A method for recovering nano-hydroxyapatite from sludge

By employing hydrothermal synthesis, incineration, and alkaline leaching, the problems of long process flow and co-dissolution of impurities in the existing technology of sludge recovery of apatite have been solved, realizing the preparation of nano-hydroxyapatite with high efficiency and low cost, meeting the needs of functional materials.

CN119079952BActive Publication Date: 2026-11-17HUAZHONG UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411205068.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2026-11-17
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing process for recovering phosphorus from sludge to prepare hydroxyapatite is relatively long, and the high-concentration acid leaching method leads to the co-dissolution of impurities and heavy metals, affecting purity and safety.

Method used

The method employs hydrothermal synthesis, incineration, and alkaline leaching. By adjusting the pH value of the sludge with target additives, the Ca/Mg bound phosphorus is converted into Fe/Al bound phosphorus. The phosphorus is then leached with low-concentration alkaline solution and precipitated with calcium source to form hydroxyapatite.

Benefits of technology

The preparation process has been shortened, costs have been reduced, and the purity and safety of hydroxyapatite have been improved, meeting the needs of functional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079952B_ABST
    Figure CN119079952B_ABST
Patent Text Reader

Abstract

This invention relates to the field of sludge resource utilization technology, and more particularly to a method for recovering nano-hydroxyapatite from sludge. The technical solution provided by this invention involves sequentially performing hydrothermal synthesis and moisture removal on sludge with added target additives to obtain oven-dried hydrothermal sludge. The oven-dried hydrothermal sludge is then incinerated to obtain sludge incineration ash. The ash is leached using a target alkaline solution, and after solid-liquid separation, a phosphorus-containing leachate is obtained. Finally, a calcium source is added to the phosphorus-containing leachate to obtain hydroxyapatite. Therefore, the above technical solution utilizes a target alkaline solution to leach phosphorus from sludge with added target additives, thus shortening the process flow for preparing hydroxyapatite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sludge resource utilization technology, and in particular to a method for recovering nano-hydroxyapatite from sludge. Background Technology

[0002] Pollutants and nutrients in wastewater aggregate under the action of rapidly multiplying bacteria and chemical agents, eventually forming sludge. With the continuous development of medicine and materials science, the demand for functional materials such as artificial bones, artificial teeth, surgical implants, drug carriers, and liquid chromatography columns is also increasing. At the same time, the production of hydroxyapatite is also rising, leading to increased demand for its raw materials (such as phosphorus).

[0003] In related technologies, the main method for recovering phosphorus from sludge and preparing hydroxyapatite is acid leaching recovery; however, this method has a long process flow.

[0004] Therefore, there is an urgent need for a method to recover nano-hydroxyapatite from sludge to solve this technical problem. Summary of the Invention

[0005] This invention provides a method for recovering nano-hydroxyapatite from sludge, which can shorten the process flow for preparing hydroxyapatite.

[0006] This invention provides a method for recovering nano-hydroxyapatite from sludge, comprising:

[0007] The sludge with the target additive was subjected to hydrothermal synthesis and water removal in sequence to obtain oven-dry hydrothermal sludge.

[0008] The absolute dry hydrothermal sludge is incinerated to obtain sludge incineration ash;

[0009] The sludge incineration ash was leached using the target alkaline solution, and a phosphorus-containing leachate was obtained after solid-liquid separation.

[0010] A calcium source was added to the phosphorus-containing leachate to obtain hydroxyapatite.

[0011] As can be seen from the above scheme, the method for recovering nano-hydroxyapatite from sludge provided by the present invention involves sequentially performing hydrothermal synthesis and water removal on sludge with added target additives to obtain oven-dry hydrothermal sludge. The oven-dry hydrothermal sludge is then incinerated to obtain sludge incineration ash. The ash is leached using a target alkaline solution, and after solid-liquid separation, a phosphorus-containing leachate is obtained. Finally, a calcium source is added to the phosphorus-containing leachate to obtain hydroxyapatite. Therefore, the above technical solution utilizes a target alkaline solution to leach phosphorus from sludge with added target additives, thus shortening the process flow for preparing hydroxyapatite. Attached Figure Description

[0012] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0013] Figure 1 This is a schematic diagram of a method for recovering nano-hydroxyapatite from sludge according to an embodiment of the present invention;

[0014] Figure 2 A comparison chart of hydroxyapatite recovered by this method and commercial-grade hydroxyapatite provided in this embodiment of the invention;

[0015] Figure 3 The thermodynamic equilibrium calculation system diagram of the precipitation reaction between impurity components and target phosphorus-containing products in phosphorus-containing leachate provided in the embodiments of the present invention is shown. Detailed Implementation

[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0017] Please see Figure 1 One embodiment of the present invention provides a method for preparing hydroxyapatite based on sludge, the method comprising:

[0018] Step 100: The sludge with the target additive is subjected to hydrothermal synthesis and water removal in sequence to obtain absolutely dry hydrothermal sludge.

[0019] Step 102: Incinerate the dry hydrothermal sludge to obtain sludge incineration ash;

[0020] Step 104: Use the target alkaline solution to leach the sludge incineration ash, and obtain a phosphorus-containing leachate after solid-liquid separation;

[0021] Step 106: Add a calcium source to the phosphorus-containing leachate to obtain hydroxyapatite.

[0022] In this embodiment, sludge with the target additive is subjected to hydrothermal synthesis and water removal sequentially to obtain oven-dry hydrothermal sludge. The oven-dry hydrothermal sludge is then incinerated to obtain sludge incineration ash. The ash is leached using a target alkaline solution, and after solid-liquid separation, a phosphorus-containing leachate is obtained. Finally, a calcium source is added to the phosphorus-containing leachate to obtain hydroxyapatite. Therefore, the above technical solution utilizes a target alkaline solution to leach sludge with the target additive to obtain phosphorus, thus shortening the process flow for preparing hydroxyapatite.

[0023] In one embodiment of the present invention, the target additive includes at least one of the target acid and organic solid waste.

[0024] In one embodiment of the present invention, the target acid solution includes at least one selected from sulfuric acid, hydrochloric acid, nitric acid, formic acid, acetic acid, oxalic acid, citric acid, and ascorbic acid.

[0025] In one embodiment of the present invention, the organic solid waste includes at least one of a first organic solid waste and a second organic solid waste. The first organic solid waste includes at least one of waste plastics containing sulfur or chlorine, medical waste, and waste tires. The second organic solid waste includes at least one of waste paper containing active ingredients, cotton and linen fabrics, and medicinal residues.

[0026] In this embodiment, the use of target additives and sludge for hydrothermal treatment is to regulate the form of phosphorus, promote the directional conversion of Ca / Mg bound phosphorus and organic phosphorus to Fe / Al bound phosphorus, and thus realize the recovery of phosphorus from sludge.

[0027] Since Fe / Al bound phosphorus in sludge is soluble in alkali, but Ca / Mg bound phosphorus is difficult to dissolve in alkali, it is necessary to add a targeted additive to convert Ca / Mg bound phosphorus and organic phosphorus in the sludge into Fe / Al bound phosphorus. Studies have shown that in a slightly acidic hydrothermal process, organic phosphorus and Ca / Mg bound phosphorus in sludge decompose and convert to Fe / Al bound phosphorus. Therefore, adding the targeted additive before hydrothermal synthesis to adjust the pH of the sludge creates the pH environment required for the above conversion reaction, thus promoting the conversion of phosphorus forms to Fe / Al bound phosphorus.

[0028] The first organic solid waste containing sulfur and chlorine will generate acidic substances such as HCl and H2SO4 during the hydrothermal process, while the second organic solid waste containing active ingredients will generate acidic substances such as phenols, lactic acid and glycolic acid during the hydrothermal process. This can also reduce the pH of the sludge, thereby promoting the conversion of phosphorus into Fe / Al bound phosphorus, and realizing the resource utilization of solid waste.

[0029] In this embodiment, the filtrate after solid-liquid separation of hydrothermal sludge contains unconsumed organic or inorganic acids, or various organic acidic substances generated during the hydrothermal process from organic solid waste. When this filtrate is used for solid-liquid ratio adjustment in subsequent hydrothermal processes, the acidic substances can further promote the directional conversion of organic phosphorus and Ca / Mg-bound phosphorus in the new sludge to Fe / Al-P. In this way, the required amount of target acid solution or organic solid waste can be reduced, thereby lowering process costs.

[0030] In some embodiments, sludge is mixed with the target additive and the solid-liquid ratio is adjusted to be 1:8 to 1:15. Water is used to adjust the solid-liquid ratio during the first hydrothermal synthesis, and the filtrate obtained after solid-liquid separation from the previous hydrothermal reaction is used to adjust the solid-liquid ratio in subsequent hydrothermal processes.

[0031] In some embodiments, the hydrothermal reaction temperature is 150–300°C and the hydrothermal reaction time is 5–300 min.

[0032] In some implementations, the incineration temperature is 750–900°C to ensure the incineration effect of the dry hydrothermal sludge.

[0033] In one embodiment of the present invention, the pH value of the product obtained by hydrothermal synthesis is 3 to 6.

[0034] In this embodiment, the pH value of the product obtained by hydrothermal synthesis is 3 to 6 to ensure that Ca / Mg bound phosphorus and organic phosphorus in the sludge are fully converted into Fe / Al bound phosphorus.

[0035] In one embodiment of the present invention, the target alkaline solution includes at least one of sodium hydroxide solution, potassium hydroxide solution and ammonia water.

[0036] In this embodiment, current processes widely employ high-concentration acid leaching to extract phosphorus. This method leads to the significant dissolution of impurities and heavy metals along with the phosphorus. These impurities and heavy metals exhibit poor solubility, or even complete non-dissolution, under alkaline conditions. This means that using a target alkaline solution for phosphorus leaching can effectively avoid the co-dissolution of impurities and heavy metals, thereby shortening the preparation steps of hydroxyapatite. To achieve this objective, the type and concentration of the target alkaline solution were optimized, and it was determined that the target alkaline solution would be used to leach sludge incineration ash.

[0037] In related technologies, some leachates typically use organic or inorganic acid solutions to leach phosphorus. The concentration of these organic or inorganic acid solutions is often greater than 0.5 mol / L. Under the aforementioned acidic leaching conditions, major impurities such as Fe, Al, and Mg, as well as heavy metals such as Cu, Pb, Zn, Cr, and Mn, dissolve in large quantities along with the phosphorus. These impurities then co-precipitate with phosphorus during the phosphorus recovery process, reducing the purity and safety of hydroxyapatite. Furthermore, to avoid interference from these impurities in the purity of hydroxyapatite, it is often necessary to remove impurities through methods such as pH pre-precipitation or cation exchange resin methods, and then adjust the pH to the optimal precipitation range for hydroxyapatite to obtain the highest possible yield. This method often requires 6-8 detailed steps for purification and pH adjustment, significantly increasing the complexity of the entire phosphorus recovery process and the cost of reagents. However, the target alkaline solution in this embodiment achieves the leaching of phosphorus in sludge incineration ash, while effectively avoiding the problem of impurity elements and heavy metals dissolving together. This method effectively simplifies the processing procedure and reduces processing costs.

[0038] In one embodiment of the present invention, the concentration of the target alkaline solution is 0.06 to 0.20 mol / L, which can ensure the leaching effect of the target alkaline solution on phosphorus in sludge incineration ash.

[0039] In this embodiment, thermodynamic calculations show that, under normal temperature and pressure conditions, hydroxyapatite exhibits an independent precipitation range under alkaline conditions with a pH above 11.0. Figure 3 As shown, other phosphorus-containing products (such as Fe3(PO4)2, MgNH4PO4, Ca5(PO4)3OH) and solid impurities (such as Fe(OH)3, Al(OH)3, Mg(OH)2, Ca(OH)2) cannot undergo precipitation reactions within this range. Therefore, by controlling the alkali concentration and ensuring that the pH of the leachate is within this range, it is theoretically possible to achieve the individual precipitation of Ca5(PO4)3OH, thereby ensuring its purity.

[0040] In some embodiments, the solid-liquid ratio of sludge incineration ash to target alkaline solution is 1:50 to 1:200, the leaching time is 2 to 4 hours, and the tumbling and shaking rate is 60 to 200 rpm.

[0041] In one embodiment of the present invention, the phosphorus-containing leachate is used to circulate and leach the incineration ash of freshly dried hydrothermal sludge. When the pH value of the phosphorus-containing leachate is less than 11, the circulation and leaching of the phosphorus-containing leachate is stopped.

[0042] In this embodiment, the phosphorus-containing leachate is reused in the cyclic leaching of phosphorus from the incineration ash of new oven-dry hydrothermal sludge, which can reduce reagent consumption.

[0043] In some embodiments, the phosphorus-containing leaching solution can be filtered using a filter head such as 0.45 μm to remove any solid particles that have not been properly separated.

[0044] In one embodiment of the present invention, after obtaining the phosphorus-containing leachate through solid-liquid separation and before adding a calcium source to the phosphorus-containing leachate, the method further includes:

[0045] An impurity removal agent is added to the phosphorus-containing leachate to remove arsenic and copper elements, resulting in a purified phosphorus-containing leachate.

[0046] In this embodiment, a purification agent is used to remove arsenic and copper elements from the phosphorus-containing leachate to ensure the purity of hydroxyapatite.

[0047] In one embodiment of the present invention, the impurity removal agent is ammonium sulfide, and the molar amount of sulfur in the ammonium sulfide is the sum of 1.5 times the molar amount of arsenic and copper in the phosphorus-containing leachate.

[0048] In one embodiment of the present invention, step 106 may specifically include:

[0049] A calcium source was added to the purified phosphorus-containing leachate and stirred to obtain a mixed solution;

[0050] Allow the mixed solution to stand for curing;

[0051] The mixed solution after static curing was subjected to solid-liquid separation to obtain a solid product;

[0052] The solid product was washed with deionized water and then freeze-dried.

[0053] The freeze-dried solid product was calcined in air to obtain hydroxyapatite.

[0054] In this embodiment, the obtained hydroxyapatite is microscopically composed of fine particles with particle sizes ranging from tens to hundreds of nanometers, and the Ca, P, and O elements exhibit a uniform symbiotic distribution. Figure 2 As shown, in Figure 2 In the diagram, a and b represent a comparison of the macroscopic morphology of hydroxyapatite obtained by this method and commercial-grade hydroxyapatite, respectively; c and d represent a comparison of the microscopic morphology of hydroxyapatite obtained by this method and commercial-grade hydroxyapatite, respectively; e represents the elemental distribution uniformity test of the hydroxyapatite obtained by this method; and f represents a comparison of the crystal structure of the hydroxyapatite recovered by this method and commercial-grade hydroxyapatite. Figure 2 It can be seen that the hydroxyapatite prepared in the embodiments of the present invention has greatly improved uniformity.

[0055] In addition, the impurity content of hydroxyapatite meets the standards of liquid chromatography column (Biorad CHT Part 2.4: Purity), raw material standards for surgical implants (GB / T23101.6), and commercial grade reagents. The data are shown in Table 1 (which shows the high-resolution liquid chromatography column grade, surgical implant raw material, commercial grade, analytical grade reagents, and products recovered by this method).

[0056] Table 1 Comparison of Hydroxyapatite with Standard Limits

[0057]

[0058]

[0059] In some embodiments, the mixture is stirred at a speed of 60–200 rpm for 10–60 min. Then stirring is stopped.

[0060] In some implementations, the curing time of the mixed solution can be 0.5 to 24 hours.

[0061] In some implementations, vacuum filtration is used to separate the solid and liquid components of the mixed solution, thereby achieving better separation of the solid and liquid components.

[0062] In some embodiments, the solid product is washed three times with deionized water to remove impurity ions from the solid product.

[0063] In some embodiments, the calcination temperature can be 700–900°C, and the calcination time can be 0.5–2 hours to ensure that the freeze-dried solid product is fully calcined.

[0064] In one embodiment of the present invention, the calcium source includes at least one of solid powder CaCl2 and Ca(NO3)2, and the molar ratio of the calcium source to the phosphorus element in the phosphorus-containing leachate is 1.667:1.

[0065] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for recovering nano-hydroxyapatite from sludge, characterized in that, include: The sludge with the target additive was subjected to hydrothermal synthesis and water removal in sequence to obtain oven-dry hydrothermal sludge. The absolute dry hydrothermal sludge is incinerated to obtain sludge incineration ash; The sludge incineration ash was leached using the target alkaline solution, and a phosphorus-containing leachate was obtained after solid-liquid separation. A calcium source was added to the phosphorus-containing leachate to obtain hydroxyapatite; The target additive includes at least one of the target acid solution and organic solid waste, wherein the target acid solution includes at least one of sulfuric acid, hydrochloric acid, nitric acid, formic acid, acetic acid, oxalic acid, citric acid and ascorbic acid; The organic solid waste includes at least one of waste plastics containing sulfur or chlorine, medical waste, and waste tires. The pH value of the product obtained by hydrothermal synthesis is 3-6; The target alkaline solution includes at least one of sodium hydroxide solution, potassium hydroxide solution and ammonia water, and the concentration of the target alkaline solution is 0.06~0.20 mol / L.

2. The method according to claim 1, characterized in that, The phosphorus-containing leachate is used for cyclic leaching of incinerator ash from fresh, dry hydrothermal sludge. When the pH value of the phosphorus-containing leachate is less than 11, the cyclic leaching of the phosphorus-containing leachate is stopped.

3. The method according to claim 1, characterized in that, After obtaining the phosphorus-containing leachate through solid-liquid separation and before adding a calcium source to the phosphorus-containing leachate, the method further includes: An impurity removal agent is added to the phosphorus-containing leachate to remove arsenic and copper elements from the leachate, thereby obtaining a purified phosphorus-containing leachate.

4. The method according to claim 3, characterized in that, The impurity removal agent is ammonium sulfide, and the molar amount of sulfur in the ammonium sulfide is the sum of 1.5 times the molar amount of arsenic and copper in the phosphorus-containing leachate.

5. The method according to any one of claims 1-4, characterized in that, The addition of a calcium source to the phosphorus-containing leachate to obtain hydroxyapatite includes: A calcium source was added to the purified phosphorus-containing leachate and stirred to obtain a mixed solution; The mixed solution was allowed to stand for curing. The mixed solution after static curing was subjected to solid-liquid separation to obtain a solid product; The solid product was washed with deionized water and then freeze-dried. The freeze-dried solid product was calcined in air to obtain hydroxyapatite.

6. The method according to claim 5, characterized in that, The calcium source includes at least one of solid powder CaCl2 and Ca(NO3)2, and the molar ratio of the calcium source to the phosphorus element in the phosphorus-containing leachate is 1.667:1.

Citation Information

Patent Citations

  • Preparation method for phosphorus-containing sludge-based carbon material with high bioavailability

    CN107857245A

  • Method for preparing pyrolytic carbon with high biological available phosphorus content from calcium-based conditioning excess sludge