

[0033] The above-mentioned self-healing mode means that the keyhole defect can be eliminated autonomously during the multi-pass printing process; the genetic mode means that the keyhole defect cannot be eliminated naturally by evolution during the multi-pass printing process.

[0034] Step 4: According to the self-healing conditions of the multi-pass forming keyhole, the multi-pass forming parameters are adjusted so that the keyhole of the multi-pass forming specimen can self-heal during the forming process, and finally an additive specimen without an internal keyhole is obtained. Specifically: When the keyhole defect meets the conditions of the self-healing mode, the multi-pass forming parameters of step 2 are maintained to select a multi-pass additive forming process, so that the keyhole of the multi-pass formed specimen can self-heal during the forming process, and finally an additive specimen without an internal keyhole is obtained.

[0035] When the self-healing conditions are met, combined Figure 1 The post-printing molten pool will remelt the keyhole in the previous molten pool, causing the trapped gas to float up or even overflow directly, achieving the effect of self-healing of the keyhole defect.

[0036] When the keyhole defect meets the conditions of the inheritance mode, the inherited keyhole defect self-healing active control is performed, that is, the multi-channel forming parameters are adjusted to perform the multi-channel additive forming process until the keyhole defect of the multi-channel forming sample meets the self-healing mode, and then the multi-channel forming parameters that meet the self-healing mode are maintained to select the multi-channel additive forming process, so that the keyhole of the multi-channel forming sample can self-heal during the forming process, and finally an additive sample without an internal keyhole is obtained; wherein the multi-channel forming parameters include scanning spacing and scanning strategy. Preferably, the scanning spacing is 90~120μm; the scanning strategy can be selected from one of the unidirectional scanning strategy and the round-trip scanning strategy.

[0037] Specifically, the above-mentioned genetic keyhole defect self-healing active control process includes: (a) Forming parameter design: According to the distribution of defects under different process parameters in single-pass forming in step 1, the multi-pass forming parameter design is adjusted, mainly by changing the scanning interval to adjust the vertical distance from the bottom of the deepest molten pool of the forming layer to the junction of the two adjacent molten pools relative to the lowest forming plane, and by changing the layer thickness.

[0038] (b) Repeat the modeling, powder baking, substrate and scraper installation, gas washing, and characterization steps in step 2 to determine whether the keyhole self-healing condition satisfies the self-healing mode, until the keyhole defect of the multi-pass formed sample satisfies the self-healing mode. Then, the multi-pass forming parameters that meet the self-healing mode are maintained to select the multi-pass additive forming process, so that the keyhole of the multi-pass formed sample can self-heal during the forming process, and the keyhole is transferred from the inside of the sample to the surface of the sample.

[0039] Step 5: Post-process the additive sample obtained in step 4 to completely eliminate the keyhole.

[0040] The keyhole self-healing active control sample is mechanically cut to remove surface defects. Preferably, the cutting depth is greater than 2 to 5 times the thickness of the powder bed, for example, the cutting depth is 1 mm. The principle of the cutting process is as follows: Figure 3 As shown, the keyhole is completely eliminated and a completely dense sample is obtained.

[0041] The following is described in conjunction with specific embodiments: Unless otherwise specified, the materials, tools, equipment, etc. used in the embodiments of the present invention are all commercially available.

[0042] The metal material in the embodiment of the present invention is additively manufactured using a laser powder bed melting process using a BLT-S210 device. Example 1

[0043] Step 1: Preparation and characterization of single-pass forming specimens (a) Modeling: Use 3D modeling software to design a single-pass forming model with a model length of 5 mm. Design the single-pass forming process parameters, laser power of 100 W, scanning rate of 50 mm / s, powder bed thickness of 40 μm, and then slice the model layer by layer to generate the corresponding engineering files.

[0044] (b) Powder drying: The TC4 metal powder raw material is screened to obtain a spherical powder with a maximum particle size not exceeding 2 to 3 times the thickness of its powder bed, and then placed in a drying oven for drying. The spherical powder with a particle size range of 15 to 53 μm and a normal distribution is obtained by screening and dried at 100°C for 2 hours.

[0045] (c) Install the substrate and scraper: Select a clean and flat metal substrate with the same or similar composition as the printing material. Select a clean and smooth TC4 substrate with a thickness greater than 17 mm. Fix it on the additive manufacturing printing work platform. Place the dried metal powder in the equipment powder supply bin and install the scraper.

[0046] (d) Gas washing: Use a manually operated scraper to evenly spread the first layer of powder on the workbench, then seal the equipment, introduce high-purity argon gas, control the oxygen content in the forming chamber below 50ppm, and start printing.

[0047] (e) Characterization: After printing, the substrate is removed and the single-pass formed sample is characterized by metallography or scanning electron microscopy, such as Figure 4 Shown is a scanning electron microscope image of TC4 single-channel forming.

[0048] The molten pool width, depth and defect location of the single-track forming specimen were characterized. The molten pool width was 416.33 μm, the molten pool depth was 819.05 μm, and the vertical distance from the bottom of the defect to the bottom of the molten pool was 253.06 μm.

[0049] Step 2, preparation and characterization of multi-pass forming specimens: (a) Modeling: Use 3D modeling software to design a multi-pass forming model with a model length of 5 mm. Design the single-layer multi-pass forming process parameters, laser power 100 W, scanning rate 50 mm / s, powder bed thickness 40 μm, scanning spacing 150 μm, number of printing passes 5, and then slice the model layer by layer to generate the corresponding engineering files.

[0050] (b) Powder drying: The TC4 metal powder raw material is screened to obtain a spherical powder with a maximum particle size not exceeding 2 to 3 times the thickness of its powder bed, and then placed in a drying oven for drying. The spherical powder with a particle size range of 15 to 53 μm and a normal distribution is obtained by screening and dried at 100°C for 2 hours.

[0051] (c) Install the substrate and scraper: Select a clean and flat metal substrate with the same or similar composition as the printing material. Select a clean and smooth TC4 substrate with a thickness greater than 17 mm. Fix it on the additive manufacturing printing work platform. Place the dried metal powder in the equipment powder supply bin and install the scraper.

[0052] (d) Gas washing: Use a manually operated scraper to evenly spread the first layer of powder on the workbench, then seal the equipment, introduce high-purity argon gas, control the oxygen content in the forming chamber below 50ppm, and start printing.

[0053] (e) Characterization: After printing, the substrate is removed and the multi-pass formed samples are characterized by metallography or scanning electron microscopy, such as Figure 5Shown is a scanning electron microscope image of TC4 single-layer multi-channel forming.

[0054] exist Figure 5 In the figure, the defects existing in single-pass forming are self-healed in single-layer multi-pass forming. The vertical distance from the junction of the two adjacent molten pools with the lowest level relative to the forming plane to the bottom of the deepest molten pool of the forming layer is calculated to be 73.34 μm.

[0055] In step 1, the vertical distance between the bottom of the defect and the bottom of the molten pool is 253.06 μm. In step 2, the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer is 73.34 μm. Therefore, the following defect self-healing judgment conditions are proposed: The vertical distance between the bottom of the defect and the bottom of the molten pool is ≥ the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed. The defect is in self-healing mode. The vertical distance between the bottom of the defect and the bottom of the molten pool is ≤ the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed. The defect is a genetic mode.

[0056] Step 3, active control of genetic keyhole defect self-healing: (a) Modeling: A multi-pass forming model with a model length of 5 mm was designed using 3D modeling software. The multi-pass forming process parameters were designed to meet the keyhole self-healing conditions, with a laser power of 100 W, a scanning rate of 50 mm / s, a powder bed thickness of 40 μm, and 5 printing passes. The model was then sliced ​​layer by layer and the corresponding engineering files were generated.

[0057] (b) Powder drying: The TC4 metal powder raw material is screened to obtain a spherical powder with a maximum particle size not exceeding 2 to 3 times the thickness of its powder bed, and then placed in a drying oven for drying. The spherical powder with a particle size range of 15 to 53 μm and a normal distribution is obtained by screening and dried at 100°C for 2 hours.

[0058] (c) Install the substrate and scraper: Select a clean and flat metal substrate with the same or similar composition as the printing material, select a clean and smooth TC4 substrate with a thickness greater than 17 mm, fix it on the additive manufacturing printing work platform, place the dried metal powder in the equipment powder supply bin, and install the scraper; (d) Gas washing: Use a manually operated scraper to evenly spread the first layer of powder on the workbench, then seal the equipment, introduce high-purity argon gas, control the oxygen content in the forming chamber below 50ppm, and start printing; (e) Characterization: After printing, the substrate is removed and the multi-pass formed samples are characterized by metallography or scanning electron microscopy, such as Figure 6 Shown is a scanning electron microscope image of TC4 multilayer single-channel forming.

[0059] exist Figure 6 In the multi-layer single-pass forming, the keyhole existing in the single-pass forming is transferred to the sample surface in the multi-layer single-pass forming, and the keyhole self-healing is achieved inside the sample. In the multi-layer single-pass forming, the vertical distance from the junction of the two adjacent molten pools with the lowest forming plane to the bottom of the deepest molten pool of the forming layer is 40μm in layer thickness, which meets the keyhole self-healing conditions, and the sample realizes active control of keyhole self-healing.

[0060] Step 4, post-manufacturing processing to completely eliminate the keyhole: The keyhole self-healing active control sample was mechanically cut to remove surface defects. The cutting depth was 1 mm. The principle of the cutting process is as follows: Figure 3 As shown, the keyhole is completely eliminated and a completely dense sample is obtained. Example 2

[0061] Based on the experiments of step 1 and step 2 in Example 1, the active control strategy of genetic keyhole defect self-healing in step 3 is changed, and the specific implementation method is as follows: (a) Modeling: A multi-pass forming model was designed using 3D modeling software with a model length of 5 mm. The single-layer multi-pass forming process parameters were designed so that the keyhole self-healing condition was not met. The laser power was 100 W, the scanning rate was 50 mm / s, the powder bed thickness was 40 μm, the scanning spacing was 180 μm, and the number of printing passes was 5. The model was then sliced ​​layer by layer and the corresponding engineering files were generated.

[0062] (b) Powder drying: The TC4 metal powder raw material is screened to obtain a spherical powder with a maximum particle size not exceeding 2 to 3 times the thickness of its powder bed, and then placed in a drying oven for drying. The spherical powder with a particle size range of 15 to 53 μm and a normal distribution is obtained by screening and dried at 100°C for 2 hours.

[0063] (c) Install the substrate and scraper: Select a clean and flat metal substrate with the same or similar composition as the printing material, select a clean and smooth TC4 substrate with a thickness greater than 17 mm, fix it on the additive manufacturing printing work platform, place the dried metal powder in the equipment powder supply bin, and install the scraper; (d) Gas washing: Use a manually operated scraper to evenly spread the first layer of powder on the workbench, then seal the equipment, introduce high-purity argon gas, control the oxygen content in the forming chamber below 50ppm, and start printing; (e) Characterization: After printing, the substrate is removed and the multi-pass formed samples are characterized by metallography or scanning electron microscopy, such as Figure 7 Shown is a scanning electron microscope image of TC4 single-layer multi-channel forming.

[0064] exist Figure 7 The defects existing in single-pass forming did not self-heal in single-layer multi-pass forming. The vertical distance from the junction of the two adjacent molten pools at the lowest relative to the forming plane to the bottom of the deepest molten pool of the forming layer was calculated to be 225.41 μm.

[0065] In Example 1, the vertical distance between the bottom of the defect and the bottom of the molten pool obtained in step 1 single-pass forming is 253.06 μm, verifying the keyhole self-healing judgment condition: The vertical distance between the bottom of the defect and the bottom of the molten pool is 253.06μm < the vertical distance between the junction of the two adjacent molten pools at the lowest forming plane and the bottom of the deepest molten pool of the forming layer is 225.41μm + the thickness of the powder bed is 40μm The keyhole self-healing condition is not met. Figure 7 The existence of an internal keyhole also verifies that keyhole inheritance occurs when the keyhole self-healing condition is not met.

[0066] Step 4, post-manufacturing processing to completely eliminate the keyhole: The keyhole self-healing active control sample was mechanically cut to remove surface defects. The cutting depth was 1 mm. The principle of the cutting process is as follows: Figure 3 As shown, the keyhole is completely eliminated and a completely dense sample is obtained.

[0067] The process from the proposal of multi-channel keyhole self-healing conditions to the active control of genetic keyhole self-healing, and finally the complete elimination of the keyhole to obtain a dense sample is as follows: Figure 8 shown.

[0068] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing, characterized in that: The method comprises the following steps: Step 1: subjecting metal powder to a single-pass additive forming process under a multi-parameter combination to obtain a single-pass forming specimen, and obtaining a vertical distance between the bottom of the keyhole defect of the single-pass forming specimen and the bottom of the molten pool; Step 2: Based on the forming process parameters in step 1, a multi-pass additive forming process is performed under a multi-parameter combination to obtain a multi-pass forming sample, and the vertical distance from the bottom of the deepest molten pool of the forming layer at the junction of the two adjacent molten pools at the lowest relative to the forming plane and the powder bed thickness are obtained; Step 3: according to the vertical distance between the bottom of the keyhole defect and the bottom of the molten pool, the vertical distance between the junction of the two adjacent molten pools at the lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer, and the thickness of the powder bed, the self-healing conditions of the multi-channel formed keyholes are obtained; Step 4: According to the self-healing condition of the multi-pass forming keyhole, the multi-pass forming parameters are adjusted so that the keyhole of the multi-pass forming sample can self-heal during the forming process, and finally an additive sample without an internal keyhole is obtained; Step 5: Post-process the additive sample obtained in step 4 to completely eliminate the keyhole.

2. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing according to claim 1, characterized in that: The metal includes at least one of titanium alloy, aluminum alloy and intermetallic compound.

3. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing according to claim 1, characterized in that: In step 1, the parameter selection of the single-pass additive manufacturing includes powder particle size, laser power, scanning rate, powder bed thickness and heat source type; The heat source is one of laser, plasma beam and electron beam.

4. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing as claimed in claim 1, characterized in that: In step 1, the method for obtaining the vertical distance between the bottom of the keyhole defect of the single-pass forming sample and the bottom of the molten pool is: Performing metallographic or scanning electron microscopy characterization on the single-pass formed sample to obtain the locations of the molten pool and keyhole defects of the single-pass formed sample; According to the positions of the molten pool and the keyhole defect of the single-pass forming sample, the vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is obtained.

5. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing as claimed in claim 1, characterized in that: In step 2, based on the forming process parameters in step 1, a multi-pass additive forming process under a multi-parameter combination is performed to obtain a multi-pass forming sample, specifically: On the basis of maintaining the single-pass forming parameter selection of step 1, the scanning spacing and scanning strategy are coupled to perform a multi-pass additive forming process to obtain a multi-pass forming specimen.

6. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing according to claim 1, characterized in that: In step 2, the method for obtaining the vertical distance from the bottom of the deepest molten pool of the forming layer to the junction of the two adjacent molten pools with respect to the lowest forming plane is: Performing metallographic or scanning electron microscopy characterization on the multi-pass formed sample to obtain the molten pool position of the multi-pass formed sample; According to the molten pool position of the multi-pass forming sample, the vertical distance between the junction of the two adjacent molten pools lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer is obtained.

7. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing as claimed in claim 1, characterized in that: In step 3, the method for determining the self-healing condition of the multi-channel formed keyhole is specifically as follows: The vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is ≥ the vertical distance between the junction of the two adjacent molten pools with respect to the lowest forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed layer, and the keyhole defect is in a self-healing mode; The vertical distance between the bottom of the keyhole defect and the bottom of the molten pool is ≤ the vertical distance between the junction of the two adjacent molten pools lowest relative to the forming plane and the bottom of the deepest molten pool of the forming layer + the thickness of the powder bed. The keyhole defect is a genetic mode.

8. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing as claimed in claim 7, characterized in that: In step 4, when the keyhole defect meets the conditions of the self-healing mode, the multi-pass forming parameters of step 2 are maintained to select a multi-pass additive forming process, so that the keyhole of the multi-pass formed specimen can self-heal during the forming process, and finally an additive specimen without an internal keyhole is obtained.

9. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing as claimed in claim 7, characterized in that: In step 4, when the keyhole defect meets the condition of the inheritance mode, the multi-pass forming parameters are adjusted to perform the multi-pass additive forming process until the keyhole defect of the multi-pass formed sample meets the self-healing mode, and the multi-pass additive forming process is performed while maintaining the multi-pass forming parameters that meet the self-healing mode, so that the keyhole of the multi-pass formed sample can self-heal during the forming process, and finally an additive sample without an internal keyhole is obtained; The multi-pass forming parameters include scanning spacing and scanning strategy.

10. The method for eliminating keyholes in metal additive manufacturing based on interlayer self-healing according to claim 1, characterized in that: In step 5, the post-processing of the additive sample is surface cutting.

Citation Information

Patent Citations

  • Method for testing laser metal direct forming based on self-healing mechanism

    CN101590571A

  • Preparation method of bionic impact-resistant multilayer composite gradient material based on amorphous alloy

    CN111299584A

  • Method for repairing defects of lap joint positions of adjacent sub-areas formed by selective laser melting

    CN111974990A

  • Method for machining part by using laser melting forming device

    CN113059188A

  • Laser additive manufactured AlCoCrFeNi2 eutectic high-entropy alloy and strengthening method thereof