Novel release agent for epoxy resin pultrusion process and preparation method thereof

By using new release agents composed of polymeric greases and other products in the epoxy resin pultrusion process, the problems of poor mold release effect and high temperature resistance of traditional release agents are solved, efficient mold release and wear resistance are achieved, and composite materials are improved. Surface quality and production efficiency.

CN119078050APending Publication Date: 2024-12-06SHANGHAI ZHONGJU TONGSHUO MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210249.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional epoxy resin release agents have problems such as poor mold release effect, impermanence to high temperature and high production costs in the pultrusion process, which affects the surface quality and mold life of the composite material, and has low production efficiency.

Method used

Using a new release agent, including polymeric oils, emulsifiers, salt forming agents, solvents, compatibilizers and film forming agents, it is prepared by polymerization reaction to form a wear-resistant and non-corrosive release layer, simplifying the formulation and improving storage stability.

Benefits of technology

It achieves a high strength and wear-resistant mold release capability, reduces the scrap rate and defect rate, extends the mold life, and improves production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119078050A_ABST
    Figure CN119078050A_ABST
Patent Text Reader

Abstract

The invention discloses a novel release agent for an epoxy resin pultrusion process and a preparation method thereof, the release agent is composed of polymerized grease, a solvent, an auxiliary agent and the like, the release agent has a good demolding effect, and the production efficiency and the product quality in the pultrusion process can be effectively improved. The invention further provides a simple and convenient production method, and the efficient epoxy resin release agent can be rapidly prepared. The high-temperature-resistant composite material release agent provided by the invention has the characteristics of good chemical stability, high temperature resistance and good storage stability, forms uniform missible oil through compounding of an emulsifier, has low interfacial tension, and has a substantive auxiliary effect on preparation of a composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of a release agent for demoulding, in particular to a novel release agent for epoxy resin pultrusion process and a preparation method thereof. Background Art

[0002] Composite materials, as a material with excellent properties such as light weight, high strength and corrosion resistance, have been widely used in modern industry. Pultrusion technology, as an important production process for composite materials, is also growing and developing. As an essential chemical additive in the pultrusion process of composite materials, release agents play a vital role in the pultrusion process. However, the role of release agents affects the development of the composite material pultrusion process. At present, there are several difficulties: First, in the pultrusion process, the plastic is squeezed and stretched in the mold, and it is easy to produce friction with the mold surface. If there is no release agent to reduce friction, it will cause adhesion between the mold and the plastic, making it difficult to demold. Second, without the friction-reducing effect of the release agent, it is easy to cause surface defects such as scratches and flaws, affecting the surface quality and appearance of the product; third, without the release agent to reduce friction, the demoulding force will increase, increasing the difficulty and risk of demoulding, which may cause mold damage or product deformation; fourth, the mold surface is damaged: in the pultrusion process, the high temperature and high pressure of the plastic are easy to cause wear and corrosion to the mold surface. Without the protective effect of the release agent, the service life of the mold will be shortened; fifth, it affects production efficiency: the release agent can reduce the friction resistance between the mold and the plastic, reduce the demoulding force, and improve production efficiency. If the release agent is not added, it may lead to reduced production efficiency and increased production costs.

[0003] The development trend of composite materials is good. As an important part of it, pultrusion technology is also constantly innovating and developing, providing important support and driving force for the development of modern industry. In the pultrusion process, epoxy resin release agent is an important auxiliary material. Traditional epoxy resin release agents have problems such as poor demoulding effect and high production cost. Therefore, it is necessary to provide a new epoxy resin release agent to solve the problems existing in the prior art. CN 103419308 A patent discloses an epoxy resin release agent, which includes polyvinyl alcohol, industrial alcohol, washing powder and water. The beneficial effects of the invention are: (1) the raw materials are easy to obtain, the preparation is easy, the product is non-toxic, and the demoulding effect is good; (2) since there is no imported material, the product technology is based on localization, the material source is wide, and the production cost is greatly reduced, but the release agent is not resistant to high temperature, which greatly limits the application of the product. Patent CN 111349308 A discloses a release agent for epoxy resin LED packaging material and its preparation method. The release agent is prepared by addition reaction of the following raw materials in parts by weight: low hydrogen silicone oil, olefin compound, platinum catalyst. As an additive, it can be directly added to the curing agent of epoxy resin LED packaging material and remain stable. However, the interfacial energy of the product is relatively high. Therefore, if a release agent with low interfacial energy, high mobility and high temperature resistance can be prepared, it will be of great significance in the field of release agents and have broad market prospects. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the problem solved by the present invention is to provide a new release agent for epoxy resin pultrusion process which has strong demoulding ability, good wear resistance and is non-corrosive to the mold, and a preparation method thereof.

[0005] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0006] A novel release agent for epoxy resin pultrusion process comprises the following components by weight: 25-200 parts by weight of polymerized oil, 10-50 parts by weight of emulsifier, 5-10 parts by weight of salt former, 2-5 parts by weight of solvent, 2-5 parts by weight of compatibilizer, 2-5 parts by weight of film former and 2-5 parts by weight of dispersant.

[0007] Furthermore, the following components are included by weight: 70 parts by weight of polymerized oil, 15 parts by weight of emulsifier, 5 parts by weight of salt former, 2 parts by weight of solvent, 2 parts by weight of compatibilizer, 2 parts by weight of film former and 2 parts by weight of dispersant.

[0008] Furthermore, the polymerized oil is a diene terminal polymer.

[0009] Furthermore, the emulsifier is one or more of glyceryl monostearate, sucrose fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, sodium stearoyl lactylate, calcium stearoyl lactylate, phospholipids, propylene glycol fatty acid ester, soybean lecithin, sodium lauryl sulfate, polyoxyethylene fatty acid ester, polyglycerol fatty acid ester, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyoxyethylene castor oil, polyoxypropylene glycerol ether, polyoxyethylene oleate, potassium stearate, and sodium dodecylbenzene sulfonate.

[0010] Furthermore, the salt-forming agent is one or more of sodium chloride, sodium sulfate, potassium nitrate, ammonium sulfate, ammonium chloride, barium chloride, ammonium carbonate, sodium phosphate, potassium phosphate, and sodium acetate.

[0011] Furthermore, the solvent is at least one of heptane, isoheptane, octane, isooctane, nonane, isononane, decane, isodecane, undecane, dodecane, tridecane, and tetradecane.

[0012] Furthermore, the film-forming agent is one or more of polyvinyl alcohol, polyacrylamide, sodium carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, ethyl cellulose, polyethylene glycol, povidone, gelatin, gum arabic, starch, rosin, terpene resin, phenolic resin, epoxy resin, polyester resin, polyurethane resin, acrylic resin, and silicone resin.

[0013] Furthermore, the dispersant is potassium dodecyl phosphate.

[0014] A method for preparing polymerized grease in a novel release agent for epoxy resin pultrusion process, comprising the following steps:

[0015] (1) Raw material preparation: select natural vegetable oil and purify it;

[0016] (2) Initiator selection: Select the initiator tert-butyl oxybenzoate to start the polymerization reaction;

[0017] (3) Preparation of reaction system: Mixing monomer, initiator and solvent in a reaction vessel;

[0018] (4) Nitrogen protection: The reaction is carried out under a nitrogen atmosphere to avoid interference from oxygen;

[0019] (5) heating reaction: heating the reaction system to a temperature of 80 to 120° C. to promote the polymerization reaction;

[0020] (6) Cooling: After the polymerization reaction is completed, cool to room temperature;

[0021] (7) Product separation: Separate the polymerized oil by precipitation, filtration, and centrifugation;

[0022] (8) Purification: washing the polymerized oil with a solvent to remove unreacted raw materials and by-products;

[0023] (9) Drying: Drying the polymerized oil in a vacuum to remove the residual solvent and obtain the polymerized oil;

[0024] (10) Preparation of release agent: polymerized oil, emulsifier, salt-forming agent, solvent, compatibilizer, film-forming agent and dispersant are mixed and heated to obtain a release agent.

[0025] The polymerized oil monomers include: methyl methacrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, cyclohexyl acrylate, n-butyl methacrylate, isopropyl methacrylate, methyl phenyl acrylate, and two of the styrene monomers.

[0026] The simplified structural formula of the polymer grease is shown below:

[0027]

[0028] Among them, R1 and R2 are C6~C 12 Methyl; x and y are natural numbers, and 30≤x+y≤1000.

[0029] The beneficial effects of the present invention are as follows:

[0030] 1. The double bonds of the monomers of the reactive release agent of the present invention are cross-linked under the action of the initiator during the composite material molding process to form a complete, uniform, and high-strength release layer. The coating formed by the release agent of the present invention has strong demoulding ability, good wear resistance, no corrosion to the mold, and does not affect the subsequent painting or electroplating process of the product.

[0031] 2. The microscopic regular "cage-shaped" or "double-plywood-shaped" geometric structure improves the surface quality of the product and reduces the scrap rate and defect rate.

[0032] 3. Since the present invention uses the high temperature of 120-200°C under the processing conditions to initiate the addition reaction of olefin double bonds, generally no additional initiator and inhibitor need to be added, which can simplify the formulation and improve the storage stability of the product. However, adding initiators and inhibitors can further expand the application scope of the release agent of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a test diagram of the mechanical properties of pultruded plates, where the abscissa is strain (%) and the ordinate is stress (MPa).

[0034] Figure 2 This is a TGA graph of thermal stability of the release agent, where the abscissa is temperature (°C) and the ordinate is weight percentage (%).

[0035] Figure 3 Sample size diagram for cutting to perform standard ASTM D3039. DETAILED DESCRIPTION

[0036] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0037] Example 1

[0038] Weigh 200 parts of the diene terminal polymer prepared by polymerization of styrene monomer and butadiene monomer in benzoyl peroxide as a catalyst and cyclohexane as a solvent, weigh 50 parts of the composite emulsifier of sorbitan fatty acid ester and propylene glycol fatty acid ester, weigh 10 parts of the salt-forming agent sodium sulfate, weigh 10 parts of the solvent benzyl alcohol, weigh 10 parts of the compatibilizer, weigh 10 parts of the film-forming agent polyvinyl alcohol, and weigh 5 parts of the dispersant potassium dodecyl phosphate. In a reactor with an emulsification temperature of 80°C, the speed is 2800r / min, the vacuum degree is 0.05MPa, and the homogenization is carried out for 120min to obtain a release agent 1.

[0039] Example 2

[0040] Weigh 200 parts of the diene terminal polymer prepared by polymerization of styrene monomer and butadiene monomer in benzoyl peroxide as a catalyst and cyclohexane as a solvent, weigh 40 parts of the composite emulsifier of sorbitan fatty acid ester and propylene glycol fatty acid ester, weigh 8 parts of the salt-forming agent sodium sulfate, weigh 8 parts of the solvent benzyl alcohol, weigh 8 parts of the compatibilizer, weigh 8 parts of the film-forming agent polyvinyl alcohol, and weigh 5 parts of the dispersant potassium dodecyl phosphate. In a reactor with an emulsification temperature of 80°C, the speed is 2800r / min, the vacuum degree is 0.05MPa, and the homogenization is carried out for 120min to obtain a release agent 2.

[0041] Example 3

[0042] Weigh 200 parts of the diene terminal polymer prepared by polymerization of styrene monomer and butadiene monomer in benzoyl peroxide as a catalyst and cyclohexane as a solvent, weigh 30 parts of the composite emulsifier of sorbitan fatty acid ester and propylene glycol fatty acid ester, weigh 6 parts of the salt-forming agent sodium sulfate, weigh 6 parts of the solvent benzyl alcohol, weigh 6 parts of the compatibilizer, weigh 6 parts of the film-forming agent polyvinyl alcohol, and weigh 5 parts of the dispersant potassium dodecyl phosphate. In a reactor with an emulsification temperature of 80°C, the speed is 2800r / min, the vacuum degree is 0.05MPa, and the homogenization is carried out for 120min to obtain a release agent 3.

[0043] Example 4

[0044] Weigh 150 parts of the diene terminal polymer prepared by polymerization of styrene monomer and butadiene monomer in benzoyl peroxide as a catalyst and cyclohexane as a solvent, weigh 50 parts of the composite emulsifier of sorbitan fatty acid ester and propylene glycol fatty acid ester, weigh 10 parts of the salt-forming agent sodium sulfate, weigh 10 parts of the solvent benzyl alcohol, weigh 10 parts of the compatibilizer, weigh 10 parts of the film-forming agent polyvinyl alcohol, and weigh 5 parts of the dispersant potassium dodecyl phosphate. In a reactor with an emulsification temperature of 80°C, the speed is 2800r / min, the vacuum degree is 0.05MPa, and the homogenization is carried out for 120min to obtain a release agent 4.

[0045] Example 5

[0046] Weigh 150 parts of the diene terminal polymer prepared by polymerization of styrene monomer and butadiene monomer in benzoyl peroxide as a catalyst and cyclohexane as a solvent, weigh 40 parts of the composite emulsifier of sorbitan fatty acid ester and propylene glycol fatty acid ester, weigh 8 parts of the salt-forming agent sodium sulfate, weigh 8 parts of the solvent benzyl alcohol, weigh 8 parts of the compatibilizer, weigh 8 parts of the film-forming agent polyvinyl alcohol, and weigh 5 parts of the dispersant potassium dodecyl phosphate. In a reactor with an emulsification temperature of 80°C, the speed is 2800r / min, the vacuum degree is 0.05MPa, and the homogenization is carried out for 120min to obtain a release agent 5.

[0047] Example 6

[0048] Weigh 150 parts of the diene terminal polymer prepared by polymerization of styrene monomer and butadiene monomer in benzoyl peroxide as a catalyst and cyclohexane as a solvent, weigh 30 parts of the composite emulsifier of sorbitan fatty acid ester and propylene glycol fatty acid ester, weigh 6 parts of the salt-forming agent sodium sulfate, weigh 6 parts of the solvent benzyl alcohol, weigh 6 parts of the compatibilizer, weigh 6 parts of the film-forming agent polyvinyl alcohol, and weigh 5 parts of the dispersant potassium dodecyl phosphate. In a reactor with an emulsification temperature of 80°C, the speed is 2800r / min, the vacuum degree is 0.05MPa, and the homogenization is carried out for 120min to obtain a release agent 6.

[0049] Performance test and comparative test

[0050] Test 1: Surface tension test of release agent

[0051] The release agents of Examples 1-6 were taken to test the surface tension of the release agents. The prepared samples were tested according to the implementation standard GB / T 6541-1986 (Method for determination of interfacial tension of petroleum products oil against water (ring method)). The results showed that the surface tension of Examples 1-6 was less than 30 mPa.s.

[0052] Test 2 Storage stability test of release agent

[0053] The release agents of Examples 1 to 6 were tested for storage stability. The release agent samples of Examples 1 to 6 were respectively placed in graduated cylinders (or centrifuge tubes) and left to stand at (30±2)° C. The release agents of Examples 1 to 6 were all stable within 12 months.

[0054] Test 3 Thermal stability test of release agent

[0055] The release agents of Examples 1 to 6 were respectively taken to test the thermal stability of the release agents using a thermogravimetric analyzer.

[0056] Under the protection of N2 atmosphere, the release agent samples of Examples 1-6 were placed in a crucible of a heating furnace and heated at 10°C min -1 The temperature was raised from 35°C to 500°C at a rate of 100°C, and the mass loss of the test sample in the temperature range of 35-500°C was measured. The thermal stability test results of the release agent are attached. Figure 2 .

[0057] Figure 2 The results show that the release agents of Examples 1-6 all have good thermal stability.

[0058] Test 4 Pultruded board test

[0059] Take the release agent of Example 6, add epoxy resin at an addition amount of 2%, and cut samples at pultrusion speeds of 0.2m / min, 0.4m / min, 0.6m / min, 0.8m / min, and 1.0m / min respectively to implement standard ASTM D3039. When testing the tensile strength, the experimental speed is 10mm / min, and the mechanical properties of the above materials are tested. The test results are attached. Figure 1 ; See attached for sample size Figure 3 .

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A novel release agent for epoxy resin pultrusion process, characterized in that: The invention comprises the following components by weight: 25-200 parts by weight of polymerized oil, 10-50 parts by weight of emulsifier, 5-10 parts by weight of salt former, 2-5 parts by weight of solvent, 2-5 parts by weight of compatibilizer, 2-5 parts by weight of film former and 2-5 parts by weight of dispersant.

2. The novel release agent for epoxy resin pultrusion process according to claim 1, characterized in that: The composition comprises the following components by weight: 70 parts by weight of polymerized oil, 15 parts by weight of emulsifier, 5 parts by weight of salt former, 2 parts by weight of solvent, 2 parts by weight of compatibilizer, 2 parts by weight of film former and 2 parts by weight of dispersant.

3. The novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: The polymerized grease is a diene terminal polymer.

4. The novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: The emulsifier is one or more of glyceryl monostearate, sucrose fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, sodium stearoyl lactylate, calcium stearoyl lactylate, phospholipids, propylene glycol fatty acid ester, soybean lecithin, sodium lauryl sulfate, polyoxyethylene fatty acid ester, polyglycerol fatty acid ester, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyoxyethylene castor oil, polyoxypropylene glycerol ether, polyoxyethylene oleate, potassium stearate, and sodium dodecylbenzene sulfonate.

5. The novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: The salt-forming agent is one or more of sodium chloride, sodium sulfate, potassium nitrate, ammonium sulfate, ammonium chloride, barium chloride, ammonium carbonate, sodium phosphate, potassium phosphate, and sodium acetate.

6. The novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: The solvent is at least one of heptane, isoheptane, octane, isooctane, nonane, isononane, decane, isodecane, undecane, dodecane, tridecane and tetradecane.

7. The novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: The film-forming agent is one or more of polyvinyl alcohol, polyacrylamide, sodium carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, ethyl cellulose, polyethylene glycol, povidone, gelatin, gum arabic, starch, rosin, terpene resin, phenolic resin, epoxy resin, polyester resin, polyurethane resin, acrylic resin, and silicone resin.

8. The novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: The dispersant is potassium dodecyl phosphate.

9. A method for preparing a novel release agent for epoxy resin pultrusion process according to any one of claims 1 to 2, characterized in that: Here are the steps: (1) Raw material preparation: select natural vegetable oil and purify it; (2) Initiator selection: Select the initiator tert-butyl oxybenzoate to start the polymerization reaction; (3) Preparation of reaction system: Mixing monomer, initiator and solvent in a reaction vessel; (4) Nitrogen protection: The reaction is carried out under a nitrogen atmosphere to avoid interference from oxygen; (5) heating reaction: heating the reaction system to a temperature of 80 to 120° C. to promote the polymerization reaction; (6) Cooling: After the polymerization reaction is completed, cool to room temperature; (7) Product separation: Separate the polymerized oil by precipitation, filtration, and centrifugation; (8) Purification: washing the polymerized oil with a solvent to remove unreacted raw materials and by-products; (9) Drying: Drying the polymerized oil in a vacuum to remove the residual solvent and obtain the polymerized oil; (10) Preparation of release agent: polymerized oil, emulsifier, salt-forming agent, solvent, compatibilizer, film-forming agent and dispersant are mixed and heated to obtain a release agent.