Thermal post-crosslinking agent for polyimide as well as preparation method and application of thermal post-crosslinking agent
By using the isocyanate technology of crosslinking after heating in polyimide, the problems of poor solubility and poor fluidity of traditional crosslinking agents during processing are solved, and the preparation of high-performance polyimide films is realized, with excellent pulling Extension and processability.
Patent Information
- Application Number
- CN202411114374.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-06
AI Technical Summary
The crosslinking agent of traditional polyimide has problems such as poor solubility, high viscosity and poor flow performance during processing. It is difficult to apply in high-pressure and high-stress environments, and it is difficult to realize high-performance polyimide films.
A thermal crosslinking agent for polyimide is used. The crosslinking agent has no crosslinking ability before heating, but can be converted into isocyanate after heating, and is used for crosslinking to prepare polyimide films. Through Curtius rearrangement reaction Cross-linking is performed after heating to ensure strong processability and excellent performance.
The high-performance processing of polyimide films is achieved, with a breaking strength of 164.03MPa and an elongation of breaking reaching 9.8%, solving the problem of difficult processing of traditional crosslinking agents and improving the performance of polyimide.
Smart Images

Figure CN119080636A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic crosslinking agents, and in particular relates to a thermal post-crosslinking agent for polyimide and a preparation method and application thereof. Background Art
[0002] Polyimide (PI) is a widely used special engineering plastic. It contains a large number of imide ring structures in the main chain and is one of the organic polymer materials with the best comprehensive performance. Due to its excellent heat resistance, mechanical properties, dimensional stability and chemical corrosion resistance, it is widely used in integrated electrical appliances, communication substrates and flexible displays.
[0003] However, the traditional cross-linking agent for preparing polyimide, such as isocyanate, has a fast cross-linking speed, resulting in poor solubility, high viscosity, and poor flow properties of the obtained polyimide, which affects the processing technology and performance. In addition, the modulus of polyimide prepared by traditional cross-linking agents is generally 1.5-3.0GPа, the tensile strength is 70-100MPa, and the elongation at break is 2-15%, which is difficult to be used in some extreme environments with high pressure and high stress. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a thermal post-crosslinking agent for polyimide and a preparation method and application thereof. The crosslinking agent has no crosslinking ability before heating, but can be converted into isocyanate after heating, and isocyanate can be cross-linked to prepare polyimide, so that good fluidity can be ensured before heating, and the processability is strong, and the processing technology of polyimide can be improved. When used, the thermal post-crosslinking agent is first mixed with the prepolymer for film coating, and after the film coating is completed, the acyl azide is converted into isocyanate by heating for cross-linking to prepare a polyimide film, which not only solves the problem of difficult processing of polyimide film, but also completes the crosslinking of polyimide, so that the performance of polyimide is improved.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A thermal post-crosslinking agent for polyimide, wherein the structural formula of the thermal post-crosslinking agent is:
[0007]
[0008] One of the methods for preparing the thermal post-crosslinking agent for polyimide provided by the present invention comprises the following steps:
[0009] (1) Under the protection of inert gas, phloroglucinol, p-fluorobenzonitrile and carbonate are dissolved in an organic solvent, stirred at 145-155° C. for 1.5-2.5 hours, then heated to 175-185° C. for 15-18 hours, and subjected to post-treatment to obtain 1,3,5-tris(4-carboxyphenoxy)benzene;
[0010] (2) Under an ice bath, 1,3,5-tris(4-carboxyphenoxy)benzene is dissolved in an organic solvent, and then triethylamine and diphenylphosphoryl azide are added. The mixture is stirred at room temperature for 1.5 to 2.5 hours, and after post-treatment, 1,3,5-tris(4-acylazidophenoxy)benzene is obtained.
[0011] Furthermore, in step (1), the molar ratio of phloroglucinol, p-fluorobenzonitrile and carbonate is 1:3.1-3.2:4.5-5.5; and the carbonate is any one of sodium carbonate and potassium carbonate.
[0012] In step (1), the organic solvent is a mixed solvent of N-methyl-2-pyrrolidone and toluene in a volume ratio of 1:1; and the concentration of phloroglucinol in the organic solvent is 0.20 to 0.30 mol / mL.
[0013] In step (1), the post-treatment method is: cooling the reaction solution to room temperature, adding water and hydrochloric acid to acidify to produce a precipitate, then filtering, adding the collected precipitate to a mixed solution of distilled water and ethanol, and adding sodium hydroxide, reflux the mixed solution overnight, and then distilling under reduced pressure to remove ethanol, cooling the mixture to room temperature, adding distilled water, acidifying with concentrated hydrochloric acid aqueous solution to pH <7, then filtering, collecting the precipitate, recrystallizing with a mixed solution of ethanol and water in a volume ratio of 1:1, collecting the recrystallized product, and drying.
[0014] In step (2), the usage ratio of 1,3,5-tris(4-carboxyphenoxy)benzene, triethylamine and diphenylphosphoryl azide is 0.5-0.7 g: 1-1.1 mL: 1-1.5 g.
[0015] In step (2), the organic solvent is tetrahydrofuran.
[0016] In step (2), the post-treatment method is: after concentrating the reaction solution, purifying it by column chromatography with a mixture of petroleum ether and ethyl acetate in a volume ratio of 4:1, collecting the purified product, concentrating and drying it.
[0017] The second method for preparing the thermal post-crosslinking agent for polyimide provided by the present invention comprises the following steps:
[0018] (A) Under the protection of inert gas, phloroglucinol and potassium carbonate are dissolved in an organic solvent, and then 4-bromomethylbenzoate is added, and the mixture is stirred at 50-55° C. for 2-3 hours, and post-treated to obtain product A;
[0019] (B) hydrolyzing product A to obtain product B;
[0020] (C) In an ice bath, product B is dissolved in an organic solvent, and then triethylamine and diphenylphosphoryl azide are added, and the mixture is stirred at room temperature for 1.5 to 2.5 hours. After post-treatment, a thermal post-crosslinking agent is obtained.
[0021] Among them, the structural formula of product A is:
[0022] The structural formula of product B is:
[0023] Furthermore, in step (A), the molar ratio of phloroglucinol to 4-bromomethylbenzoate is 1:3-4; and the 4-bromomethylbenzoate is methyl 4-bromomethylbenzoate or ethyl 4-bromomethylbenzoate.
[0024] In step (A), the organic solvent is DMF; the post-treatment method is as follows: after the reaction solution is concentrated, column chromatography is performed for purification using a mixture of petroleum ether and ethyl acetate in a volume ratio of 3:1, and the purified product is collected, concentrated, and dried.
[0025] In step (B), the hydrolysis conditions are: using sodium hydroxide as a catalyst, methanol as a solvent, stirring the reaction at room temperature for 3 to 5 hours, and then distilling under reduced pressure.
[0026] In step (C), the usage ratio of product B, triethylamine and diphenylphosphoryl azide is 1.4-1.6 g: 1.5-1.7 mL: 2.5-3.0 g.
[0027] In step (C), the organic solvent is tetrahydrofuran; the post-treatment method is: after the reaction solution is concentrated, it is purified by column chromatography with a mixture of petroleum ether and ethyl acetate in a volume ratio of 4:1, and the purified product is collected, concentrated and dried.
[0028] The invention also provides application of the thermal post-crosslinking agent for polyimide in preparing a polyimide film.
[0029] The thermal post-crosslinking agent for polyimide provided by the present invention is an acyl azide compound synthesized with phloroglucinol as a raw material. Such compound has no crosslinking ability before heating, but can decompose isocyanate after heating, and isocyanate can be used as a crosslinking agent for preparing polyimide. In this way, since no crosslinking reaction occurs before heating, the good fluidity of the polyimide raw material can be ensured, the processability is strong, and the processing technology of the polyimide can be improved.
[0030] The thermal post-crosslinking agent for polyimide provided by the present invention reacts as follows after heating: When in use, the hot post-crosslinking agent is mixed with the prepolymer polyamic acid solution for preparing polyimide, and at this time, acyl azide will not crosslink with the prepolymer, so the mixed solution containing acyl azide and prepolymer has good fluidity and low viscosity, and is easy to apply film, avoiding the difficult processing characteristics caused by the crosslinked structure after crosslinking. Then, by heating the mixture of the two, the crosslinking agent containing acyl azide undergoes a thermal rearrangement reaction due to the Curtius rearrangement reaction, and is converted into a crosslinking agent containing an isocyanate group, and the isocyanate group can be polymerized with the polyimide at the amine end. In this way, the Curtius rearrangement reaction is used to heat post-crosslink the polyimide, and the film coating process of the polyimide is realized, avoiding the processing difficulty problem of first crosslinking and then film coating, and also improving the performance of the polyimide film by crosslinking.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The thermal post-crosslinking agent for polyimide provided by the present invention cleverly avoids the problem that cross-linked polyimide is difficult to coat, and successfully completes the thermal post-crosslinking of polyimide, thereby preparing a polyimide film with excellent performance, the breaking strength of which can reach 164.03MPa, the elongation at break reaches 9.8%, and the film has excellent tensile properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The synthetic route of thermal post-crosslinking agent I for polyimide is shown in FIG.
[0034] Figure 2 This is the hydrogen NMR spectrum of 1,3,5-tris(4-carboxyphenoxy)benzene;
[0035] Figure 3 is the hydrogen NMR spectrum of the thermal post-crosslinking agent I for polyimide;
[0036] Figure 4 The synthetic route of thermal post-crosslinking agent II for polyimide is shown;
[0037] Figure 5 is the hydrogen nuclear magnetic spectrum of the product A in the embodiment;
[0038] Figure 6 It is the hydrogen spectrum nuclear magnetic spectrum of the product B in the embodiment;
[0039] Figure 7 This is the H NMR spectrum of the thermal post-crosslinking agent II for polyimide;
[0040] Figure 8 This is a test of the mechanical properties of polyimide before and after cross-linking. DETAILED DESCRIPTION
[0041] The present invention is described in detail below with reference to the embodiments.
[0042] Example 1
[0043] A thermal post-crosslinking agent I for polyimide, having the structural formula:
[0044]
[0045] The synthetic route of the thermal post-crosslinking agent I for polyimide is as follows Figure 1 shown.
[0046] The preparation method of the thermal post-crosslinking agent I for polyimide comprises the following steps:
[0047] (1) Under the protection of nitrogen, dissolve phloroglucinol [0.63 g 5 mmol], p-fluorobenzonitrile [1.91 g 15.8 mmol], and potassium carbonate [3.11 g 22.5 mmol] in 10 mL In a mixture of N-methyl-2-pyrrolidone and 10 mL of toluene, stir and react at 150°C for 2 h, then heat to 180°C and continue stirring and reacting for 16 h, cool the reaction solution to room temperature, add 100 mL of water and 10 mL of 36.5% hydrochloric acid to acidify and produce a precipitate, then filter, add the collected precipitate to 50 mL of distilled water and 50 mL of ethanol, and add sodium hydroxide [13 g, 0.2 mol], reflux the mixture at 90°C overnight, and then distill under reduced pressure to remove ethanol. After the mixture is cooled to room temperature, add 100 mL of distilled water, acidify with 25 mL of 3.65% hydrochloric acid aqueous solution to pH <7, then filter, collect the precipitate, recrystallize with a mixed solution of ethanol and water in a volume ratio of 1:1, collect the recrystallized product, and dry to obtain a white powder, namely 1,3,5-tris(4-carboxyphenoxy)benzene, whose nuclear magnetic hydrogen spectrum is as follows Figure 2 As shown;
[0048] (2) In an ice bath at 0°C, 1,3,5-tris(4-carboxyphenoxy)benzene [0.6123 g 1.259 mmol] was dissolved in 10 mL of tetrahydrofuran, 1.03 mL of triethylamine was added, and the mixture was stirred for 10 min. 1.31 g 4.76 mmol] of diphenylphosphoryl azide (DPPA) was added, and the mixture was stirred at room temperature for 2 h. After the reaction solution was concentrated, column chromatography was performed using a mixed solution of petroleum ether:ethyl acetate = 4:1 by volume as an eluent. The purified product was collected, concentrated, and dried to obtain a white powder, 1,3,5-tris(4-acylazidophenoxy)benzene, whose H NMR spectrum was as follows: Figure 3 shown.
[0049] Example 2
[0050] A thermal post-crosslinking agent II for polyimide, having the structural formula:
[0051]
[0052] The synthetic route of the polyimide thermal post-crosslinking agent II is as follows Figure 4 shown.
[0053] The preparation method of the thermal post-crosslinking agent II for polyimide comprises the following steps:
[0054] (1) Under nitrogen protection, phloroglucinol [1.482 g 11.75 mmol] and potassium carbonate [16.2383 g 117.5 mmol] were dissolved in 60 mL DMF and stirred at 50° C. for 30 min. Then [10 g 41.135 mmol] 4-bromomethylbenzoate was dissolved in 30 mL DMF and then added dropwise to the reaction system. The mixture was stirred at 50° C. for 2 h. After the reaction, the reaction solution was concentrated and purified by a silica gel column. The eluent was a mixture of PE and EA in a volume ratio of 3:1. The purified product was collected, concentrated and dried to obtain product A, whose structural formula is Its H NMR spectrum is Figure 5 As shown;
[0055] (2) Dissolve 0.62 g of product A in 20 mL of methanol, then add 6.43 mL of 2 M sodium hydroxide solution, stir at room temperature for 4 h, and distill under reduced pressure to obtain product B, whose structural formula is Its H NMR spectrum is Figure 6 As shown;
[0056] (3) Under 0°C ice bath, product B [1.53 g 2.895 mmol] was dissolved in 20 mL tetrahydrofuran, 1.61 mL triethylamine was added, and the mixture was stirred for 10 min to dissolve, and 2.7883 g 10.132 mmol] diphenylphosphoryl azide (DPPA) was added, and the mixture was stirred at room temperature for 2 h. After the reaction solution was concentrated, column chromatography was performed using a mixed solution of petroleum ether:ethyl acetate = 4:1 as an eluent, and the purified product was collected, concentrated and dried to obtain a white powder, thereby obtaining a thermal post-crosslinking agent for polyimide, and its H NMR spectrum was as follows: Figure 7 shown.
[0057] Application Examples
[0058] The polyimide prepared in the above embodiment is applied to the preparation of polyimide film using a thermal post-crosslinking agent.
[0059] The preparation method of the polyamic acid solution with a solid content of 20% in each embodiment and comparative example is as follows: in a 1L three-necked flask, 64.046g of 2,2'-bis(trifluoromethyl)diaminobiphenyl was added, and 625mL of anhydrous DMAC solvent was added under nitrogen. After stirring and dissolving, 61.42g of 4,4'-oxydiphthalic anhydride was added in three batches. After the viscosity reached 8000mpa.s, stirring was stopped to obtain a polyamic acid solution with a solid content of 20% for standby use.
[0060] Application Example 1
[0061] To 100 g of a polyamic acid solution having a solid content of 20%, 20 mg of the thermal post-crosslinking agent for polyimide prepared in Example 1 was added, and after all dissolved, it was coated on a coating machine to obtain a polyamic acid coating, and then placed in an 80° C. oven and heated to 300° C. at a heating rate of 40° C. per hour for 5 min, the heating was directly turned off, and after cooling, it was placed in water, and the film was automatically taken off to obtain a polyimide film.
[0062] Application Example 2
[0063] To 100 g of a polyamic acid solution having a solid content of 20%, 20 mg of the thermal post-crosslinking agent for polyimide prepared in Example 2 was added, and after all dissolved, it was coated on a coating machine to obtain a polyamic acid coating, and then placed in an 80° C. oven and heated to 300° C. at a heating rate of 40° C. per hour for 5 min, the heating was directly turned off, and after cooling, it was placed in water, and the film was automatically taken off to obtain a polyimide film.
[0064] Application Comparative Example 1
[0065] 100g of a polyamic acid solution with a solid content of 20% was coated on a coater to obtain a polyamic acid coating, and then placed in an 80°C oven and heated to 300°C at a heating rate of 40°C per hour for 5 minutes. The heating was directly turned off, and after cooling, it was placed in water and the film was automatically taken off to obtain a polyimide film.
[0066] Application Comparative Example 2
[0067] 20 mg of 1,3,5-tri(4-aminophenoxy)benzene was added to 100 g of a polyamic acid solution with a solid content of 20%. After stirring, a gel effect occurred, the viscosity increased, and it was difficult to process into a film. Therefore, no subsequent film was pushed to form a coating.
[0068] Application Comparative Example 3
[0069] To 100g of a polyamic acid solution with a solid content of 20%, 20mg of triphenylmethane triisocyanate crosslinking agent was added. After all the solution was dissolved, the solution was coated on a coating machine to obtain a polyamic acid coating. The solution was then placed in an 80°C oven and heated to 300°C at a heating rate of 40°C per hour for 5 minutes. The heating was directly turned off. After cooling, the solution was placed in water and the film was automatically removed to obtain a polyimide film.
[0070] The elongation at break and the breaking strength of the polyimide film obtained in each application example were tested. The test conditions for the stretching speed and the elongation at break were: the stretching speed was 50 mm / min, and the marking line spacing was 100 mm.
[0071] The test results are shown in Table 1.
[0072] Table 1
[0073]
[0074] The above-mentioned detailed description of a thermal post-crosslinking agent for polyimide and its preparation method and application with reference to the embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A thermal post-crosslinking agent for polyimide, characterized in that: The structural formula of the thermal post-crosslinking agent is:
2. The method for preparing a thermal post-crosslinking agent for polyimide according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Under the protection of inert gas, phloroglucinol, p-fluorobenzonitrile and carbonate are dissolved in an organic solvent, stirred at 145-155° C. for 1.5-2.5 hours, then heated to 175-185° C. for 15-18 hours, and subjected to post-treatment to obtain 1,3,5-tris(4-carboxyphenoxy)benzene; (2) Under an ice bath, 1,3,5-tris(4-carboxyphenoxy)benzene is dissolved in an organic solvent, and then triethylamine and diphenylphosphoryl azide are added. The mixture is stirred at room temperature for 1.5 to 2.5 hours, and after post-treatment, 1,3,5-tris(4-acylazidophenoxy)benzene is obtained.
3. The preparation method according to claim 2, characterized in that: In step (1), the molar ratio of phloroglucinol, p-fluorobenzonitrile and carbonate is 1:3.1-3.2:4.5-5.5; the carbonate is any one of sodium carbonate and potassium carbonate.
4. The preparation method according to claim 2, characterized in that: In step (1), the organic solvent is a mixed solvent of N-methyl-2-pyrrolidone and toluene in a volume ratio of 1:1; and the concentration of phloroglucinol in the organic solvent is 0.20 to 0.30 mol / mL.
5. The preparation method according to claim 2, characterized in that: In step (2), the usage ratio of 1,3,5-tri(4-carboxyphenoxy)benzene, triethylamine and diphenylphosphoryl azide is 0.5-0.7 g: 1-1.1 mL: 1-1.5 g.
6. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (A) Under the protection of inert gas, phloroglucinol and potassium carbonate are dissolved in an organic solvent, and then 4-bromomethylbenzoate is added, and the mixture is stirred at 50-55° C. for 2-3 hours, and post-treated to obtain product A; (B) hydrolyzing product A to obtain product B; (C) In an ice bath, product B is dissolved in triethylamine, and then diphenylphosphoryl azide is added. The mixture is stirred at room temperature for 1.5 to 2.5 hours, and a thermal post-crosslinking agent is obtained after post-treatment.
7. The preparation method according to claim 6, characterized in that: In step (A), the molar ratio of phloroglucinol to 4-bromomethylbenzoate is 1:3-4; the 4-bromomethylbenzoate is methyl 4-bromomethylbenzoate or ethyl 4-bromomethylbenzoate.
8. The preparation method according to claim 6, characterized in that: In step (B), the hydrolysis conditions are: using sodium hydroxide as a catalyst, methanol as a solvent, and stirring the reaction at room temperature for 3 to 5 hours.
9. The preparation method according to claim 6, characterized in that: In step (C), the usage ratio of product B, triethylamine and diphenylphosphoryl azide is 1.4-1.6 g: 1.5-1.7 mL: 2.5-3.0 g.
10. Use of the thermal post-crosslinking agent for polyimide according to claim 1 in preparing a polyimide film.