High-thermal-conductivity heterostructure near-infrared fluorescent ceramic, preparation method and application of high-thermal-conductivity heterostructure near-infrared fluorescent ceramic in near-infrared detection of grain quality

Through the periodically arranged square mesh skeleton structure heterogeneous fluorescent ceramics, the problem of difficult to take into account both the heat transfer and fluorescence efficiency of fluorescent ceramics is solved, high thermal conductivity and high light extraction efficiency are achieved, and the resistance to thermal fracture is enhanced. It is suitable for large-scale Power lighting and near-infrared light display.

CN119080479AActive Publication Date: 2024-12-06HENAN UNIVERSITY OF TECHNOLOGY
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202411197854.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The problems of fluorescent ceramics in the difficult to balance heat transfer and fluorescence efficiency, and the disordered refraction of the beam and thermally induced fracture limit their development in the fields of high-power illumination and near-infrared light display.

Method used

The square mesh skeleton structure heterogeneous fluorescent ceramics are used to fill the microscopic voids of the square mesh skeleton ceramics, and the high thermal conductivity heterogeneous structure is constructed by photocuring 3D printing technology and gel technology. Achieve orderly scattering and efficient heat transmission of light beams in ceramic bodies.

Benefits of technology

It significantly improves the thermal conductivity coefficient of the ceramic and the ordered beam scattering efficiency, avoids heat accumulation, enhances the resistance to thermal fracture, and improves the light extraction efficiency and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080479A_ABST
    Figure CN119080479A_ABST
Patent Text Reader

Abstract

The invention discloses a high-thermal-conductivity heterostructure near-infrared fluorescent ceramic as well as a preparation method and application thereof. The high-thermal-conductivity heterostructure near-infrared fluorescent ceramic is periodically arranged square grid skeleton heterostructure fluorescent ceramic, and the periodically arranged square grid skeleton heterostructure fluorescent ceramic is utilized to solve the problems that heat transfer and fluorescence efficiency of a ceramic body are difficult to consider, light beams are disorderly refracted and thermally induced fracture is caused. The preparation method comprises the following steps: preparing a ceramic biscuit by combining a photocuring 3D printing technology with a gel technology: printing gel-state slurry with a component X into periodically arranged square grid skeleton ceramics, and introducing near-infrared fluorescent ceramic slurry with a component Y into microscopic gaps of the square grid skeleton ceramics, and the periodically arranged square grid skeleton heterogeneous fluorescent ceramics are constructed. High absorption efficiency, high heat conduction and high light extraction efficiency can be achieved through the periodically-arranged square grid framework structure heterogeneous fluorescent ceramic, and the fluorescent ceramic and a blue laser / LED chip excitation source are packaged and then widely applied to the fields of illumination and grain quality near-infrared detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of fluorescent ceramic preparation, lighting and near-infrared light display, and specifically relates to a high thermal conductivity heterostructure near-infrared fluorescent ceramic, a preparation method and an application in near-infrared detection of grain quality. Background Art

[0002] Blue LED / laser excited fluorescent ceramics can be widely used in ultra-high brightness and long-distance lighting and display fields, such as automotive laser headlights, laser near-infrared detection and laser display. Researchers have studied the thermal conductivity, luminous efficiency, light color and light temperature of fluorescent ceramics through various methods and achieved remarkable results. However, fluorescent ceramics still have problems such as difficulty in balancing heat transfer and fluorescence efficiency, disordered refraction of light beams, and the physical direction and size of light beams, which greatly affect the application and promotion of fluorescent ceramics and also limit their development in the fields of high-power lighting and near-infrared light display.

[0003] In addition to the lighting field, the steps of near-infrared detection of grain quality are to irradiate the grain sample to be tested with near-infrared light to obtain the original spectrum of the absorbance value, then denoise, pre-process and screen the characteristic wavelengths of the original spectrum, and then substitute the characteristic wavelengths into the prediction model of the grain sample quality index to obtain the near-infrared detection value of the grain sample quality. The key to near-infrared detection of grain quality lies in the miniaturization of the light source (excitation source) device, and high luminous efficiency and high thermal stability must be considered in coordination. Existing near-infrared light sources and near-infrared luminescent materials have problems such as low luminous efficiency, poor thermal stability and low power, and there is no detection device for high-efficiency and high-heat-resistant laser near-infrared light sources in China. Therefore, it is urgent to explore high-efficiency and high-heat-resistant near-infrared fluorescent ceramics and their light sources under laser excitation.

[0004] A Chinese patent (publication number CN117585988A) discloses a multilayer composite structure ceramic with high thermal conductivity and high mechanical properties. The patent prepares single-layer blanks of alumina, yttrium oxide and aluminum nitride respectively by tape casting, and forms a composite structure ceramic after sequential cyclic lamination. A Chinese patent (publication number CN115519074A) discloses a composite structure ceramic core and its preparation method. The patent increases the high-temperature creep resistance of the main structure by bonding an alumina core in a hollow hole in a silicon-based ceramic core. A Chinese patent (publication number CN118206369A) discloses a composite structure fluorescent ceramic for regulating photothermal performance, which solves the problem of thermal runaway of the fluorescent body through a circumferentially arranged heat conduction aid. A Chinese patent (publication number CN118206379A) ​​discloses a fluorescent ceramic with a circumferentially coated multilayer ceramic structure for white light LEDs, which is mainly formed by tape casting lamination. However, the above patents all target specific problems and introduce macroscopic composite structures to enhance the photothermal function of a single ceramic block.

[0005] In addition, the invention patent CN114845978A discloses a ceramic structure, in which the first truss structure and the second truss structure are superimposed, and the through holes between the layers are perpendicular to each other, and the through holes serve as the flow path for the heat medium to flow. The core purpose of the ceramic is heat insulation or heat exchange. However, the essence of the patent belongs to a porous ceramic material with a heat dissipation channel. The invention patent (publication number CN114530439A) discloses a fluorescent heat dissipation integrated metal bracket material, the raw material of which is alumina or aluminum nitride, and the core preparation process is to use a constant pressure device to make the solid fluorescent sheet fit tightly with the metal ring and the metal heat dissipation bracket. The essence of the patent is only a physical combination. The invention patent (publication number CN113050228A) discloses a light source refractive ceramic bracket, the essence of which is to use the refractive prism diaphragm set at the direct light outlet of the ceramic to transmit the incident light signal in multiple branches and replicate independent light beams. However, after removing the refractive prism diaphragm, the patent will lose its light splitting function.

[0006] In summary, it is necessary to focus on the surface and interface construction of ceramic functional systems, realize the precise regulation of surface and interface structure and function, and thereby enhance the precise construction of the material information multifunctional guidance of ceramic blocks, which is of great significance for solving the problems of ceramics used in lighting and near-infrared light display. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a high thermal conductivity heterostructure near-infrared fluorescent ceramic and its preparation method and application, in view of the problems that current fluorescent ceramics have difficulty in balancing heat transfer and fluorescence efficiency, disordered refraction of light beams and thermal fracture, so as to solve the problems that heat transfer and fluorescence efficiency of the ceramic body are difficult to balance, disordered refraction of light beams and thermal fracture, and achieve high absorption efficiency, high thermal conductivity and high light extraction efficiency.

[0008] To achieve the above purpose, the present invention proposes a heterogeneous fluorescent ceramic with a periodically arranged square grid skeleton structure. The periodically arranged square grid skeleton structure can not only improve the thermal conductivity of the ceramic block, but also enable the orderly scattering of light beams in the ceramic block to enhance the luminous efficiency and the fluorescence conversion of the heterogeneous components orderly distributed in the microscopic gaps, which can be used as Ceramics resistant to thermally induced fracture at high temperatures for lighting and near-infrared light displays.

[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions: A near-infrared fluorescent ceramic with a high thermal conductivity heterogeneous structure, wherein the near-infrared fluorescent ceramic with a high thermal conductivity heterogeneous structure is a heterogeneous fluorescent ceramic with a periodically arranged square grid skeleton, wherein the fluorescent ceramic comprises a periodically arranged square grid skeleton ceramic and a near-infrared fluorescent ceramic filled in the gaps of the square grid skeleton ceramic, wherein the square grid skeleton is printed by a gel slurry with a component of X, and the component of the near-infrared fluorescent ceramic is Y, wherein X is at least one of Al2O3 and AlN; Y is aluminosilicate, and the luminescent center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+ At least one of the following: X can not only efficiently transmit heat to prevent the ceramic body from thermal failure, but also can control the orderly refraction of the light beam in the ceramic body. Y uses the ordered heterostructure in the ceramic body to emit high-quality near-infrared light under the excitation of the blue laser / LED chip. The periodically arranged square grid skeleton structure heterogeneous fluorescent ceramic can achieve high absorption efficiency, high thermal conductivity and high light extraction efficiency. After the fluorescent ceramic is packaged with the blue laser / LED chip excitation source, it is widely used in the field of lighting and near-infrared light display.

[0010] The basic unit of the periodically arranged square grid skeleton ceramic is composed of a first layer, a second layer, and a third layer of square grid skeleton ceramics arranged in sequence from bottom to top. The layer heights of the square grid skeleton ceramics are all 50 μm-150 μm, and the side lengths of the square grid skeleton ceramics are all 20-30 mm. The total height of the high thermal conductivity heterostructure near-infrared fluorescent ceramic, i.e., the periodically arranged square grid skeleton heterogeneous fluorescent ceramic, is 1.5-45 mm.

[0011] The grids constituting the square grid skeleton ceramics are squares, the grid side lengths of the first layer of square grid skeleton ceramics and the second layer of square grid skeleton ceramics are equal and are both 100μm-300μm, the grid side length of the third layer of square grid skeleton ceramics is 48%-52% of the grid side length of the first or second layer of square grid skeleton ceramics; the grid widths h of the first, second and third layers of square grid skeleton ceramics are equal and are 20μm-40μm.

[0012] The second layer of square grid skeleton ceramic is arranged on the first layer of square grid skeleton ceramic and the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap between the two is achieved. The third layer of square grid skeleton ceramic is arranged on the second layer of square grid skeleton ceramic and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved.

[0013] Furthermore, the periodically arranged square grid skeleton heterogeneous fluorescent ceramic is repeated with three layers of square grid skeleton ceramics formed by the first layer, the second layer and the third layer of square grid skeleton ceramics as a basic unit, and the number of repetitions is determined by the height of the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic finally obtained.

[0014] The present invention also provides a method for preparing the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic, which uses light-curing 3D printing technology combined with gel technology to construct a periodically arranged square grid skeleton heterogeneous fluorescent ceramic, including the following steps: (1) A ceramic blank is prepared by using a combination of light-curing 3D printing technology and gel technology: a gel slurry with a component X is printed into a periodically arranged square grid skeleton ceramic, a near-infrared fluorescent ceramic slurry with a component Y is introduced into the microscopic gaps of the square grid skeleton ceramic, and after the gel is cured, a periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank is constructed; (2) The periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank is fired and then sintered at high temperature to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

[0015] Furthermore, the method of printing the gel slurry with component X into a periodically arranged square grid skeleton ceramic in step (1) is as follows: ① Pre-drying the powder X, and then placing the powder X, surfactant ammonium oxide OA and anhydrous ethanol in a ball mill, and ball milling for 2-4 h at a rotation speed of 200-250 r / min to prepare a suspension, wherein the powder X is at least one of Al2O3 and AlN, with a particle size of 10-50 μm, the grinding ball is a high-purity alumina ball, and the mass of the surfactant ammonium oxide OA is 1 / 90-1 / 110 of the mass of the powder X, and the mass of the anhydrous ethanol is 2-3 times the mass of the powder X; using a rotary evaporator at a heating temperature of 50-70°C to remove the anhydrous ethanol in the suspension, and then placing it in an oven for heat treatment at 80°C-100°C for 5h-6h; after cooling to room temperature, grinding the obtained powder, and passing it through a 100-200 mesh sieve to obtain the modified powder X; ② Add pentaerythritol tetraacrylate, 1-6-hexanediol diacrylate, polyurethane acrylate, n-octanol, and polyethylene glycol to deionized water to prepare a premix, wherein the concentration of pentaerythritol tetraacrylate is 18-20 wt%, the concentration of 1-6-hexanediol diacrylate is 24-26 wt%, the concentration of polyurethane acrylate is 18-20 wt%, the concentration of n-octanol is 18-20 wt%, and the concentration of polyethylene glycol is 14-16 wt%. Add the modified powder X prepared in ① and 2 wt% of the mass of the powder X dispersant BYK 9077 to the premix, and ball mill for 10-12 h at a rotation speed of 300-350 r / min to prepare a square grid skeleton ceramic slurry with a solid content of 50 vol%-55 vol%; ③ Add 0.5-1.5 wt % of the photoinitiator Irgacure 819 to the square grid skeleton ceramic slurry, ball mill for 10-15 min at a rotation speed of 300-350 r / min, and then place it in the material tank of the DLP 3D printer; ④Set the printing parameters to layer thickness of 10 μm, single layer curing time of 3 s, and exposure energy density of 31.5 mj / cm 2 , using Solidworks software to build a three-dimensional model of the square grid skeleton structure of the first layer, and importing it into the printer through CeraRay software, preparing the square grid skeleton ceramic body of the first layer by cumulative printing layer by layer, and performing UV irradiation photocuring throughout the process to obtain the square grid skeleton ceramic body of the first layer; ⑤Put the first layer of square grid skeleton ceramic body back on the workbench of the 3D printer, use Solidworks software to build a three-dimensional model of the second layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the second layer of square grid skeleton ceramic body by cumulative printing layer by layer on the basis of the first layer, and perform UV irradiation photocuring throughout the process to obtain a double-layer square grid skeleton ceramic body, wherein the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap of the two is achieved; ⑥Put the double-layer square grid skeleton structure ceramic body back on the workbench of the 3D printer, use Solidworks software to establish a three-dimensional model of the third layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the third layer of square grid skeleton structure ceramic body by cumulative printing layer by layer on the square grid skeleton structure ceramic body, and perform UV irradiation photocuring throughout the process, and finally obtain a cured three-layer square grid skeleton ceramic, wherein the grid side length of the third layer of square grid skeleton ceramic is 48%-52% of the first layer or the second layer, and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked, and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved; ⑦ Place the three layers of square grid skeleton ceramics back on the workbench of the 3D printer, and repeat steps ④-⑥ until a periodically arranged square grid skeleton ceramic of the desired height is obtained.

[0016] Furthermore, the method of constructing a square grid skeleton heterogeneous fluorescent ceramic blank by introducing a near-infrared fluorescent ceramic slurry with a component Y into the microscopic gaps of the square grid skeleton in step (1) is as follows: the near-infrared ceramic slurry with a component Y is placed in a sealed container, and the container is placed in a micro-negative pressure environment by utilizing the suction effect of a negative pressure fan; the solidified periodically arranged square grid skeleton ceramic is placed in a sealed container, so that it is completely infiltrated by the micro-negative pressure slurry with a component Y and fills the microscopic gaps; the periodically arranged square grid skeleton ceramic filled with the Y slurry is moved into a temperature and humidity control box, the temperature is set to 40°C-50°C, the humidity is set to 60%-70%, and it is left to dry for 12-16 hours to obtain a square grid skeleton heterogeneous fluorescent ceramic blank.

[0017] Further, the preparation method of the near-infrared fluorescent ceramic slurry with component Y is as follows: ① Add dispersant ammonium citrate and pH regulator tetramethyl ammonium hydroxide to deionized water to prepare a premixed solution; wherein the concentration of the dispersant ammonium citrate is 0.5 wt%-0.8 wt%, and the concentration of the pH regulator tetramethyl ammonium hydroxide is 1.0 wt%-1.5 wt%; ②Pre-dry the component powder Y of the near-infrared fluorescent ceramic, add the powder Y into the premixed liquid in 5-6 times, and use an alumina ball mill to grind at a low speed of 60-100 r / min. The powder Y is aluminosilicate, and the luminescence center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+at least one of the following: the particle size of powder Y is 100-200 nm, the grinding balls are high-purity alumina balls, and the mass ratio of powder Y to grinding balls is 1:2; after all powder Y is added to the premixed liquid, ball milling is performed for 10-12 h to obtain a ceramic slurry with a solid content of 55 vol%-60 vol%; wherein powder Y is added to the premixed liquid for ball milling in 5-6 times, the amount added in the 1st to 2nd time is 10%-20% of the mass of powder Y, the amount added in the 3rd to 4th time is 30-40% of the mass of powder Y, and the amount added in the 5th to 6th time is 40%-60% of the mass of powder Y; ③ Add 1-3 wt% of monomer acrylamide AM and crosslinking agent N,N'-methylenebisacrylamide to the ceramic slurry obtained in ②, the mass ratio of AM to N,N'-methylenebisacrylamide is 1 / 12-1 / 14, and continue ball milling for 4-6 h to obtain a uniform ceramic slurry; ④ Pour the uniformly ball-milled ceramic slurry obtained in ③ into a vacuum defoaming tank. Based on the mass of the uniformly ball-milled ceramic slurry, add 0.1-0.3 wt.% of catalyst tetramethylethylenediamine and 0.2-0.3 wt.% of initiator ammonium persulfate. Defoam for 3 min using a rotary vacuum defoamer, and gently stir with a glass rod for 10-12 s to obtain a near-infrared ceramic slurry with a component Y, wherein the catalyst tetramethylethylenediamine is added in the form of an aqueous solution with a mass concentration of 75%, and the initiator ammonium persulfate is added in the form of an aqueous solution with a mass concentration of 95%.

[0018] Furthermore, the specific operation of biscuit firing in step (2) is as follows: placing the heterogeneous fluorescent ceramic biscuit in an alumina crucible, heating the biscuit to 380°C-400°C at a heating rate of 0.5-0.6°C / min and keeping the temperature for 12 h-16 h, heating the biscuit to 750°C-850°C at a heating rate of 1-2°C / min and keeping the temperature for 7 h-9 h, and biscuit firing in a muffle furnace to discharge organic matter in the biscuit.

[0019] Furthermore, the high temperature sintering operation in step (2) is as follows: the bisque-fired heterogeneous fluorescent ceramic blank is heated to 1500°C-1550°C in a nitrogen atmosphere or an argon atmosphere at a heating rate of 0.3°C / min-0.5°C / min and kept at that temperature for 10-15 h. After the heat preservation, the temperature is cooled to room temperature at a cooling rate of 0.6°C / min-0.8°C / min to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

[0020] The present invention also provides the application of the high thermal conductivity heterostructure near-infrared fluorescent ceramic in the field of fluorescent conversion lighting and near-infrared light display. The composite structure heterogeneous fluorescent ceramic with multifunctional guidance and precision construction for lighting and near-infrared light display provided by the present invention can simultaneously improve the thermal conductivity and orderly scattering of light beams to enhance luminous efficiency. When the high thermal conductivity heterostructure near-infrared fluorescent ceramic is applied to lighting and near-infrared light display devices, the excitation source is a blue laser or a blue LED chip, and the thermal conductivity of the high thermal conductivity heterostructure near-infrared fluorescent ceramic is 20-275 Wm −1 K −1 , the luminous efficiency is 200-290lm / W.

[0021] The present invention also provides an application of the high thermal conductivity heterostructure near-infrared fluorescent ceramic in the field of near-infrared grain detection. When the high thermal conductivity heterostructure near-infrared fluorescent ceramic is applied to NIR-LED / LD devices, the wavelength range is 700-1500nm, the photoelectric conversion efficiency is 20%-30%, and the correlation coefficient is 0.9870-0.9990.

[0022] Compared with the prior art, the present invention has the following beneficial effects: (1) The square grid skeleton structure heterogeneous fluorescent ceramics with periodic arrangement proposed in the present invention can significantly reduce the phonon scattering of heat at the interface of heterogeneous ceramics and reduce the thermal resistance of the heterogeneous interface by using the heterogeneous surface interface structure. Importantly, the square grid skeleton structure proposed in the present invention relies on the microscopic efficient interconnected heat conduction channels in the ceramic block to significantly improve the thermal conductivity of the ceramic block, with a thermal conductivity coefficient of up to 20-275 Wm −1 K −1 , which is much higher than the thermal conductivity of the fluorescent material with component Y in the ceramic block.

[0023] (2) The heterogeneous fluorescent ceramics with periodic arrangement of square grid skeleton structure proposed in the present invention utilize the microscopic efficient interconnected heat conduction channels in the ceramic block and the heterogeneous heterogeneous microscopic interface structure to solve the heat transport problem of near-infrared fluorescent ceramics, thereby avoiding the heat accumulation phenomenon in the ceramic block under high-power LD / LED excitation. The waste heat generated by the fluorescent material with the component Y dispersed in the ceramic block is efficiently dissipated.

[0024] (3) The heterogeneous fluorescent ceramics with periodically arranged square grid skeleton structure proposed in the present invention, the microscopic heterogeneous interface composed of AlN and Al2O3 with matching thermal expansion coefficients and fluorescent materials can reduce the stress concentration and damage in the ceramic block caused by temperature changes, and improve the reliability, durability and resistance to thermal fracture of the ceramic block during thermal cycling. The microscopic efficient interconnected heat conduction channels in the ceramic block have a much higher resistance to thermal shock than the fluorescent material with component Y dispersed in the ceramic block. Therefore, the ceramics proposed in the present invention are extremely resistant to thermal fracture.

[0025] (4) The heterogeneous fluorescent ceramic with a periodically arranged square grid skeleton structure proposed in the present invention refracts the excitation light beam onto the fluorescent material multiple times through the refractive index difference between the AlN and Al2O3 materials of the square grid skeleton structure and the fluorescent material dispersed in the ceramic block, thereby increasing the orderly refraction of the light beam and greatly improving the light extraction efficiency in the ceramic block.

[0026] (5) The heterogeneous fluorescent ceramic with a periodically arranged square grid skeleton structure proposed in the present invention can effectively change the light emitting direction of the ceramic block and the physical size of the light beam by designing the number of periods of the square grid skeleton structure, that is, the number of cycles of the three-layer square grid skeleton ceramic. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the periodically arranged square skeleton ceramic structure of the present invention (only the first, second and third layers are listed). DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. The raw materials used in the following examples are all commercially available products with a purity greater than 99.9%. The particle size range of X is 10-50 μm, and the particle size range of each component in Y is 100-200 nm.

[0029] Example 1 like Figure 1 As shown, a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic, the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic is a periodically arranged square grid skeleton heterogeneous fluorescent ceramic, the fluorescent ceramic includes a periodically arranged square grid skeleton ceramic and a near-infrared fluorescent ceramic filled in the gaps of the square grid skeleton ceramic, the square grid skeleton is printed by a gel slurry with a component of X, the component of the near-infrared fluorescent ceramic is Y, wherein X is AlN; Y is aluminosilicate, and the luminescent center is Cr 3+ 、Ce 3+ .

[0030] The basic unit of the periodically arranged square grid skeleton ceramic is composed of a first layer, a second layer, and a third layer of square grid skeleton ceramics. The areas of the first layer, the second layer, and the third layer of square grid skeleton ceramics are equal. The height of each layer of square grid skeleton ceramics, i.e., the layer height, is 50 μm, and the side length is 20 mm. The total height of the high thermal conductivity heterostructure near-infrared fluorescent ceramic is 15 mm.

[0031] The grids constituting the square grid skeleton ceramics are all squares, wherein the grid sides of the first layer of square grid skeleton ceramics 1 and the second layer of square grid skeleton ceramics 2 are equal to 100 μm, and the grid side length of the third layer of square grid skeleton ceramics 3 is 48%-52% of the grid side length of the first or second layer of square grid skeleton ceramics, i.e., about 50 μm, and the width h is 20 μm.

[0032] The second layer of square grid skeleton ceramic 2 is arranged on the first layer of square grid skeleton ceramic 1 and the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap between the two is achieved. The third layer of square grid skeleton ceramic 3 is arranged on the second layer of square grid skeleton ceramic and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved.

[0033] The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic for LED / laser lighting in this embodiment comprises the following steps: (1) Using photocuring 3D printing technology combined with gel technology to prepare ceramic green body: Print the gel slurry with component X into a periodically arranged square grid skeleton ceramic. The specific steps are as follows: ① Pre-dry the powder X, then place the powder X, surfactant ammonium oxide OA and anhydrous ethanol in a ball mill, and ball mill for 2 hours at a rotation speed of 200 r / min to prepare a suspension, wherein the powder X is at least one of Al2O3 and AlN, with a particle size of 10 μm, the grinding balls are high-purity alumina balls, the mass of surfactant ammonium oxide OA is 1 / 90 of the mass of the powder X, and the mass of anhydrous ethanol is twice the mass of the powder X; use a rotary evaporator at a heating temperature of 50°C to remove the anhydrous ethanol in the suspension, and then place it in an oven for heat treatment at 80°C for 5 hours; after cooling to room temperature, grind the obtained powder and pass it through a 100-mesh sieve to obtain the modified powder X; ② Add pentaerythritol tetraacrylate, 1-6-hexanediol diacrylate, polyurethane acrylate, n-octanol, and polyethylene glycol to deionized water to prepare a premix, wherein the concentration of pentaerythritol tetraacrylate is 19 wt%, the concentration of 1-6-hexanediol diacrylate is 25 wt%, the concentration of polyurethane acrylate is 20 wt%, the concentration of n-octanol is 20 wt%, and the concentration of polyethylene glycol is 16 wt%. Add the modified powder X prepared in ① and the dispersant BYK9077 accounting for 2 wt% of the mass of the powder X to the premix, and ball mill for 10 h at a rotation speed of 300 r / min to prepare a square grid skeleton ceramic slurry with a solid content of 50 vol%; ③ Add the photoinitiator Irgacure 819, which accounts for 0.5wt% of the total mass of the square grid skeleton ceramic slurry, into the square grid skeleton structure ceramic slurry, ball mill for 10min at a rotation speed of 300 r / min, and then place it in the material tank of the DLP 3D printer; ④Set the printing parameters to layer thickness of 10 μm, single layer curing time of 3 s, and exposure energy density of 31.5 mj / cm 2 , using Solidworks software to build a three-dimensional model of the square grid skeleton structure of the first layer, and importing it into the printer through CeraRay software, preparing the square grid skeleton ceramic body of the first layer by cumulative printing layer by layer, and performing UV irradiation photocuring throughout the process to obtain the square grid skeleton ceramic body of the first layer; ⑤Put the first layer of square grid skeleton ceramic body back on the workbench of the 3D printer, use Solidworks software to build a three-dimensional model of the second layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the second layer of square grid skeleton ceramic body by cumulative printing layer by layer on the basis of the first layer, and perform UV irradiation photocuring throughout the process to obtain a double-layer square grid skeleton ceramic body, wherein the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap of the two is achieved; ⑥Put the double-layer square grid skeleton structure ceramic body back on the workbench of the 3D printer, use Solidworks software to establish a three-dimensional model of the third layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the third layer of square grid skeleton structure ceramic body by cumulative printing layer by layer on the square grid skeleton structure ceramic body, and perform UV irradiation photocuring throughout the process, and finally obtain a cured three-layer square grid skeleton ceramic, wherein the grid side length of the third layer of square grid skeleton ceramic is 48-52% of the first or second layer, that is, about 50 μm, and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked, and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved; ⑦ Place the three-layer square grid skeleton ceramic back on the workbench of the 3D printer, and repeat steps ④-⑥ 10 times until a periodically arranged square grid skeleton ceramic with a total height of 1.5 mm is obtained. It should be noted that the first layer of the periodically repeatedly printed square grid skeleton ceramic is strictly aligned with the first layer of the square grid skeleton ceramic printed in the previous cycle.

[0034] (2) Introducing a near-infrared fluorescent ceramic slurry with a component of Y into the microscopic voids of the square grid skeleton ceramic obtained in (1), and constructing a periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank after the gel is cured; the method is as follows: ① Add dispersant ammonium citrate and pH regulator tetramethyl ammonium hydroxide to deionized water to prepare a premixed solution; wherein the concentration of the dispersant ammonium citrate is 0.5wt%, and the concentration of the pH regulator tetramethyl ammonium hydroxide is 1.0wt%; ②Pre-dry the powder Y of the near-infrared fluorescent ceramic component, add the powder Y into the premixed liquid in 5 times, and use an alumina ball mill to grind at a low speed of 60r / min. The powder Y is aluminosilicate, and the luminescent center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+ At least one of the following: the particle size of powder Y is 100 nm, the grinding balls are high-purity alumina balls, and the mass ratio of powder Y to grinding balls is 1:2; after all powder Y is added to the premixed liquid, ball milling is performed for 10 hours to obtain a ceramic slurry with a solid content of 55 vol%; wherein powder Y is added to the premixed liquid for ball milling in 5 times, the amount added in the 1st-2nd time is 20% of the mass of powder Y, the amount added in the 3rd-4th time is 40% of the mass of powder Y, and the amount added in the 5th time is 40% of the mass of powder Y; ③ Add 1wt% of monomer acrylamide AM and crosslinking agent N,N'-methylenebisacrylamide to the ceramic slurry obtained in ②, the mass ratio of AM to N,N'-methylenebisacrylamide is 1 / 12, and continue ball milling for 4h to obtain a uniform ceramic slurry; ④ Pour the uniformly ball-milled ceramic slurry obtained in ③ into a vacuum defoaming tank, and add 0.1wt.% of catalyst tetramethylethylenediamine and 0.2wt.% of initiator ammonium persulfate based on the mass of the uniformly ball-milled ceramic slurry, defoam for 3 min with a rotary vacuum defoamer, and gently stir with a glass rod for 10s to obtain a near-infrared ceramic slurry with a component Y, wherein the catalyst tetramethylethylenediamine is added in the form of an aqueous solution with a mass concentration of 75%, and the initiator ammonium persulfate is added in the form of an aqueous solution with a mass concentration of 95%; ⑤ Place the near-infrared ceramic slurry with component Y into a sealed container, and make the container in a micro-negative pressure environment by utilizing the suction effect of the negative pressure fan; place the cured periodically arranged square grid skeleton ceramic in a sealed container so that it is completely infiltrated by the micro-negative pressure slurry with component Y and filled with microscopic gaps, move the periodically arranged square grid skeleton ceramic filled with Y slurry into a temperature and humidity control box, set the temperature to 40°C and the humidity to 60%, and let it stand and dry for 12 hours to obtain the square grid skeleton heterogeneous fluorescent ceramic blank.

[0035] (3) The periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank was placed in an alumina crucible, heated to 380°C at a heating rate of 0.5°C / min and kept at this temperature for 12 h, then heated to 750°C at a heating rate of 1°C / min and kept at this temperature for 7 h, and sintered in a muffle furnace to remove organic matter from the blank. The sintered heterogeneous fluorescent ceramic blank was heated to 1500°C at a heating rate of 0.3°C / min in a nitrogen atmosphere or an argon atmosphere and kept at this temperature for 10 h. After the end of the heat preservation, the blank was cooled to room temperature at a cooling rate of 0.6°C / min to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

[0036] The thermal conductivity of the periodically arranged non-continuous truss structure heterogeneous fluorescent ceramic prepared in this embodiment is 20Wm −1 K −1 ; Under the excitation of 450nm blue light LED, the luminous efficiency is as high as 208.6lm / W; under the excitation of 450nm blue light LD, the luminous efficiency is as high as 264.2lm / W.

[0037] When high thermal conductivity heterostructure near-infrared fluorescent ceramics and LEDs are packaged into NIR-LED devices and applied to grain detection, the emission spectrum covers a range of 700-1500nm. When the driving current is 180 mA, the photoelectric conversion efficiency is 20% and the correlation coefficient is 0.9870. When heterostructure near-infrared fluorescent ceramics and blue light LDs are packaged into NIR-LD devices and applied to grain detection, the emission spectrum covers a range of 700-1500nm.

[0038] Example 2 like Figure 1 As shown, a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic, the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic is a periodically arranged square grid skeleton heterogeneous fluorescent ceramic, the fluorescent ceramic includes a periodically arranged square grid skeleton ceramic and a near-infrared fluorescent ceramic filled in the gaps of the square grid skeleton ceramic, the square grid skeleton is printed by a gel slurry with a component of X, and the component of the near-infrared fluorescent ceramic is Y, wherein X is Al2O3; Y is aluminosilicate, and the luminescence center is Cr 3+ , Yb 3+ .

[0039] The basic unit of the periodically arranged square grid skeleton ceramic is composed of a first layer, a second layer, and a third layer of square grid skeleton ceramics. The areas of the first layer, the second layer, and the third layer of square grid skeleton ceramics are equal. The height of each layer of square grid skeleton ceramics, i.e., the layer height, is 150 μm, and the side length is 30 mm. The total height of the high thermal conductivity heterostructure near-infrared fluorescent ceramic is 45 mm.

[0040] The grids constituting the square grid skeleton ceramics are all squares, wherein the grid sides of the first layer of square grid skeleton ceramics 1 and the second layer of square grid skeleton ceramics 2 are equal in length, both being 300 μm, and the grid sides of the third layer of square grid skeleton ceramics 3 are 48%-52% of the grid sides of the first or second layer of square grid skeleton ceramics, i.e., about 150 μm, and the width h is 40 μm.

[0041] Other implementations are the same as in Example 1.

[0042] The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic for LED / laser lighting in this embodiment comprises the following steps: (1) Using photocuring 3D printing technology combined with gel technology to prepare ceramic green body: Print the gel slurry with component X into a periodically arranged square grid skeleton ceramic. The specific steps are as follows: ① Pre-dry the powder X, then place the powder X, surfactant ammonium oxide OA and anhydrous ethanol in a ball mill, and mill for 4 h at a rotation speed of 250 r / min to prepare a suspension, wherein the powder X is at least one of Al2O3 and AlN, with a particle size of 50 μm, the grinding balls are high-purity alumina balls, the mass of surfactant ammonium oxide OA is 1 / 110 of the mass of the powder X, and the mass of anhydrous ethanol is 3 times the mass of the powder X; use a rotary evaporator at a heating temperature of 70°C to remove the anhydrous ethanol in the suspension, and then place it in an oven for heat treatment at 100°C for 6h; after cooling to room temperature, grind the obtained powder and pass it through a 200-mesh sieve to obtain the modified powder X; ② Add pentaerythritol tetraacrylate, 1-6-hexanediol diacrylate, polyurethane acrylate, n-octanol and polyethylene glycol to deionized water to prepare a premix, wherein the concentration of pentaerythritol tetraacrylate is 20 wt%, the concentration of 1-6-hexanediol diacrylate is 26 wt%, the concentration of polyurethane acrylate is 20 wt%, the concentration of n-octanol is 18 wt%, and the concentration of polyethylene glycol is 16 wt%. Add the modified powder X prepared in ① and the dispersant BYK9077 accounting for 2 wt% of the mass of the powder X to the premix, and ball mill for 12 h at a rotation speed of 350 r / min to prepare a square grid skeleton ceramic slurry with a solid content of 55 vol%; ③ Add 1.5 wt % of the photoinitiator Irgacure 819 to the square grid skeleton ceramic slurry, ball mill for 15 min at a speed of 350 r / min, and then place it in the material tank of the DLP3D printer; ④Set the printing parameters to layer thickness of 10 μm, single layer curing time of 3 s, and exposure energy density of 31.5 mj / cm 2, using Solidworks software to build a three-dimensional model of the square grid skeleton structure of the first layer, and importing it into the printer through CeraRay software, preparing the square grid skeleton ceramic body of the first layer by cumulative printing layer by layer, and performing UV irradiation photocuring throughout the process to obtain the square grid skeleton ceramic body of the first layer; ⑤Put the first layer of square grid skeleton ceramic body back on the workbench of the 3D printer, use Solidworks software to build a three-dimensional model of the second layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the second layer of square grid skeleton ceramic body by cumulative printing layer by layer on the basis of the first layer, and perform UV irradiation photocuring throughout the process to obtain a double-layer square grid skeleton ceramic body, wherein the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap of the two is achieved; ⑥Put the double-layer square grid skeleton structure ceramic body back on the workbench of the 3D printer, use Solidworks software to establish a three-dimensional model of the third layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the third layer of square grid skeleton structure ceramic body by cumulative printing layer by layer on the square grid skeleton structure ceramic body, and perform UV irradiation photocuring throughout the process, and finally obtain a cured three-layer square grid skeleton ceramic, wherein the grid side length of the third layer of square grid skeleton ceramic is 48%-52% of the first or second layer, that is, about 150 μm, and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked, and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved; ⑦ Place the three-layer square grid skeleton ceramic back on the workbench of the 3D printer, and repeat steps ④-⑥ 100 times until a periodically arranged square grid skeleton ceramic with a total height of 45 mm is obtained.

[0043] (2) Introducing a near-infrared fluorescent ceramic slurry with a component of Y into the microscopic voids of the square grid skeleton ceramic obtained in (1), and constructing a periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank after the gel is cured; the method is as follows: ① Add dispersant ammonium citrate and pH regulator tetramethylammonium hydroxide to deionized water to prepare a premixed solution; wherein the concentration of dispersant ammonium citrate is 0.8 wt %, and the concentration of pH regulator tetramethylammonium hydroxide is 1.5 wt %; ②Pre-dry the component powder Y of the near-infrared fluorescent ceramic, add the powder Y into the premixed liquid in 6 times, and use an alumina ball mill to grind at a low speed of 100 r / min. The powder Y is aluminosilicate, and the luminescence center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+ At least one of the following: the particle size of powder Y is 200 nm, the grinding balls are high-purity alumina balls, and the mass ratio of powder Y to grinding balls is 1:2; after all powder Y is added to the premixed liquid, ball milling is performed for 10-12 h to obtain a ceramic slurry with a solid content of 60 vol%; wherein powder Y is added to the premixed liquid for ball milling in 6 times, the amount added in the 1st to 2nd times is 10% of the mass of powder Y, the amount added in the 3rd to 4th times is 30% of the mass of powder Y, and the amount added in the 5th to 6th times is 60% of the mass of powder Y; ③ Add 3 wt% of monomer acrylamide AM and cross-linking agent N,N'-methylenebisacrylamide to the ceramic slurry obtained in ②, the mass ratio of AM to N,N'-methylenebisacrylamide is 1 / 14, and continue ball milling for 6 h to obtain a uniform ceramic slurry; ④ Pour the uniformly ball-milled ceramic slurry obtained in ③ into a vacuum defoaming tank, add 0.3 wt.% of catalyst tetramethylethylenediamine and 0.3 wt.% of initiator ammonium persulfate based on the mass of the uniformly ball-milled ceramic slurry, defoam for 3 min with a rotary vacuum defoamer, and gently stir with a glass rod for 12 s to obtain a near-infrared ceramic slurry with a component Y, wherein the catalyst tetramethylethylenediamine is added in the form of an aqueous solution with a mass concentration of 75%, and the initiator ammonium persulfate is added in the form of an aqueous solution with a mass concentration of 95%; ⑤ Place the near-infrared ceramic slurry with component Y into a sealed container, and use the suction effect of the negative pressure fan to make the container in a micro-negative pressure environment; place the cured periodically arranged square grid skeleton ceramic in a sealed container so that it is completely infiltrated by the micro-negative pressure slurry with component Y and filled with microscopic gaps, move the periodically arranged square grid skeleton ceramic filled with Y slurry into a temperature and humidity control box, set the temperature to 50°C and the humidity to 70%, and let it stand and dry for 16 hours to obtain the square grid skeleton heterogeneous fluorescent ceramic blank.

[0044] (3) The periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank was placed in an alumina crucible, heated to 400 °C at a heating rate of 0.6 °C / min and kept at this temperature for 16 h, then heated to 850 °C at a heating rate of 2 °C / min and kept at this temperature for 9 h, and sintered in a muffle furnace to remove the organic matter in the blank. The sintered heterogeneous fluorescent ceramic blank was heated to 1550 °C at a heating rate of 0.5 °C / min in a nitrogen atmosphere or an argon atmosphere and kept at this temperature for 15 h. After the holding period, the blank was cooled to room temperature at a cooling rate of 0.8 °C / min to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

[0045] The thermal conductivity of the periodically arranged non-continuous truss structure heterogeneous fluorescent ceramic prepared in this embodiment is 275 Wm −1 K −1 ; Under the excitation of 450nm blue light LED, the luminous efficiency is as high as 230.4lm / W; under the excitation of 450nm blue light LD, the luminous efficiency is as high as 289.6lm / W.

[0046] When high thermal conductivity heterostructure near-infrared fluorescent ceramics and LEDs are packaged into NIR-LED devices and applied to grain detection, the emission spectrum covers a range of 700-1500nm. When the driving current is 180 mA, the photoelectric conversion efficiency is 30% and the correlation coefficient is 0.9990; when heterostructure near-infrared fluorescent ceramics and blue light LDs are packaged into NIR-LD devices and applied to grain detection, the emission spectrum covers a range of 700-1500nm.

[0047] Example 3 like Figure 1 As shown, a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic, the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic is a periodically arranged square grid skeleton heterogeneous fluorescent ceramic, the fluorescent ceramic includes a periodically arranged square grid skeleton ceramic and a near-infrared fluorescent ceramic filled in the gaps of the square grid skeleton ceramic, the square grid skeleton is printed by a gel slurry with a component of X, and the component of the near-infrared fluorescent ceramic is Y, wherein X is Al2O3 and AlN; Y is aluminosilicate, and the luminescence center is Cr 3+ 、Nd 3+ .

[0048] The basic unit of the periodically arranged square grid skeleton ceramic is composed of a first layer, a second layer, and a third layer of square grid skeleton ceramics. The areas of the first layer, the second layer, and the third layer of square grid skeleton ceramics are equal. The height of each layer of square grid skeleton ceramics, i.e., the layer height, is 100 μm, and the side length is 25 mm. The total height of the high thermal conductivity heterostructure near-infrared fluorescent ceramic is 30 mm.

[0049] The grids constituting the square grid skeleton ceramics are all squares, wherein the grid sides of the first layer of square grid skeleton ceramics 1 and the second layer of square grid skeleton ceramics 2 are equal in length and are both 200 μm, and the grid side length of the third layer of square grid skeleton ceramics 3 is 48%-52% of the grid side length of the first or second layer of square grid skeleton ceramics, i.e., about 100 μm, and the width h is 30 μm.

[0050] Other implementations are the same as in Example 1.

[0051] The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic for LED / laser lighting in this embodiment comprises the following steps: (1) Using photocuring 3D printing technology combined with gel technology to prepare ceramic green body: Print the gel slurry with component X into a periodically arranged square grid skeleton ceramic. The specific steps are as follows: ① Pre-dry the powder X, then place the powder X, surfactant ammonium oxide OA and anhydrous ethanol in a ball mill, and mill for 3 h at a rotation speed of 220 r / min to prepare a suspension, wherein the powder X is at least one of Al2O3 and AlN, with a particle size of 30 μm, the grinding balls are high-purity alumina balls, the mass of surfactant ammonium oxide OA is 1 / 100 of the mass of the powder X, and the mass of anhydrous ethanol is 2.5 times the mass of the powder X; use a rotary evaporator at a heating temperature of 60°C to remove the anhydrous ethanol in the suspension, and then place it in an oven for heat treatment at 90°C for 5.5 h; after cooling to room temperature, grind the obtained powder and pass it through a 150-mesh sieve to obtain the modified powder X; ② Add pentaerythritol tetraacrylate, 1-6-hexanediol diacrylate, polyurethane acrylate, n-octanol and polyethylene glycol to deionized water to prepare a premix, wherein the concentration of pentaerythritol tetraacrylate is 19wt%, the concentration of 1-6-hexanediol diacrylate is 26wt%, the concentration of polyurethane acrylate is 19wt%, the concentration of n-octanol is 20wt%, and the concentration of polyethylene glycol is 16wt%. Add the modified powder X prepared in ① and the dispersant BYK 9077 accounting for 2 wt% of the mass of the powder X to the premix, and ball mill for 11 h at a rotation speed of 320 r / min to prepare a square grid skeleton ceramic slurry with a solid content of 52vol%; ③ Add 1wt% of the photoinitiator Irgacure 819 to the square grid skeleton ceramic slurry, ball mill for 12 min at a rotation speed of 320r / min, and then place it in the material tank of the DLP 3D printer; ④Set the printing parameters to layer thickness of 10 μm, single layer curing time of 3 s, and exposure energy density of 31.5 mj / cm 2, using Solidworks software to build a three-dimensional model of the square grid skeleton structure of the first layer, and importing it into the printer through CeraRay software, preparing the square grid skeleton ceramic body of the first layer by cumulative printing layer by layer, and performing UV irradiation photocuring throughout the process to obtain the square grid skeleton ceramic body of the first layer; ⑤Put the first layer of square grid skeleton ceramic body back on the workbench of the 3D printer, use Solidworks software to build a three-dimensional model of the second layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the second layer of square grid skeleton ceramic body by cumulative printing layer by layer on the basis of the first layer, and perform UV irradiation photocuring throughout the process to obtain a double-layer square grid skeleton ceramic body, wherein the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap of the two is achieved; ⑥Put the double-layer square grid skeleton structure ceramic body back on the workbench of the 3D printer, use Solidworks software to establish a three-dimensional model of the third layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the third layer of square grid skeleton structure ceramic body by cumulative printing layer by layer on the square grid skeleton structure ceramic body, and perform UV irradiation photocuring throughout the process, and finally obtain a cured three-layer square grid skeleton ceramic, wherein the grid side length of the third layer of square grid skeleton ceramic is 48%-52% of the first or second layer, that is, about 100 μm, and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked, and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved; ⑦ Place the three-layer square grid skeleton ceramics back on the workbench of the 3D printer, and repeat steps ④-⑥ 100 times until a periodically arranged square grid skeleton ceramic with a total height of 30 mm is obtained.

[0052] (2) Introducing a near-infrared fluorescent ceramic slurry with a component of Y into the microscopic voids of the square grid skeleton ceramic obtained in (1), and constructing a periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank after the gel is cured; the method is as follows: ① Add dispersant ammonium citrate and pH regulator tetramethylammonium hydroxide to deionized water to prepare a premixed solution; wherein the concentration of dispersant ammonium citrate is 0.6wt%, and the concentration of pH regulator tetramethylammonium hydroxide is 1.2wt%; ②Pre-dry the powder Y of the near-infrared fluorescent ceramic component, add the powder Y into the premixed liquid in 6 times, and use an alumina ball mill to grind at a low speed of 80 r / min. The powder Y is aluminosilicate, and the luminescence center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+ at least one of the following: the particle size of powder Y is 150 nm, the grinding balls are high-purity alumina balls, and the mass ratio of powder Y to grinding balls is 1:2; after all powder Y is added to the premixed liquid, ball milling is performed for 11 h to obtain a ceramic slurry with a solid content of 52 vol%; wherein powder Y is added to the premixed liquid for ball milling in 6 times, the amount added in the 1st to 2nd times is 15% of the mass of powder Y, the amount added in the 3rd to 4th times is 35% of the mass of powder Y, and the amount added in the 5th to 6th times is 50% of the mass of powder Y; ③ Add 2 wt% of monomer acrylamide AM and crosslinking agent N,N'-methylenebisacrylamide to the ceramic slurry obtained in ②, the mass ratio of AM to N,N'-methylenebisacrylamide is 1 / 13, and continue ball milling for 5 h to obtain a uniform ceramic slurry; ④ Pour the uniformly ball-milled ceramic slurry obtained in ③ into a vacuum defoaming tank, and add 0.2wt.% of catalyst tetramethylethylenediamine and 0.25wt.% of initiator ammonium persulfate based on the mass of the uniformly ball-milled ceramic slurry, defoam for 3 min with a rotary vacuum defoamer, and gently stir with a glass rod for 11s to obtain a near-infrared ceramic slurry with a component Y, wherein the catalyst tetramethylethylenediamine is added in the form of an aqueous solution with a mass concentration of 75%, and the initiator ammonium persulfate is added in the form of an aqueous solution with a mass concentration of 95%; ⑤ Place the near-infrared ceramic slurry with component Y into a sealed container, and make the container in a micro-negative pressure environment by utilizing the suction effect of the negative pressure fan; place the solidified periodically arranged square grid skeleton ceramic in a sealed container so that it is completely infiltrated by the micro-negative pressure slurry with component Y and filled with microscopic gaps, move the periodically arranged square grid skeleton ceramic filled with Y slurry into a temperature and humidity control box, set the temperature to 45°C and the humidity to 65%, and let it stand and dry for 14 hours to obtain the square grid skeleton heterogeneous fluorescent ceramic blank.

[0053] (3) The periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank was placed in an alumina crucible, heated to 390 °C at a heating rate of 0.6 °C / min and kept at this temperature for 14 h, then heated to 800 °C at a heating rate of 2 °C / min and kept at this temperature for 8 h, and sintered in a muffle furnace to remove organic matter from the blank. The sintered heterogeneous fluorescent ceramic blank was heated to 1525 °C at a heating rate of 0.4 °C / min in a nitrogen atmosphere or an argon atmosphere and kept at this temperature for 12 h. After the end of the keeping temperature, the temperature was cooled to room temperature at a cooling rate of 0.7 °C / min to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

[0054] The thermal conductivity of the periodically arranged square grid skeleton structure heterogeneous fluorescent ceramic prepared in this embodiment is 132.1 Wm −1 K −1 , under the excitation of 450nm blue light LED, the luminous efficiency is as high as 220.7lm / W; under the excitation of 450nm blue light LD, the luminous efficiency is as high as 279.4lm / W.

[0055] When the high thermal conductivity heterostructure near-infrared fluorescent ceramics and LED are packaged into NIR-LED devices and applied to grain detection, the emission spectrum covers a range of 700-1500nm. When the driving current is 180 mA, the photoelectric conversion efficiency is 24.6% and the correlation coefficient is 0.9896; when the heterostructure near-infrared fluorescent ceramics and blue light LD are packaged into NIR-LD devices and applied to grain detection, the emission spectrum covers a range of 700-1500nm.

[0056] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A high thermal conductivity heterostructure near-infrared fluorescent ceramic, It is characterized in that The high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic is a periodically arranged square grid skeleton heterogeneous fluorescent ceramic, the fluorescent ceramic includes a periodically arranged square grid skeleton ceramic and a near-infrared fluorescent ceramic filled in the gaps of the square grid skeleton ceramic, the square grid skeleton is printed by a gel slurry with a component of X, and the component of the near-infrared fluorescent ceramic is Y, wherein X is Al 2 O 3 , AlN; Y is aluminosilicate, and the luminescent center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+ At least one of; The basic unit of the periodically arranged square grid skeleton ceramic is composed of a first layer, a second layer, and a third layer of square grid skeleton ceramics arranged in sequence from bottom to top, the layer heights of the square grid skeleton ceramics are all equal to 50 μm-150 μm, the side lengths of the square grid skeleton ceramics are all equal to 20-30 mm, and the total height of the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic, i.e., the periodically arranged square grid skeleton heterogeneous fluorescent ceramic, is 1.5-45 mm; The grids constituting the square grid skeleton ceramics are square, the grid sides of the first layer of square grid skeleton ceramics and the second layer of square grid skeleton ceramics are equal in length and are both 100 μm-300 μm, the grid side length of the third layer of square grid skeleton ceramics is 48%-52% of the grid side length of the first layer or the second layer of square grid skeleton ceramics; the grid widths h of the first layer, the second layer, and the third layer of square grid skeleton ceramics are equal and are 20 μm-40 μm; The second layer of square grid skeleton ceramic is arranged on the first layer of square grid skeleton ceramic and the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap between the two is achieved. The third layer of square grid skeleton ceramic is arranged on the second layer of square grid skeleton ceramic and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved.

2. The high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 1, It is characterized in that The periodically arranged square grid skeleton heterogeneous fluorescent ceramic is repeated with three layers of square grid skeleton ceramics formed by the first layer, the second layer and the third layer of square grid skeleton ceramics as a basic unit, and the number of repetitions is determined by the height of the high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic finally obtained.

3. The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 1 or 2, It is characterized in that The photocuring 3D printing technology combined with the gel technology is used to construct a periodically arranged square grid skeleton heterogeneous fluorescent ceramic, including the following steps: (1) Using photocuring 3D printing technology combined with gel technology to prepare ceramic blanks: printing a gel slurry with a component X into a periodically arranged square grid skeleton ceramic, introducing a near-infrared fluorescent ceramic slurry with a component Y into the microscopic gaps of the square grid skeleton ceramic, and constructing a periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank; (2) The periodically arranged square grid skeleton heterogeneous fluorescent ceramic blank is fired and then sintered at high temperature to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

4. The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 3, It is characterized in that The method of printing the gel slurry with component X into a periodically arranged square grid skeleton ceramic in step (1) is as follows: ① Pre-dry the powder X, then place the powder X, surfactant ammonium oxide OA and anhydrous ethanol in a ball mill, and mill for 2-4 h at a speed of 200-250 r / min to prepare a suspension, wherein the powder X is Al 2 O 3 , AlN, with a particle size of 10-50 μm, the grinding ball is a high-purity alumina ball, the mass of the surfactant ammonium oxide OA is 1 / 90-1 / 110 of the mass of the powder X, and the mass of the anhydrous ethanol is 2-3 times the mass of the powder X; the anhydrous ethanol in the suspension is removed by a rotary evaporator at a heating temperature of 50-70°C, and then placed in an oven for heat treatment at 80°C-100°C for 5h-6h; after cooling to room temperature, the obtained powder is ground and passed through a 100-200 mesh sieve to obtain the modified powder X; ② Add pentaerythritol tetraacrylate, 1-6-hexanediol diacrylate, polyurethane acrylate, n-octanol, and polyethylene glycol to deionized water to prepare a premix, wherein the concentration of pentaerythritol tetraacrylate is 18-20 wt%, the concentration of 1-6-hexanediol diacrylate is 24-26 wt%, the concentration of polyurethane acrylate is 18-20 wt%, the concentration of n-octanol is 18-20 wt%, and the concentration of polyethylene glycol is 14-16 wt%. The modified powder X prepared in ① and 2 wt% of the mass of the powder X dispersant BYK 9077 are added to the premix, and the mixture is ball-milled at a rotation speed of 300-350 r / min for 10-12 h to prepare a square grid skeleton ceramic slurry with a solid content of 50 vol%-55 vol%; ③ Add 0.5-1.5 wt % of the photoinitiator Irgacure 819 to the square grid skeleton ceramic slurry, ball mill for 10-15 min at a rotation speed of 300-350 r / min, and then place it in the material tank of the DLP 3D printer; ④Set the printing parameters to layer thickness of 10 μm, single layer curing time of 3 s, and exposure energy density of 31.5 mj / cm 2 , using Solidworks software to build a three-dimensional model of the square grid skeleton structure of the first layer, and importing it into the printer through CeraRay software, preparing the square grid skeleton ceramic body of the first layer by cumulative printing layer by layer, and performing UV irradiation photocuring throughout the process to obtain the square grid skeleton ceramic body of the first layer; ⑤Put the first layer of square grid skeleton ceramic body back on the workbench of the 3D printer, use Solidworks software to build a three-dimensional model of the second layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the second layer of square grid skeleton ceramic body by cumulative printing layer by layer on the basis of the first layer, and perform UV irradiation photocuring throughout the process to obtain a double-layer square grid skeleton ceramic body, wherein the grid intersection of the second layer of square grid skeleton ceramic is located at the center of the grid gap of the first layer of square grid skeleton ceramic and the maximum area overlap of the two is achieved; ⑥Put the double-layer square grid skeleton structure ceramic body back on the workbench of the 3D printer, use Solidworks software to establish a three-dimensional model of the third layer of square grid skeleton structure ceramic, import it into the printer through CeraRay software, prepare the third layer of square grid skeleton structure ceramic body by cumulative printing layer by layer on the square grid skeleton structure ceramic body, and perform UV irradiation photocuring throughout the process, and finally obtain a cured three-layer square grid skeleton ceramic, wherein the grid side length of the third layer of square grid skeleton ceramic is 48%-52% of the first layer or the second layer, and the grid intersection of the third layer of square grid skeleton ceramic is located at the center of the gap after the first layer of square grid skeleton ceramic and the second layer of square grid skeleton ceramic are stacked, and the maximum area overlap with the second layer of square grid skeleton ceramic is achieved; ⑦ Place the three layers of square grid skeleton ceramics back on the workbench of the 3D printer, and repeat steps ④-⑥ until a periodically arranged square grid skeleton ceramic of the desired height is obtained.

5. The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 3, It is characterized in that The method of constructing a square grid skeleton heterogeneous fluorescent ceramic blank by introducing a near-infrared fluorescent ceramic slurry with a component Y into the microscopic gaps of the square grid skeleton in step (1) is as follows: placing the near-infrared ceramic slurry with a component Y into a sealed container, and making the container in a micro-negative pressure environment by using the suction effect of a negative pressure fan; placing the solidified periodically arranged square grid skeleton ceramic in a sealed container, so that it is completely infiltrated by the micro-negative pressure slurry with a component Y and fills the microscopic gaps; moving the periodically arranged square grid skeleton ceramic filled with the Y slurry into a temperature and humidity control box, setting the temperature to 40°C-50°C and the humidity to 60%-70%, and standing to dry for 12-16 hours to obtain a square grid skeleton heterogeneous fluorescent ceramic blank.

6. The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 5, It is characterized in that The preparation method of the near-infrared fluorescent ceramic slurry with component Y is as follows: ① Adding dispersant ammonium citrate and pH regulator tetramethylammonium hydroxide to deionized water to prepare a premixed solution; wherein the concentration of the dispersant ammonium citrate is 0.5 wt%-0.8 wt%, and the concentration of the pH regulator tetramethylammonium hydroxide is 1.0 wt%-1.5 wt%; ②Pre-dry the component powder Y of the near-infrared fluorescent ceramic, add the powder Y into the premixed liquid in 5-6 times, and use an alumina ball mill to grind at a low speed of 60-100 r / min. The powder Y is aluminosilicate, and the luminescence center is Cr 3+ And contains Ce 3+ , Yb 3+ , Nd 3+ at least one of the following: the particle size of powder Y is 100-200 nm, the grinding balls are high-purity alumina balls, and the mass ratio of powder Y to grinding balls is 1:2; after all powder Y is added to the premixed liquid, ball milling is performed for 10-12 h to obtain a ceramic slurry with a solid content of 55 vol%-60vol%; wherein powder Y is added to the premixed liquid for ball milling in 5-6 times, the amount added in the 1st to 2nd time is 10%-20% of the mass of powder Y, the amount added in the 3rd to 4th time is 30-40% of the mass of powder Y, and the amount added in the 5th to 6th time is 40%-60% of the mass of powder Y; ③ Add 1-3 wt% of monomer acrylamide AM and crosslinking agent N,N'-methylenebisacrylamide to the ceramic slurry obtained in ②, the mass ratio of AM to N,N'-methylenebisacrylamide is 1 / 12-1 / 14, and continue ball milling for 4-6 h to obtain a uniform ceramic slurry; ④ Pour the uniformly ball-milled ceramic slurry obtained in ③ into a vacuum defoaming tank. Based on the mass of the uniformly ball-milled ceramic slurry, add 0.1-0.3 wt.% of catalyst tetramethylethylenediamine and 0.2-0.3 wt.% of initiator ammonium persulfate. Defoam for 3 min using a rotary vacuum defoamer, and gently stir with a glass rod for 10-12 s to obtain a near-infrared ceramic slurry with a component Y, wherein the catalyst tetramethylethylenediamine is added in the form of an aqueous solution with a mass concentration of 75%, and the initiator ammonium persulfate is added in the form of an aqueous solution with a mass concentration of 95%.

7. The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 3, It is characterized in that The specific operation of bisque firing in step (2) is as follows: placing the heterogeneous fluorescent ceramic bisque blank in an alumina crucible, heating the blank to 380°C-400°C at a heating rate of 0.5-0.6°C / min and keeping the temperature for 12 h-16 h, heating the blank to 750°C-850°C at a heating rate of 1-2°C / min and keeping the temperature for 7 h-9 h, and bisque firing the blank in a muffle furnace to discharge organic matter from the blank.

8. The method for preparing the high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 3, It is characterized in that The operation of high temperature sintering in step (2) is as follows: the bisque-fired heterogeneous fluorescent ceramic blank is heated to 1500°C-1550°C in a nitrogen atmosphere or an argon atmosphere at a heating rate of 0.3°C / min-0.5°C / min and kept at this temperature for 10-15 h. After the heat preservation, the temperature is cooled to room temperature at a cooling rate of 0.6°C / min-0.8°C / min to obtain a high thermal conductivity heterogeneous structure near-infrared fluorescent ceramic.

9. The high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 1 or 2 is used in the field of fluorescence conversion lighting and near-infrared light display. Features: When high thermal conductivity heterostructure near-infrared fluorescent ceramics are used in lighting and near-infrared light display devices, the excitation source is a blue laser or a blue LED chip, and the thermal conductivity of high thermal conductivity heterostructure near-infrared fluorescent ceramics is 20-275 Wm −1 K −1 , the luminous efficiency is 200-290lm / W.

10. The high thermal conductivity heterostructure near-infrared fluorescent ceramic according to claim 1 is used in the field of near-infrared grain detection. Features: When high thermal conductivity heterostructure near-infrared fluorescent ceramics are applied to NIR-LED / LD devices, the wavelength range is 700-1500nm, the photoelectric conversion efficiency is 20%-30%, and the correlation coefficient is 0.9870-0.9990.

Citation Information

Patent Citations

  • Light source refraction ceramic support and processing technology

    CN113050228A

  • Fluorescent sheet heat dissipation integrated packaging method for LED light source

    CN114530439A

  • Ceramic core with composite structure and preparation method thereof

    CN115519074A

  • High-thermal-conductivity high-mechanical-property multilayer composite structure ceramic and preparation method thereof

    CN117585988A

  • Composite structure fluorescent ceramic capable of regulating and controlling photo-thermal performance as well as preparation method and application of composite structure fluorescent ceramic

    CN118206369A