Preparation method of iron-based Prussian blue positive electrode material

By using bipyridine and phenanthrene as complexing agents in iron-pylprus blue cathode material, the problem of poor reversible specific capacity and cycle performance of existing materials is solved, and the chemical stability and electrochemical performance of the materials are improved, thus achieving the realization of the achievement of More efficient battery performance and longer life.

CN119080026APending Publication Date: 2024-12-06ZHEJIANG SHANGAO NEW ENERGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411203960.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing iron-based Prussian blue cathode material has low reversible specific capacity, poor rate performance and cycle performance, which limits the development of sodium ion batteries.

Method used

Bipyridine and phenanthroline are used as complexing agents to improve chemical stability by forming a more stable chelating structure with iron ions, and enhance electron transfer efficiency and oxidation through good conjugated structure and coordination ability of nitrogen atoms. Reversibility of reduction reaction.

Benefits of technology

It significantly improves the chemical stability and electrochemical performance of iron-based Prussian blue cathode material, improves the charging and discharge rate and efficiency of the battery, extends the battery life, and improves environmental friendliness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of an iron-based Prussian blue positive electrode material. The preparation method comprises the following steps: dissolving sodium ferrocyanide and sodium salt in deionized water to form a solution A; dissolving iron salt in deionized water to form a solution B; dissolving sodium citrate and a complexing aid in deionized water to form a solution C; slowly dropwise adding the solution A and the solution B into the solution C by using a peristaltic pump in an N2 atmosphere, and carrying out stirring reaction, aging, centrifugal separation, washing and drying to obtain an iron-based Prussian blue positive electrode material; according to the present invention, the co-complexing agent is obtained by stirring reaction of allyl tributyl phosphorus chloride, 6-amino-2, 2 '-dipyridyl, 1, 10-phenanthroline-4, 7-diamine, toluene and sodium ethoxide, and the prepared co-complexing agent can improve the chemical stability, enhance the electrochemical performance and improve the environmental friendliness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sodium ion batteries, in particular to a method for preparing an iron-based Prussian blue positive electrode material. Background Art

[0002] The widespread use of traditional fossil energy materials has led to many environmental problems, the instability of sustainable clean energy, and the development of large-scale energy storage systems is urgent. At present, lithium-ion batteries have the advantages of high energy density and long cycle life, and are widely used in portable devices ranging from mobile phones to new energy vehicles to large-scale energy storage power station systems. However, the low reserves of lithium resources limit their development and application in large-scale energy storage. In recent years, sodium-ion batteries (SIBs) are a promising new battery technology due to the high abundance of sodium resources in the earth's crust and the similar electrochemical properties of sodium and lithium. However, the realization of large-scale use of SIBs remains a huge challenge. In particular, the positive electrode materials have serious phase changes and capacity attenuation, so it is necessary to explore positive electrode materials with excellent performance.

[0003] Prussian blue analogs (PBAs) are considered to be suitable cathode materials due to their open framework structure (large ion diffusion channels) and high theoretical capacity (85-170 mAh / g). Among them, iron-based Prussian blue (FeHCF) has the advantages of about 170 mAh / g theoretical capacity, long life and low cost, and is considered to be the most promising cathode material.

[0004] Chinese patent CN117430134B: discloses a method for preparing a manganese-iron-based sodium Prussian blue positive electrode material and a positive electrode material prepared by the method, belonging to the field of sodium ion batteries. Sodium ferrocyanide, a suspension of elemental manganese powder and an ethylenediaminetetraacetic acid solution are prepared in an appropriate molar ratio, and the ethylenediaminetetraacetic acid solution is added dropwise to the suspension under appropriate conditions, and then the manganese-iron-based sodium Prussian blue positive electrode material is obtained after aging, washing and vacuum drying.

[0005] Chinese patent CN114709402A: relates to the preparation and application of a carbon-coated sodium iron-based Prussian blue positive electrode material, belonging to the field of sodium ion battery technology. The specific steps are as follows: S1: grind ferrous sulfate and sodium ferrocyanide according to a certain ratio and put them into an agate jar, and put a certain amount of agate beads; S2: add a certain amount of organic solvent into a ball mill; S3: place the mixed raw materials into the ball mill for ball milling; S4: wash the mixture obtained in step S3 with water and alcohol; S5: vacuum dry the washed product at 100°C to 120°C to obtain bare material FeHCF before carbon coating; S6: put bare material FeHCF and a certain amount of Ketjen black into a ball mill; S7: perform dry ball milling coating under the protection of inert gas; S8: vacuum dry the FeHCF@KB material obtained in step S7 at 100°C to 120°C to obtain a carbon-coated sodium iron-based Prussian blue positive electrode material; S9: perform a three-step water removal treatment on the electrode after the material is coated.

[0006] Chinese patent CN113488646A: relates to a Prussian blue type sodium ion battery positive electrode material and its preparation method. Transition metal salt and tartaric acid are dissolved in deionized water to form solution A, sodium ferrocyanide decahydrate and ascorbic acid are dissolved in deionized water to form solution B, and polyvinyl pyrrolidone and sodium chloride are dissolved in deionized water to form solution C. Solution A and solution B are added to solution C simultaneously through a peristaltic pump, and heated and stirred in a N2 atmosphere until the solution becomes a suspension after the dropwise addition is completed; the suspension is then kept heated and stirred for 12 hours, and finally aged at room temperature for 24 hours, followed by centrifugal washing with deionized water and anhydrous ethanol three times each, and finally vacuum dried at 120°C for 24 hours to obtain a Prussian blue type positive electrode material.

[0007] The iron-based Prussian blue positive electrode materials prepared by the above patents and prior art have disadvantages such as low reversible specific capacity, poor rate performance and cycle performance. Summary of the invention

[0008] This patent provides a new method for improving the chemical stability, enhancing the electrochemical performance and improving the environmental friendliness of positive electrode materials.

[0009] In order to achieve the above purpose, the preparation method of the positive electrode material is as follows:

[0010] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0011] S1: Dissolve 5-10 parts of sodium ferrocyanide and 15-25 parts of sodium salt in 40-50 parts of deionized water to form solution A;

[0012] S2: dissolving 5-10 parts of iron salt in 40-50 parts of deionized water to form solution B;

[0013] S3: dissolving 40-50 parts of sodium citrate and 0.03-0.4 parts of a complexing aid in 100-200 parts of deionized water to form a solution C;

[0014] S4: Solutions A and B are pumped in N 2 Under the atmosphere, slowly add dropwise to solution C, stir and react for 5-10 hours at 50-80°C and 300-500 rpm, and age for 16-24 hours;

[0015] S5: After aging, centrifugation is performed, and the precipitate is washed twice with anhydrous ethanol and twice with deionized water, and then placed in a vacuum drying oven at 100-120° C. for 20-25 hours to obtain an iron-based Prussian blue positive electrode material.

[0016] Preferably, the positive electrode material is as follows: Na x M[Fe(CN) 6 ] 1-y O y ·nH 2 O(M=Fe, Ni, Mn, Co, 0<x≤2, 0<y<1).

[0017] Preferably, the solutions A and B are added by a peristaltic pump at a drip rate of 100-500 μL / min under a N2 atmosphere.

[0018] Preferably, the sodium salt is one of sodium chloride, sodium carbonate, sodium acetate and sodium nitrate.

[0019] Preferably, the iron salt is one of ferric sulfate, ferrous sulfate, ferric acetate, ferrous acetate, ferric chloride, ferrous chloride, and ferric nitrate.

[0020] Preferably, the preparation method of the complexing aid is:

[0021] According to weight, 4-10 parts of propylene tributyl phosphonium chloride, 0.05-0.5 parts of 6-amino-2,2'-bipyridine, 0.003-0.05 parts of 1,10-phenanthroline-4,7-diamine, 100-150 parts of toluene, and 0.5-2 parts of sodium ethoxide are stirred for reaction for 50-100 minutes. After the reaction is completed, the toluene is removed by reduced pressure distillation to obtain a complexing agent.

[0022] Reaction mechanism

[0023] Amino-propenyl addition reaction: Propylene tributylphosphonium chloride first undergoes an amino-propenyl addition reaction with 6-amino-2,2'-bipyridine; during this process, part of the propenyl group reacts with the nitrogen atom of the amino group through a Markel addition reaction to form a stable chain structure.

[0024] Role in complexation: Further reaction with 1,10-phenanthroline-4,7-diamine adds more functional groups, which play a bridging and stabilizing role in the complexation process with sodium ferrocyanide and sodium citrate, which is conducive to the generation of iron-based Prussian blue positive electrode materials with more complex structures and richer functions.

[0025] Technical Effects

[0026] The present invention provides a method for preparing an iron-based Prussian blue positive electrode material. Compared with the prior art, the present invention has the following significant effects:

[0027] In the preparation process of iron-based Prussian blue cathode materials, the technical effects of using bipyridine and phenanthroline instead of sodium citrate as complexing agents can be analyzed in detail from multiple aspects; these technical effects mainly involve improving chemical stability, enhancing electrochemical performance and improving environmental friendliness:

[0028] 1. Improve chemical stability

[0029] Strengthening the metal-ligand complexation: Bipyridine and phenanthroline, as nitrogen-containing multidentate ligands, can form a more stable chelate structure with iron ions; the stability of this structure is better than that of the simple complex formed using sodium citrate. Therefore, the introduction of these ligands into the iron-based Prussian blue material helps to improve the chemical stability of the entire material;

[0030] Improve anti-interference ability: During the battery charging and discharging process, the electrolyte and electrode materials may be interfered by external ions; using bipyridine and phenanthroline as complexing agents can effectively shield these interferences because they can more effectively form protective complex rings with iron ions, thereby reducing the impact of external factors on battery performance.

[0031] 2. Enhance electrochemical performance

[0032] Promoting electron transfer efficiency: Bipyridine and phenanthroline can enhance the mobility of electrons in the complex due to their good conjugated structure and the coordination ability of nitrogen atoms; this enhanced electron transfer efficiency can directly improve the charge and discharge rate and efficiency of the battery, thereby improving the overall performance of the iron-based Prussian blue battery;

[0033] Optimizing redox reactions: During the charge and discharge cycle of the battery, the oxidation state of the iron ion changes; the addition of bipyridine and phenanthroline helps stabilize these oxidation state changes, reduce energy loss, and improve the reversibility of the redox reaction, which is critical to extending the battery life. DETAILED DESCRIPTION

[0034] The following is a further clear and complete description of the technical features in the technical solution provided by the present invention in conjunction with the specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Battery assembly: The iron-based Prussian blue positive electrode materials prepared in the embodiment and the comparative example were respectively used as active materials, and the mass ratio of active materials: ultrafine carbon powder (SP): polyvinylidene fluoride was 90:5:5. N-methylpyrrolidone (NMP) was added to prepare a viscous glue, which was coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12h as the positive electrode; a metal sodium sheet was used as the negative electrode; a glass fiber (Waterman) was used as a separator, and 1 mol / L NaPF 6 (EC and PC with a solvent mass ratio of 1:1) were used as the electrolyte to assemble 2032 button-type sodium-ion batteries in an Ar-protected glove box. Constant current charge and discharge mode was adopted in the voltage range of 2.0-4.0 V, and the electrochemical performance tests were carried out on a NEWARE tester: the discharge specific capacity at a current density of 20 C, and the battery capacity retention rate after 1000 cycles.

[0036] Example 1

[0037] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0038] S1: Dissolve 5 g of sodium ferrocyanide and 15 g of sodium salt in 40 g of deionized water to form solution A;

[0039] S2: Dissolve 5 g of iron salt in 40 g of deionized water to form solution B;

[0040] S3: Dissolve 40 g of sodium citrate and 0.03 g of a complexing agent in 100 g of deionized water to form solution C;

[0041] S4: Solutions A and B are pumped in N 2 Under the atmosphere, slowly add it dropwise to solution C, stir and react for 5 h at 50 °C and 300 rpm, and age for 16 h;

[0042] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 100° C. for 20 h to obtain an iron-based Prussian blue positive electrode material.

[0043] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 100 μL / min.

[0044] The sodium salt is sodium chloride.

[0045] The iron salt is ferric sulfate.

[0046] The preparation method of the complexing agent is as follows:

[0047] 4 g of allyltributylphosphonium chloride, 0.05 g of 6-amino-2,2'-bipyridine, 0.003 g of 1,10-phenanthroline-4,7-diamine, 100 g of toluene, and 0.5 g of sodium ethoxide were stirred for reaction for 50 minutes. After the reaction was completed, the toluene was removed by vacuum distillation to obtain a complexing agent.

[0048] Example 2

[0049] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0050] S1: Dissolve 6 g of sodium ferrocyanide and 18 g of sodium salt in 43 g of deionized water to form solution A;

[0051] S2: Dissolve 6 g of iron salt in 43 g of deionized water to form solution B;

[0052] S3: Dissolve 43 g of sodium citrate and 0.1 g of a complexing agent in 140 g of deionized water to form solution C;

[0053] S4: Solutions A and B are pumped in N 2 In the atmosphere, slowly add dropwise to solution C, stir and react for 6 h at 60 °C and 350 rpm, and age for 18 h;

[0054] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 105°C for 22 hours to obtain an iron-based Prussian blue positive electrode material.

[0055] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 200 μL / min.

[0056] The sodium salt is sodium carbonate.

[0057] The iron salt is ferrous sulfate.

[0058] The preparation method of the complexing agent is as follows:

[0059] 6 g of allyltributylphosphonium chloride, 0.2 g of 6-amino-2,2'-bipyridine, 0.02 g of 1,10-phenanthroline-4,7-diamine, 110 g of toluene, and 1 g of sodium ethoxide were stirred for reaction for 60 minutes. After the reaction was completed, the toluene was removed by vacuum distillation to obtain a complexing agent.

[0060] Example 3

[0061] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0062] S1: Dissolve 8 g of sodium ferrocyanide and 23 g of sodium salt in 48 g of deionized water to form solution A;

[0063] S2: 8 g of iron salt was dissolved in 48 g of deionized water to form solution B;

[0064] S3: Dissolve 48 g of sodium citrate and 0.3 g of a complexing agent in 180 g of deionized water to form solution C;

[0065] S4: Solutions A and B are pumped in N 2 In the atmosphere, slowly add it dropwise to solution C, stir and react for 8 h at 70 °C and 450 rpm, and age for 22 h;

[0066] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 115°C for 24 hours to obtain an iron-based Prussian blue positive electrode material.

[0067] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 400 μL / min.

[0068] The sodium salt is sodium acetate.

[0069] The iron salt is ferric acetate.

[0070] The preparation method of the complexing agent is as follows:

[0071] 8 g of allyltributylphosphonium chloride, 0.4 g of 6-amino-2,2'-bipyridine, 0.04 g of 1,10-phenanthroline-4,7-diamine, 140 g of toluene, and 1.5 g of sodium ethoxide were stirred for reaction for 90 minutes. After the reaction was completed, the toluene was removed by vacuum distillation to obtain a complexing agent.

[0072] Example 4

[0073] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0074] S1: Dissolve 10 g of sodium ferrocyanide and 25 g of sodium salt in 50 g of deionized water to form solution A;

[0075] S2: Dissolve 10 g of iron salt in 50 g of deionized water to form solution B;

[0076] S3: Dissolve 50 g of sodium citrate and 0.4 g of a complexing agent in 200 g of deionized water to form solution C;

[0077] S4: Solutions A and B are pumped in N 2 In the atmosphere, slowly add it dropwise to solution C, stir and react for 10 h at 80 °C and 500 rpm, and age for 24 h;

[0078] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 120° C. for 25 h to obtain an iron-based Prussian blue positive electrode material.

[0079] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 500 μL / min.

[0080] The sodium salt is sodium nitrate.

[0081] The iron salt is ferric nitrate.

[0082] The preparation method of the complexing agent is as follows:

[0083] 10 g of allyltributylphosphonium chloride, 0.5 g of 6-amino-2,2'-bipyridine, 0.05 g of 1,10-phenanthroline-4,7-diamine, 150 g of toluene, and 2 g of sodium ethoxide were stirred for reaction for 100 minutes. After the reaction was completed, the toluene was removed by vacuum distillation to obtain a complexing agent.

[0084] Comparative Example 1

[0085] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0086] S1: Dissolve 5 g of sodium ferrocyanide and 15 g of sodium salt in 40 g of deionized water to form solution A;

[0087] S2: Dissolve 5 g of iron salt in 40 g of deionized water to form solution B;

[0088] S3: dissolving 40 g of sodium citrate in 100 g of deionized water to form solution C;

[0089] S4: Solutions A and B are pumped in N 2 Under the atmosphere, slowly add it dropwise to solution C, stir and react for 5 h at 50 °C and 300 rpm, and age for 16 h;

[0090] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 100° C. for 20 h to obtain an iron-based Prussian blue positive electrode material.

[0091] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 100 μL / min.

[0092] The sodium salt is sodium chloride.

[0093] The iron salt is ferric sulfate.

[0094] Comparative Example 2

[0095] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0096] S1: Dissolve 5 g of sodium ferrocyanide and 15 g of sodium salt in 40 g of deionized water to form solution A;

[0097] S2: Dissolve 5 g of iron salt in 40 g of deionized water to form solution B;

[0098] S3: Dissolve 40 g of sodium citrate and 0.03 g of a complexing agent in 100 g of deionized water to form solution C;

[0099] S4: Solutions A and B are pumped in N 2 Under the atmosphere, slowly add it dropwise to solution C, stir and react for 5 h at 50 °C and 300 rpm, and age for 16 h;

[0100] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 100° C. for 20 h to obtain an iron-based Prussian blue positive electrode material.

[0101] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 100 μL / min.

[0102] The sodium salt is sodium chloride.

[0103] The iron salt is ferric sulfate.

[0104] The preparation method of the complexing agent is as follows:

[0105] 4 g of propylene tributyl phosphonium chloride, 0.003 g of 1,10-phenanthroline-4,7-diamine, 100 g of toluene, and 0.5 g of sodium ethoxide were stirred for reaction for 50 minutes. After the reaction was completed, the toluene was removed by vacuum distillation to obtain a complexing agent.

[0106] Comparative Example 3

[0107] A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are:

[0108] S1: Dissolve 5 g of sodium ferrocyanide and 15 g of sodium salt in 40 g of deionized water to form solution A;

[0109] S2: Dissolve 5 g of iron salt in 40 g of deionized water to form solution B;

[0110] S3: Dissolve 40 g of sodium citrate and 0.03 g of a complexing agent in 100 g of deionized water to form solution C;

[0111] S4: Solutions A and B are pumped in N 2 Under the atmosphere, slowly add it dropwise to solution C, stir and react for 5 h at 50 °C and 300 rpm, and age for 16 h;

[0112] S5: After aging, the precipitate was centrifuged and washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum drying oven at 100° C. for 20 h to obtain an iron-based Prussian blue positive electrode material.

[0113] The solutions A and B were pumped in N 2 The drop rate under atmosphere was 100 μL / min.

[0114] The sodium salt is sodium chloride.

[0115] The iron salt is ferric sulfate.

[0116] The preparation method of the complexing agent is as follows:

[0117] 4 g of allyltributylphosphonium chloride, 0.05 g of 6-amino-2,2'-bipyridine, 100 g of toluene, and 0.5 g of sodium ethoxide were stirred for reaction for 50 minutes. After the reaction was completed, the toluene was removed by vacuum distillation to obtain a complexing agent.

[0118] Test results:

[0119] Discharge specific capacity / mAh / g Capacity retention rate / % Example 1 122.8 95.6 Example 2 125.4 96.3 Example 3 128.7 97.5 Example 4 131.5 98.1 Comparative Example 1 93.6 80.7 Comparative Example 2 115.3 89.8 Comparative Example 3 116.1 91.2

[0120] Through the data analysis of the above embodiments and comparative examples, the iron-based Prussian blue positive electrode material prepared by the present invention can effectively enhance the electrochemical performance.

[0121] The above is only a preferred embodiment of the present invention and is not intended to limit the invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing an iron-based Prussian blue positive electrode material, the operating steps of which are: S1: Dissolve 5-10 parts of sodium ferrocyanide and 15-25 parts of sodium salt in 40-50 parts of deionized water to form solution A; S2: dissolving 5-10 parts of iron salt in 40-50 parts of deionized water to form solution B; S3: dissolving 40-50 parts of sodium citrate and 0.03-0.4 parts of a complexing aid in 100-200 parts of deionized water to form a solution C; S4: Solutions A and B are slowly added dropwise to solution C using a peristaltic pump under N2 atmosphere, stirred for reaction at 50-80°C and 300-500 rpm for 5-10 h, and aged for 16-24 h; S5: After aging, centrifugation is performed, and the precipitate is washed twice with anhydrous ethanol and twice with deionized water, and then placed in a vacuum drying oven at 100-120° C. for 20-25 hours to obtain an iron-based Prussian blue positive electrode material.

2. The method for preparing an iron-based Prussian blue positive electrode material according to claim 1, characterized in that: The solutions A and B were added by a peristaltic pump at a dropping rate of 100-500 μL / min under a N2 atmosphere.

3. The method for preparing an iron-based Prussian blue positive electrode material according to claim 1, characterized in that: The sodium salt is one of sodium chloride, sodium carbonate, sodium acetate and sodium nitrate.

4. The method for preparing an iron-based Prussian blue positive electrode material according to claim 1, characterized in that: The iron salt is one of ferric sulfate, ferrous sulfate, ferric acetate, ferrous acetate, ferric chloride, ferrous chloride and ferric nitrate.

5. The method for preparing an iron-based Prussian blue positive electrode material according to claim 1, characterized in that: The preparation method of the complexing agent is as follows: According to weight, 4-10 parts of propylene tributyl phosphonium chloride, 0.05-0.5 parts of 6-amino-2,2'-bipyridine, 0.003-0.05 parts of 1,10-phenanthroline-4,7-diamine, 100-150 parts of toluene, and 0.5-2 parts of sodium ethoxide are stirred for reaction for 50-100 minutes. After the reaction is completed, the toluene is removed by reduced pressure distillation to obtain a complexing agent.

Citation Information

Patent Citations

  • Photocatalytic color switching of redox imaging nanomaterials of rewritable media

    CN107209450A

  • Industrial preparation method of superfine iron-based prussian blue analogue

    CN115490245A

  • Chiral dopant, liquid composition containing the chiral dopant and liquid crystal element using the composition

    JP2004035627A