Silica and preparation method thereof

By using a large sterically hindered alcohol solvent to regulate the hydrolysis reaction of silicon tetrachloride, the problems of excessive fine particle size of silica and high carbon impurities are solved, and high purity silica is prepared to meet the purity and particle size requirements of quartz crucibles. , simplifies the process and reduces costs.

CN119080013APending Publication Date: 2024-12-06XINTE ENERGY CO LTD +1

Patent Information

Application Number
CN202411234507.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the hydrolysis rate of silicon tetrachloride is too fast, resulting in the silica particle size being too fine and the carbon impurity content is high, making it difficult to meet the purity and particle size requirements of high-purity silica in the field of quartz crucibles.

Method used

Using a large sterically hindered alcohol solvent to slow down the hydrolysis rate of silicon tetrachloride. By preparing aqueous ammonia and aqueous alcohol solutions, the hydrolysis reaction conditions, including temperature, time and ultrasonic environment, further remove unreacted substances and carbon impurities through calcination steps. , high-purity silica with a D50 particle size of 155 μm and a carbon impurity content of 78 ppm were prepared.

Benefits of technology

The particle size of silica has been successfully increased, the carbon impurity content is reduced, the process flow is simplified, the solvent used is non-toxic and harmless, the raw materials are easy to obtain, and the investment scale is small. It is suitable for the production of quartz crucibles with high purity silica.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027386800000061
    Figure BDA0005027386800000061
  • Figure BDA0005027386800000091
    Figure BDA0005027386800000091
  • Figure BDA0005027386800000101
    Figure BDA0005027386800000101
Patent Text Reader

Abstract

The invention discloses silicon dioxide and a preparation method thereof. The method comprises the following steps: 1) preparing an ammonia water solution; (2) preparing an alcohol water solution, wherein the molecular formula of alcohol is CnH2n + 1OH, and n is equal to 4, 5 and 6; (3) simultaneously adding the ammonia water solution and silicon tetrachloride into the alcohol water solution, and carrying out hydrolysis reaction on the silicon tetrachloride; and 4) filtering, washing, drying and calcining to obtain silicon dioxide. The method has the following beneficial effects that in the base catalysis nucleation process, the large-group alcohol solvent slows down the rate of forming a metastable transition state by silicon tetrachloride through a steric effect. And silicon tetrachloride hydrolysis nucleation sites are correspondingly reduced, and more silicon hydroxyl groups can be self-polymerized to enlarge the particle size, so that the particle size of silicon dioxide is increased. And the alcohol solvent is easier to wash away in the washing process and is not left on the surface of silicon dioxide, so that the carbon content of the product is reduced. The method has the advantages of simple process flow, non-toxic and harmless solvent, easily available raw materials and small investment scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic non-metallic materials, and specifically relates to silicon dioxide and a preparation method thereof. Background Art

[0002] High-purity silica is widely used in fiber-optic communications, solar photovoltaic cells, semiconductors, precision optical instruments, aerospace and other fields. It is an important cornerstone and key technology of the country's high-tech industry. High-purity silica usually refers to silica crystals with a purity greater than 99.9%. According to the purity, silica can be divided into low-end (3N), mid-end (4N), and high-end (>4N8) products. At present, low-end and mid-end products have been domestically produced, while high-end silica still needs to be imported, and the preparation technology and products are strictly restricted by Europe and the United States. At present, the high-purity silica industry generally produces high-purity silica by treating vein quartz and pegmatite granite through a combined process of calcination-water quenching-grinding classification-scrubbing-gravity separation-magnetic separation-flotation-chlorination roasting-chemical acid leaching. The domestic quartz ore reserves are very rich, but their quality is poor and it is difficult to meet the needs of industry development.

[0003] According to the particle size, silica is used in different fields. Nano-scale silica is often used in special fields such as special reinforced silicone rubber, silicone sealant, coating, printing ink, etc. Silica below 100μm is often used in emerging fields such as coatings, plastics, metal anti-corrosion, high-end thermal insulation materials, battery coating plates, as well as traditional industries such as rubber, tires, feed, coatings, shoemaking and toothpaste. Silica above 100μm is mainly used in semiconductors, photovoltaics, optical communications and electric light sources. Especially in the field of quartz crucibles, there are strict requirements for the purity and particle size of silica.

[0004] Chemical synthesis of high-purity silica refers to the synthesis of high-purity silica using silicon-containing precursors (silicon tetrachloride, organosilane) as raw materials through hydrolysis-gel-sol-drying-calcination and other steps. The silicon-containing chemical raw materials of this method are not limited by quartz ore, and the products produced have the advantages of stable quality and high purity. However, the hydrolysis rate of silicon tetrachloride is much higher than that of silicon sources such as silicates, the reaction is unsafe, easy to gel, and the product particles are too fine. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a silicon dioxide and a preparation method thereof in view of the above-mentioned deficiencies in the prior art. The purpose of the present invention is to overcome the problem that the hydrolysis rate of silicon tetrachloride in the prior art is too fast, resulting in too fine a particle size of silicon dioxide. The present invention provides a large sterically hindered alcohol solvent to slow down the hydrolysis rate of silicon tetrachloride and reduce the carbon impurity content in silicon dioxide. Finally, the silicon dioxide D50 particle size of the method reaches 155 μm, and the carbon impurity content is 78 ppm.

[0006] The technical solution adopted to solve the technical problem of the present invention is to provide a method for preparing silicon dioxide, comprising the following steps:

[0007] 1) preparing an ammonia solution;

[0008] 2) Prepare an alcohol aqueous solution, wherein the molecular formula of the alcohol is C n H 2n+1 OH, n = 4, 5, 6;

[0009] 3) adding ammonia solution and silicon tetrachloride to alcohol aqueous solution at the same time, and causing silicon tetrachloride to undergo hydrolysis reaction;

[0010] 4) Filter, wash, dry and calcine to obtain silicon dioxide.

[0011] Preferably, in the step 1), the concentration of the ammonia solution prepared is 5-20 mas%.

[0012] Preferably, in the step 2) of preparing the alcohol-water solution, the mass ratio of water to alcohol is (8-2):1.

[0013] More preferably, the mass ratio of ultrapure water to alcohol is (7-3):1.

[0014] More preferably, the mass ratio of ultrapure water to alcohol is (6-4):1.

[0015] Preferably, in step 3), the aqueous ammonia solution and silicon tetrachloride are simultaneously added to the aqueous alcohol solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0016] This step is carried out at -5 to 5°C.

[0017] Preferably, in step 3), the aqueous ammonia solution and silicon tetrachloride are simultaneously added to the aqueous alcohol solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0018] The hydrolysis reaction time in this step is 0.5 to 2 hours.

[0019] Preferably, in step 3), the aqueous ammonia solution and silicon tetrachloride are simultaneously added to the aqueous alcohol solution to hydrolyze the silicon tetrachloride.

[0020] This step is performed under ultrasonic conditions.

[0021] Preferably, the power of the ultrasonic wave is 200-1500W.

[0022] Preferably, in step 3), the aqueous ammonia solution and silicon tetrachloride are simultaneously added to the aqueous alcohol solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0023] In this step, the mass ratio of the ammonia solution to silicon tetrachloride is (4-20):1.

[0024] Preferably, in step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0025] In this step, the mass ratio of silicon tetrachloride to alcohol in the alcohol aqueous solution is (6-0.5):1.

[0026] More preferably, the mass ratio of silicon tetrachloride to the alcohol in the alcohol aqueous solution is (4-2):1.

[0027] More preferably, the mass ratio of silicon tetrachloride to the alcohol in the alcohol aqueous solution is (3.5-2.5):1.

[0028] Preferably, the step 3) wherein the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride is hydrolyzed to generate silicon dioxide, further comprises the following steps:

[0029] Let stand for aging at 20-30℃.

[0030] Preferably, the step 4) is filtering, washing, drying and calcining to obtain silicon dioxide.

[0031] The calcination process in this step is:

[0032] Keep warm at 250-350℃ for 3.5-4.5h, then keep warm at 700-900℃ for 3.5-4.5h, and finally keep warm at 1200-1300℃ for 3.5-4.5h.

[0033] The present invention also provides silicon dioxide, which is prepared by the above method.

[0034] The silicon dioxide and preparation method thereof in the present invention have the following beneficial effects: (1) In the process of base-catalyzed nucleation, the large-group alcohol solvent slows down the rate at which silicon tetrachloride forms a metastable transition state through the steric effect. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in the present invention has a simple process flow, non-toxic and harmless solvents, easily available raw materials, and a small investment scale. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with specific implementation methods.

[0036] Example 1

[0037] This embodiment provides a method for preparing silicon dioxide, comprising the following steps:

[0038] 1) preparing an ammonia solution;

[0039] 2) Prepare an alcohol aqueous solution, wherein the molecular formula of the alcohol is C n H 2n+1 OH, n = 4, 5, 6;

[0040] 3) adding ammonia solution and silicon tetrachloride to alcohol aqueous solution at the same time, and causing silicon tetrachloride to undergo hydrolysis reaction;

[0041] 4) Filter, wash, dry and calcine to obtain silicon dioxide.

[0042] This embodiment also provides a silicon dioxide, which is prepared by the above method.

[0043] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0044] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0045] Example 2

[0046] This embodiment provides a method for preparing silicon dioxide, comprising the following steps:

[0047] 1) preparing an ammonia solution;

[0048] 2) Prepare an alcohol aqueous solution, wherein the molecular formula of the alcohol is C n H 2n+1 OH, n = 4, 5, 6;

[0049] 3) adding ammonia solution and silicon tetrachloride to alcohol aqueous solution at the same time, and causing silicon tetrachloride to undergo hydrolysis reaction;

[0050] 4) Filter, wash, dry and calcine to obtain silicon dioxide.

[0051] Preferably, in the step 1), the concentration of the ammonia solution prepared is 5-20 mas%.

[0052] Preferably, in the step 2) of preparing the alcohol-water solution, the mass ratio of water to alcohol is (8-2):1.

[0053] More preferably, the mass ratio of ultrapure water to alcohol is (7-3):1.

[0054] More preferably, the mass ratio of ultrapure water to alcohol is (6-4):1.

[0055] Preferably, in step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0056] This step is carried out at -5 to 5°C.

[0057] Preferably, in step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0058] The hydrolysis reaction time in this step is 0.5 to 2 hours.

[0059] Preferably, in step 3), the aqueous ammonia solution and silicon tetrachloride are simultaneously added to the aqueous alcohol solution to hydrolyze the silicon tetrachloride.

[0060] This step is performed under ultrasonic conditions.

[0061] Low-temperature ultrasonic synthesis technology is applied to the hydrolysis reaction of silicon tetrachloride to avoid uneven mixing of large-group alcohol compounds and water in an ice-water bath, which is conducive to the full mixing of large-group alcohol compounds, water and silicon tetrachloride, and is more effective than single stirring mixing.

[0062] Preferably, the power of the ultrasonic wave is 200-1500W.

[0063] Preferably, in step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0064] In this step, the mass ratio of the ammonia solution to silicon tetrachloride is (4-20):1.

[0065] Preferably, in step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction.

[0066] In this step, the mass ratio of silicon tetrachloride to alcohol in the alcohol aqueous solution is (6-0.5):1.

[0067] More preferably, the mass ratio of silicon tetrachloride to the alcohol in the alcohol aqueous solution is (4-2):1.

[0068] More preferably, the mass ratio of silicon tetrachloride to the alcohol in the alcohol aqueous solution is (3.5-2.5):1.

[0069] Preferably, the step 3) wherein the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride is hydrolyzed to generate silicon dioxide, further comprises the following steps:

[0070] Let stand for aging at 20-30℃.

[0071] Preferably, the step 4) is filtering, washing, drying and calcining to obtain silicon dioxide.

[0072] The calcination process in this step is:

[0073] Keep warm at 250-350℃ for 3.5-4.5h, then keep warm at 700-900℃ for 3.5-4.5h, and finally keep warm at 1200-1300℃ for 3.5-4.5h.

[0074] Calcination at 250-350°C removes unreacted alcohols, water, silicon tetrachloride and other raw materials. At 700-900°C, hydroxyl groups are eliminated, chlorine and carbon impurity contents are reduced, and chemically stable high-purity silicon dioxide solids are obtained. At 1200-1300°C, the pores of silicon dioxide are eliminated, and densified silicon dioxide particles are obtained.

[0075] This embodiment also provides a silicon dioxide, which is prepared by the above method.

[0076] Specifically, this embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0077] 1) Take 70g of ultrapure water, add 70g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0078] 2) Add 40g ultrapure water and 8g tert-butyl alcohol to a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400rpm, and keep warm to 0°C to obtain an alcohol-water solution. The molecular formula of tert-butyl alcohol is as follows:

[0079]

[0080] 3) A low-temperature ultrasonic synthesizer is used to accurately control the temperature of the reaction system through a compressor refrigeration system and a temperature measurement and control system, and the temperature of the reaction solution is kept at 0°C and the ultrasonic power is 1000W. The ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400rpm, the ammonia solution of step 1) and 20g of silicon tetrachloride are added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring speed is maintained at 400rpm for 1h to carry out a hydrolysis reaction. Under near-neutral conditions, the silicon dioxide particles obtained by the hydrolysis of silicon tetrachloride are more uniform and have a narrower particle size distribution. After the prior art first adds ammonia water, the system is alkaline, which is not conducive to the hydrolysis of silicon tetrachloride. The simultaneous addition of silicon tetrachloride and ammonia water in this embodiment is conducive to maintaining the stability of the pH of the solution and obtaining silicon dioxide particles with a narrow particle size distribution.

[0081] 4) Heat the water bath to 25°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0082] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1250°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 155μm. The carbon content of the product is 78ppm.

[0083] This embodiment also provides a large-size silicon dioxide, which is prepared by the above method.

[0084] In this embodiment, a large group alcohol compound is used as a co-solvent, and some chlorine atoms of silicon tetrachloride are replaced by alkoxy groups. In the base-catalyzed nucleation process, -OH attacks the Si atom with nucleophilicity, and the rate at which the silicon compound replaced by the macromolecular alkoxy group forms a metastable transition state is relatively slow due to the steric effect. Subsequently, the rate at which the large group -OR is separated from the Si atom and replaced by -OH will also be slowed down accordingly. In this way, the sites for the hydrolysis of silicon tetrachloride into nuclei are reduced accordingly, and more silanol groups will polymerize themselves to make the particle size larger. Alcohol solvents are easy to clean and remove, do not remain on the product surface, and reduce the carbon impurity content of silicon dioxide.

[0085] Alcohol solvents include at least one of butanol, pentanol, hexanol and their alcohol isomers. Compared with low-carbon alcohols such as ethanol, high-carbon alcohol solvents have larger groups and more obvious steric effects. During the hydrolysis process, it is more difficult for hydroxide ions to attack Si atoms nucleophilically, which reduces the hydrolysis reaction rate and thus increases the particle size of silica. Compared with amphoteric surfactants, alcohol solvents have a higher solubility in water, which is conducive to removal in the filtering and washing process, thereby improving the purity of the silica product.

[0086] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0087] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0088] Example 3

[0089] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0090] 1) Take 80g of ultrapure water, add 80g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0091] 2) Add 48g of ultrapure water and 8g of n-butanol to a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400 rpm, and keep warm to 0°C to obtain an alcohol-water solution. The molecular formula of n-butanol is as follows:

[0092] CH3CH2CH2CH2-OH

[0093] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at -5°C, and the ultrasonic power is 1500W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 24 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring speed is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0094] 4) Heat the water bath to 20°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0095] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 250°C for 4 hours, then raise the temperature to 900°C and keep it for 4 hours. Finally, raise the temperature to 1300°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 112μm. The carbon content of the product is 76ppm.

[0096] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects: (1) In the process of base-catalyzed nucleation, the large-group alcohol solvent slows down the rate at which silicon tetrachloride forms a metastable transition state through the steric effect. The number of sites for silicon tetrachloride hydrolysis nucleation is reduced accordingly, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0097] Example 4

[0098] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0099] 1) Take 95g of ultrapure water, add 95g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0100] 2) Add 32g ultrapure water and 8g isobutanol to a three-necked flask reaction vessel, place in an ice-water bath, start stirring at 400rpm, keep warm to 0°C, and obtain an alcohol-water solution. The molecular formula of isobutanol is as follows:

[0101]

[0102] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, and the temperature of the reaction solution is maintained at 5°C and the ultrasonic power is 600W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 28 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring is maintained at a speed of 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0103] 4) Heat the water bath to 30°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0104] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 350°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1300°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 124μm. The carbon content of the product is 82ppm.

[0105] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0106] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0107] Example 5

[0108] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0109] 1) Take 75g of ultrapure water, add 75g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0110] 2) Add 48g of ultrapure water and 8g of sec-butyl alcohol to a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400rpm, and keep warm to 0°C to obtain an alcohol-water solution. The molecular formula of sec-butyl alcohol is as follows:

[0111]

[0112] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at 0°C, and the ultrasonic power is 200W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at 400 rpm, the ammonia solution of step 1) and 20 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0113] 4) Heat the water bath to 30°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0114] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 700°C and keep it for 4 hours. Finally, raise the temperature to 1200°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 131μm. The carbon content of the product is 83ppm.

[0115] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0116] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0117] Comparative Example 1

[0118] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0119] 1) Take 70g of ultrapure water, add 70g of 25mas% concentrated ammonia water while stirring at 400rpm to obtain a 12.5mas% ammonia solution.

[0120] 2) Add 40g ultrapure water and 8g sodium dodecyl sulfate to a three-necked flask reaction vessel, place in an ice-water bath, stir at 400rpm, and keep warm to 0°C to obtain a mixed solution. The molecular formula of sodium dodecyl sulfate is as follows:

[0121]

[0122] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction solution is maintained at 0°C and the ultrasonic power is 1000W through the compressor refrigeration system and the temperature measurement and control system. The ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the mixed solution. Under stirring at 400 rpm, the ammonia solution of step 1) and 20g of silicon tetrachloride are added to the mixed solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0123] 4) Heat the water bath to 25°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0124] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then increase the temperature to 800°C and keep it for 4 hours. Finally, increase the temperature to 1250°C and keep it for 4 hours. The D50 particle size of the high-purity silica product is 133μm. The carbon content of the product is 192ppm.

[0125] Comparative Example 2

[0126] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0127] 1) Take 70g of ultrapure water, add 70g of 25mas% concentrated ammonia water while stirring at 400rpm to obtain a 12.5mas% ammonia solution.

[0128] 2) Add 40g ultrapure water and 8g methanol to a three-necked flask reaction vessel, place in an ice-water bath, stir at 400rpm, and keep warm to 0°C to obtain an alcohol-water solution. The molecular formula of methanol is as follows:

[0129] CH3-OH

[0130] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction solution is maintained at 0°C and the ultrasonic power is 1000W through a compressor refrigeration system and a temperature measurement and control system. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at 400 rpm, the ammonia solution of step 1) and 20 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0131] 4) Heat the water bath to 25°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0132] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then increase the temperature to 800°C and keep it for 4 hours. Finally, increase the temperature to 1250°C and keep it for 4 hours. The D50 particle size of the high-purity silica product is 0.258μm. The carbon content of the product is 72ppm.

[0133] The particle size and carbon content of the silicon dioxide synthesized in Examples 2 to 5 and Comparative Examples 1 and 2 were tested, and the specific test results are shown in Table 1:

[0134] Table 1: Test results of the particle size and carbon content of the silicon dioxide synthesized in Examples 2 to 5 and Comparative Examples 1 and 2

[0135] name D50 / μm Carbon content / ppm Example 2 155 78 Example 3 112 76 Example 4 124 82 Example 5 131 83 Comparative Example 1 133 192 Comparative Example 2 0.258 72

[0136] According to the test data of Examples 2, 3, 4, 5 and Comparative Examples 1 and 2, in the technical scheme of this embodiment, tert-butyl alcohol with a large group can effectively reduce the hydrolysis rate of silicon tetrachloride and increase the particle size of the silica product. The quartz crucible prepared using the silica products of Examples 2, 3, 4, and 5 as raw materials has low impurity content, low hydroxyl content, and no bubbles agglomeration, and can be used in the direct single crystal process. In addition, compared with amphoteric surfactants such as sodium dodecyl sulfate, the carbon content of the silica product prepared by alcohol surfactants is significantly reduced. The quartz crucible prepared using the silica product of Comparative Example 1 has a high carbon impurity content, black spots in some areas, and silicon embedding and crystallization occur during high-temperature crystal pulling, making it unusable. The particle size of the silica synthesized using methanol as a co-solvent is small, at the nanometer level, and cannot be made into a quartz crucible.

[0137] Example 6

[0138] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0139] 1) Take 800g ultrapure water, add 200g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain 5mas% ammonia solution.

[0140] 2) Add 80 g of ultrapure water and 10 g of tert-butyl alcohol into a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400 rpm, and keep warm at 0° C. to obtain an alcohol-water solution.

[0141] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at 0°C, and the ultrasonic power is 1000W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 60 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring is maintained at a speed of 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0142] 4) Heat the water bath to 20°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0143] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1250°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 128μm. The carbon content of the product is 75ppm.

[0144] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0145] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0146] Example 7

[0147] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0148] 1) Take 150g ultrapure water, add 150g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0149] 2) Add 50 g of ultrapure water and 10 g of tert-butyl alcohol into a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400 rpm, and keep warm at 0° C. to obtain an alcohol-water solution.

[0150] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at 0°C, and the ultrasonic power is 1000W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 30 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0151] 4) Heat the water bath to 25°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0152] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1250°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 169μm. The carbon content of the product is 105ppm.

[0153] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0154] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0155] Example 8

[0156] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0157] 1) Take 17.5 g of ultrapure water, add 70 g of 25 mas % concentrated ammonia water while stirring at 400 rpm, and dilute to obtain a 20 mas % ammonia solution.

[0158] 2) Add 80 g of ultrapure water and 40 g of tert-butyl alcohol into a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400 rpm, and keep warm at 0° C. to obtain an alcohol-water solution.

[0159] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at 0°C, and the ultrasonic power is 1000W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 20 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring speed is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0160] 4) Heat the water bath to 30°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0161] 5) After the reaction is completed, filter, wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Subsequently, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1250°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained. The D50 particle size of the high-purity silica product is 183μm. The carbon content of the product is 126ppm.

[0162] The particle size and carbon content of the silicon dioxide synthesized in Examples 6, 7 and 8 were tested. The specific test results are shown in Table 2:

[0163] Table 2: Test results of silica particle size and carbon content synthesized in Examples 6, 7, and 8

[0164] name D50 / μm Carbon content / ppm Example 6 128 75 Example 7 169 105 Example 8 183 126

[0165] According to the test data in Examples 6, 7, and 8, in the technical solution of this embodiment, as the content of tert-butyl alcohol increases, the particle size of silicon dioxide also gradually increases, and the carbon content also increases accordingly. When the mass ratio of tert-butyl alcohol to ultrapure water is 1:5, the D50 particle size and carbon content of the silicon dioxide product reach a relative balance. The quartz crucible prepared using the silicon dioxide products of Examples 6, 7, and 8 as raw materials has low impurity content, low hydroxyl content, and no bubbles agglomerate, and can be used in the CZ single crystal process.

[0166] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0167] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0168] Example 9

[0169] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0170] 1) Take 70g of ultrapure water, add 70g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0171] 2) Add 40 g of ultrapure water and 8 g of amyl alcohol into a three-necked flask reaction container, place in an ice-water bath, start stirring at a stirring speed of 400 rpm, and keep warm at 0° C. to obtain an alcohol-water solution.

[0172] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at 0°C, and the ultrasonic power is 1000W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 20 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring speed is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0173] 4) Heat the water bath to 20°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0174] 5) After the reaction is completed, filter and wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Then, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1250°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained.

[0175] Table 3 Particle size and carbon content of silica D50 synthesized from different amyl alcohols and their alcohol isomers

[0176]

[0177]

[0178] According to the test data in Table 3, the particle size of pentanol and its alcohol isomers as co-solvents is increased compared with butanol and its alcohol isomers. However, the carbon impurity content is also increased. The quartz crucible made by using the above silicon dioxide product as raw material has low impurity content, low hydroxyl content, and no bubble aggregation, and can be used in the Czochralski single crystal process.

[0179] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0180] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0181] Example 10

[0182] This embodiment provides a method for synthesizing large-size silicon dioxide using silicon tetrachloride as a raw material, comprising the following steps:

[0183] 1) Take 70g of ultrapure water, add 70g of 25mas% concentrated ammonia water while stirring at 400rpm, and dilute to obtain a 12.5mas% ammonia solution.

[0184] 2) Add 40 g of ultrapure water and 8 g of hexanol into a three-necked flask reaction vessel, place in an ice-water bath, start stirring at a stirring speed of 400 rpm, and keep warm at 0° C. to obtain an alcohol-water solution.

[0185] 3) Using a low-temperature ultrasonic synthesizer, the temperature of the reaction system is precisely controlled through a compressor refrigeration system and a temperature measurement and control system, the temperature of the reaction solution is maintained at 0°C, and the ultrasonic power is 1000W. An ultrasonic tool head is placed through the middle port of the three-necked flask to send ultrasonic energy to the alcohol-water solution. Under stirring at a speed of 400 rpm, the ammonia solution of step 1) and 20 g of silicon tetrachloride are simultaneously added to the alcohol-water solution of step 2) through the two side ports of the three-necked flask to obtain a silicon solution, and the stirring speed is maintained at 400 rpm for 1 hour to carry out a hydrolysis reaction.

[0186] 4) Heat the water bath to 20°C and allow to stand for 1 hour to ensure that silicon tetrachloride is completely hydrolyzed. The temperature range of the standing aging is 20-30°C.

[0187] 5) After the reaction is completed, filter and wash the filter cake with ethanol first, then with ultrapure water, and dry to obtain silica. Then, put the product into a tubular furnace. Keep it at 300°C for 4 hours, then raise the temperature to 800°C and keep it for 4 hours. Finally, raise the temperature to 1250°C and keep it for 4 hours. After calcination, large-sized high-purity silica is obtained.

[0188] Table 4 Particle size and carbon content of silica D50 synthesized from different hexanols and their alcohol isomers

[0189]

[0190]

[0191] According to the test data in Table 4, the particle size of hexanol and its alcohol isomers as co-solvents is increased compared with that of pentanol and its alcohol isomers. However, the carbon impurity content is also increased. The quartz crucible made by using the above-mentioned silicon dioxide product as raw material has low impurity content, low hydroxyl content, and no bubble aggregation, and can be used in the CZ single crystal process.

[0192] The silicon dioxide and its preparation method in this embodiment have the following beneficial effects:

[0193] (1) During the base-catalyzed nucleation process, large-group alcohol solvents slow down the rate at which silicon tetrachloride forms a metastable transition state through steric hindrance. The number of sites for silicon tetrachloride hydrolysis nucleation is correspondingly reduced, and more silanol groups will polymerize themselves to increase the particle size, thereby increasing the particle size of silicon dioxide. (2) Compared with other surfactants, alcohol solvents are easier to wash away during the washing process and do not remain on the surface of silicon dioxide, thereby reducing the carbon content of the product. (3) The method for preparing high-purity silicon dioxide in this embodiment has a simple process flow, the solvent is non-toxic and harmless, the raw materials are easily available, and the investment scale is small.

[0194] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing silicon dioxide, characterized in that: The following steps are involved: 1) preparing an ammonia solution; 2) Prepare an alcohol aqueous solution, wherein the molecular formula of the alcohol is C n H 2n+1 OH, n = 4, 5, 6; 3) adding ammonia solution and silicon tetrachloride to alcohol aqueous solution at the same time, and causing silicon tetrachloride to undergo hydrolysis reaction; 4) Filter, wash, dry and calcine to obtain silicon dioxide.

2. The method for preparing silicon dioxide according to claim 1, characterized in that: In the step 1), the concentration of the ammonia solution is 5-20 mas%.

3. The method for preparing silicon dioxide according to claim 1, characterized in that: In the step 2), the mass ratio of water to alcohol in preparing the alcohol aqueous solution is (8-2):

1.

4. The method for preparing silicon dioxide according to claim 1, characterized in that: In step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction. This step is carried out at -5 to 5°C.

5. The method for preparing silicon dioxide according to claim 1, characterized in that: In step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction. The hydrolysis reaction time in this step is 0.5 to 2 hours.

6. The method for preparing silicon dioxide according to claim 1, characterized in that: In step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol solution to hydrolyze the silicon tetrachloride. This step is performed under ultrasonic conditions.

7. The method for preparing silicon dioxide according to claim 6, characterized in that: The power of ultrasound is 200~1500W.

8. The method for preparing silicon dioxide according to claim 1, characterized in that: In step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction. In this step, the mass ratio of the ammonia solution to silicon tetrachloride is (4-20):

1.

9. The method for preparing silicon dioxide according to claim 1, characterized in that: In step 3), the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution, and the silicon tetrachloride undergoes a hydrolysis reaction. In this step, the mass ratio of silicon tetrachloride to alcohol in the alcohol aqueous solution is (6-0.5):

1.

10. The method for preparing silicon dioxide according to claim 1, characterized in that: The step 3) wherein the ammonia solution and silicon tetrachloride are simultaneously added to the alcohol aqueous solution to hydrolyze the silicon tetrachloride to generate silicon dioxide, further comprises the following steps: Allow to age at 20-30°C.

11. The method for preparing silicon dioxide according to claim 1, characterized in that: The step 4) filtering, washing, drying and calcining to obtain silicon dioxide, The calcination process in this step is: Keep warm at 250-350℃ for 3.5-4.5h, then keep warm at 700-900℃ for 3.5-4.5h, and finally keep warm at 1200-1300℃ for 3.5-4.5h.

12. A silicon dioxide, characterized in that: It is prepared by the method according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Silicon-oxygen-carbon composite negative active material for lithium ion battery and preparation method thereof

    CN106941165A

  • Reduction of carbon content of silica granulate, and production of silica glass article

    CN108698886A

  • Preparation method of spherical silicon dioxide

    CN111717922A

  • Preparation method and preparation system of silicon dioxide

    CN116553561A

  • Preparation method of high-purity silicon dioxide

    CN117023595A

Cited By

  • Method for removing carbon impurities in synthetic silicon dioxide

    CN122324823A