Thermosetting shape memory polymer, composite material and preparation method and application thereof

Through the development of thermoset shape memory polymers and composite materials, the production problems of complex components in traditional manufacturing technology have been solved, and efficient and fast mold design has been achieved, which meets the deformation needs of complex components in large cavitys, and has high thermal stability and shape memory performance.

CN119081019AActive Publication Date: 2024-12-06GUANGZHOU HUANXIANG INTELLIGENT TRANSFORMATION TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411200027.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Traditional manufacturing technology is difficult to achieve efficient and fast production of complex components, especially in the mold design and production of large cavity complex components. The deformation of smart materials is insufficient and it is difficult to meet the deformation needs.

Method used

A thermoset shape memory polymer and composite material was developed, which was heat-cured by a mixture of styrene, acrylate monomer, free radical initiator and polyethylene glycol diacrylate, combined with elastomeric fiber material to form high thermal stability Composite materials with sexual and shape memory properties, suitable for smart core mold field.

Benefits of technology

The material can effectively remember the initial shape at high temperature (above 200℃), with a shape recovery and fixation rate of up to 99%. It also inhibits crack propagation through elastic fibers, improves deformation ability, and meets the molding needs of large cavity complex components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081019A_ABST
    Figure CN119081019A_ABST
Patent Text Reader

Abstract

The invention relates to a thermosetting shape memory polymer, a composite material and a preparation method and application of the thermosetting shape memory polymer and the composite material, and belongs to the technical field of shape memory materials, and the thermosetting shape memory polymer is obtained by thermocuring a mixture containing styrene, an acrylate monomer, a free radical initiator and polyethylene glycol diacrylate. The thermosetting shape memory polymer provided by the invention has excellent thermal stability and shape memory performance, and can still memorize an initial shape at a relatively high temperature, and the shape recovery rate and the fixation rate can reach 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of shape memory materials, and in particular to a thermosetting shape memory polymer, a composite material, and a preparation method and application thereof. Background Art

[0002] In the manufacturing industry, molds are important tools for component molding and have an irreplaceable and important position. With the technological changes in manufacturing engineering, higher requirements are placed on the design and production of complex components. Traditional manufacturing technology has problems such as difficulty in demoulding, complex design, and heavy mold weight. It is difficult to produce complex components with variable structures, variable curvatures, and variable cross-sections, which seriously restricts the development of complex components.

[0003] Shape memory polymer (SMP) is an emerging smart material with a unique shape memory effect. It can automatically return to its original shape under external stimulation and has broad application prospects. Combining the active deformation characteristics of SMP with the manufacturing of complex components to make shape memory smart molds will hopefully achieve active demoulding of complex components and promote efficient and fast production of complex components.

[0004] However, in the existing field of intelligent deformable core molds, the deformation of intelligent materials is limited, which makes it difficult to meet the deformation requirements of some large-cavity complex components for molds. Summary of the invention

[0005] In response to one or more technical problems existing in the prior art, the present invention provides a thermosetting shape memory polymer, a composite material, and a preparation method and application thereof. The thermosetting shape memory polymer provided by the present invention has excellent thermal stability and shape memory performance, and can still remember the initial shape at a higher temperature (above 200°C), and the shape recovery rate and fixation rate can reach 99%.

[0006] In a first aspect, the present invention provides a thermosetting shape memory polymer, wherein the thermosetting shape memory polymer is obtained by thermally curing a mixture comprising styrene, an acrylate monomer, a free radical initiator and polyethylene glycol diacrylate.

[0007] Preferably, in parts by weight, styrene is 20 to 90 parts, acrylate monomer is 10 to 80 parts, free radical initiator is 0.5 to 3 parts, and polyethylene glycol diacrylate is 0.5 to 10 parts.

[0008] Preferably, the acrylic acid ester monomers include but are not limited to one or more of methyl acrylate, butyl acrylate, methyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, and octadecyl acrylate;

[0009] The free radical initiator includes but is not limited to one or more of azobisisobutyronitrile, benzoyl peroxide, tert-butyryl peroxide, dibenzoyl peroxide, and azobisisoheptylnitrile; and / or

[0010] The number average molecular weight of polyethylene glycol diacrylate is 100-3,000.

[0011] In a second aspect, the present invention provides a thermosetting shape memory composite material, comprising the thermosetting shape memory polymer described in the first aspect and an elastic fiber material.

[0012] Preferably, the volume fraction of the elastic fiber material in the thermosetting shape memory composite material is not greater than 30%.

[0013] Preferably, the elastic fiber material is one or more of an elastic fiber layer and an elastic fiber fabric; preferably, the elastic fiber in the elastic fiber material is selected from one or more of spandex fiber, nylon fiber, polypropylene fiber, polyethylene fiber and polyurethane fiber.

[0014] The present invention provides in a third aspect a method for preparing the thermosetting shape memory composite material according to the second aspect, the preparation method comprising:

[0015] Mix styrene, acrylate monomers, free radical initiator, and polyethylene glycol diacrylate to obtain a premix;

[0016] The elastic fiber material is layered and mixed with the premix, and then thermally cured to obtain the thermosetting shape memory composite material.

[0017] Preferably, the laying angle of the elastic fibers in the elastic fiber material is -180° to 180°, preferably -45° to 45°.

[0018] Preferably, the thermal curing temperature is 60-120° C. and the time is 7-24 hours.

[0019] In a fourth aspect, the present invention provides an application of the thermosetting shape memory composite material described in the second aspect, which is used in the field of smart core molds.

[0020] Compared with the prior art, the present invention has at least the following beneficial effects:

[0021] The present invention uses styrene and acrylate monomers as polymerization monomers, and adjusts the flexibility of the molecular segments in the thermosetting shape memory polymer network through the rigid-flexible coupling molecular structure design, so that the thermosetting shape memory polymer has shape memory characteristics and large deformation ability. The polymerization monomers are polymerized under the action of free radical initiators and crosslinking agents to form a thermosetting shape memory polymer with a three-dimensional network molecular structure. Compared with thermoplastic or semi-interpenetrating network shape memory polymers, it has better thermal stability and shape memory performance, and can still remember the initial shape at higher temperatures (above 200°C), and the shape recovery rate and fixation rate can reach 99%.

[0022] The present invention obtains a thermosetting shape memory composite material by compounding a shape memory polymer matrix with an elastic fiber material, wherein the elastic fiber has good shape-conforming ability and can adapt to the deformation of the shape memory polymer matrix. Under the premise of not limiting the deformation ability of the shape memory polymer matrix, the expansion of cracks in the shape memory polymer matrix can be effectively suppressed, and the deformation ability of the composite material can be improved. The thermosetting shape memory composite material provided by the present invention has a high elongation at break, shape fixation rate and shape recovery rate at deformation temperature, and can meet the requirements of the core mold for the molding of large cavity complex components. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is a physical diagram of the large deformation recovery process of the thermosetting shape memory polymer provided in Example 1 of the present invention;

[0025] Figure 2 is a shape memory cycle curve of the thermosetting shape memory polymer provided in Example 1 of the present invention;

[0026] Figure 3 DMA curves of the shape memory polymers provided in Example 1, Example 2 and Comparative Example 1 of the present invention;

[0027] Figure 4 is a histogram of the limit strain of the shape memory polymer provided in Comparative Example 1, Example 1, Example 2 and Example 5 of the present invention at Tg-20°C;

[0028] Figure 5 is a thermogravimetric analysis curve of the shape memory polymer provided in Example 1, Example 2 and Comparative Example 1 of the present invention;

[0029] Figure 6 : are DSC test curves of the shape memory polymers provided in Examples 1, 3 and 4 of the present invention;

[0030] Figure 7 is a DMA curve of the thermosetting shape memory composite material provided in Example 5 of the present invention;

[0031] Figure 8 This is the shape memory cycle curve of the thermosetting shape memory composite material provided in Example 5 of the present invention. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] In a first aspect, the present invention provides a thermosetting shape memory polymer, wherein the thermosetting shape memory polymer is obtained by thermally curing a mixture comprising styrene, an acrylate monomer, a free radical initiator and polyethylene glycol diacrylate.

[0034] The present invention uses styrene and acrylate monomers as polymerization monomers, and adjusts the flexibility of the molecular segments in the thermosetting shape memory polymer network through the rigid-flexible coupling molecular structure design, so that the thermosetting shape memory polymer has shape memory characteristics and large deformation ability. The polymerization monomers are polymerized under the action of free radical initiators and crosslinking agents to form a thermosetting shape memory polymer with a three-dimensional network molecular structure. Compared with thermoplastic or semi-interpenetrating network shape memory polymers, it has better thermal stability and shape memory performance, and can still remember the initial shape at higher temperatures (above 200°C), and the shape recovery rate and fixation rate can reach 99%.

[0035] According to some preferred embodiments, in parts by weight, styrene is 20 to 90 parts (for example, 20, 30, 40, 50, 60, 70, 80 or 90 parts), the acrylate monomer is 10 to 80 parts (for example, 10, 20, 30, 40, 50, 60, 70 or 80 parts), the free radical initiator is 0.5 to 3 parts (for example, 0.5, 1, 1.5, 2, 2.5 or 3 parts), and polyethylene glycol diacrylate is 0.5 to 10 parts (for example, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 parts).

[0036] According to some preferred embodiments, the acrylic acid ester monomers include but are not limited to one or more of methyl acrylate, butyl acrylate, methyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, and octadecyl acrylate;

[0037] The free radical initiator includes but is not limited to one or more of azobisisobutyronitrile, benzoyl peroxide, tert-butyryl peroxide, dibenzoyl peroxide, and azobisisoheptylnitrile; and / or

[0038] The number average molecular weight of polyethylene glycol diacrylate is 100-3,000.

[0039] In a second aspect, the present invention provides a thermosetting shape memory composite material, comprising the thermosetting shape memory polymer described in the first aspect and an elastic fiber material.

[0040] The present invention obtains a thermosetting shape memory composite material by compounding a shape memory polymer matrix with an elastic fiber material, wherein the elastic fiber has good shape-conforming ability and can adapt to the deformation of the shape memory polymer matrix. Under the premise of not limiting the deformation ability of the shape memory polymer matrix, the expansion of cracks in the shape memory polymer matrix can be effectively suppressed, and the deformation ability of the composite material can be improved. The thermosetting shape memory composite material provided by the present invention has a high elongation at break, a shape fixation rate, and a shape recovery rate at the deformation temperature, and can meet the requirements of the core mold for the molding of large cavity complex components.

[0041] It should be noted that the optimum deformation temperature range of the thermosetting shape memory polymer and the thermosetting shape memory composite material of the present invention is Tg-30°C to Tg+30°C, wherein Tg is the glass transition temperature.

[0042] According to some preferred embodiments, the volume fraction of the elastic fiber material in the thermosetting shape memory composite material is no more than 30%.

[0043] The volume fraction of the elastic fiber material in the thermosetting shape memory composite material of the present invention should not be too large. The inventors have found that if the volume fraction of the elastic fiber material is too large, it will affect the continuity of the shape memory polymer matrix, thereby having a negative impact on the shape memory performance of the composite material, and even losing the shape memory performance.

[0044] According to some preferred embodiments, the elastic fiber material is one or more of an elastic fiber layer and an elastic fiber fabric; preferably, the elastic fiber in the elastic fiber material is selected from one or more of spandex fiber, nylon fiber, polypropylene fiber, polyethylene fiber, and polyurethane fiber.

[0045] The present invention provides in a third aspect a method for preparing the thermosetting shape memory composite material according to the second aspect, the preparation method comprising:

[0046] Mix styrene, acrylate monomers, free radical initiator, and polyethylene glycol diacrylate to obtain a premix;

[0047] The elastic fiber material is layered and mixed with the premix, and then thermally cured to obtain the thermosetting shape memory composite material.

[0048] The preparation method of the thermosetting shape memory composite material of the present invention is simple in process. The prepared thermosetting shape memory composite material has high elongation at break, shape fixation rate and shape recovery rate, can meet the use requirements of the deformable intelligent core mold, and is used for molding components with large cavity complex structures.

[0049] According to some preferred embodiments, the laying angle of the elastic fibers in the elastic fiber material is -180° to 180° (for example, it can be -180°, -150°, -120°, -90°, -60°, -30°, 0°, 30°, 60°, 90°, 120°, 150° or 180°), preferably -45° to 45° (for example, it can be -45°, -30°, 0°, 30° or 45°).

[0050] According to some preferred embodiments, the thermal curing temperature is 60-120°C (for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C), and the time is 7-24h (for example, 7h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h).

[0051] In a fourth aspect, the present invention provides an application of the thermosetting shape memory composite material described in the second aspect, which is used in the field of smart core molds.

[0052] The thermosetting shape memory composite material provided by the present invention has high elongation at break, shape fixation rate and shape recovery rate, can meet the use requirements of a deformable intelligent core mold, and is used for molding components with large cavity complex structures.

[0053] The molding methods of the smart core molded component made of the thermosetting shape memory composite material provided by the present invention include but are not limited to one or more of compression molding and blow molding.

[0054] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the examples. The present invention does not specifically limit the sources of the various reagents used in the examples and comparative examples, and they can be directly purchased or synthesized by themselves. The parts in the following examples and comparative examples of the present invention are parts by weight.

[0055] Example 1

[0056] A method for preparing a thermosetting shape memory polymer comprises: placing 80 parts of styrene, 20 parts of butyl acrylate, 3 parts of polyethylene glycol diacrylate 200, and 2 parts of benzoyl peroxide in a beaker, stirring for 30 minutes, ensuring uniform mixing, and obtaining a premix. Applying a release agent to the surface of the mold and drying it, repeating the operation three times. Pour the premix into the mold, and heat cure according to the following curing procedure: first keep it at 70°C for 2 hours, then keep it at 90°C for 2 hours, and finally keep it at 120°C for 3 hours, to obtain a thermosetting shape memory polymer.

[0057] like Figure 1 As shown, the thermosetting shape memory polymer prepared in this embodiment can realize a large deformation recovery process at 90° C., which intuitively shows that the thermosetting shape memory polymer prepared in this embodiment has large deformation and shape memory capabilities.

[0058] like Figure 2 As shown, the shape fixation rate and shape recovery rate of the thermosetting shape memory polymer prepared in this embodiment can still reach 99% after four shape memory cycles, and has good shape memory performance. It should be noted that Figure 2 The horizontal axis in the middle is time, and from left to right, the vertical axes are temperature (black), strain (red), and stress (blue).

[0059] Example 2

[0060] A method for preparing a thermosetting shape memory polymer comprises: placing 80 parts of styrene, 20 parts of butyl acrylate, 6 parts of polyethylene glycol diacrylate 400, and 2 parts of benzoyl peroxide in a beaker, stirring for 30 minutes, ensuring uniform mixing, and obtaining a premix. Applying a release agent to the surface of the mold and drying it, repeating the operation three times. Pour the premix into the mold, and heat cure according to the following curing procedure: first keep it at 70°C for 2 hours, then keep it at 90°C for 2 hours, and finally keep it at 120°C for 3 hours, to obtain a thermosetting shape memory polymer.

[0061] Comparative Example 1

[0062] It is basically the same as Example 1, except that the cross-linking agent is divinylbenzene.

[0063] The shape memory polymers prepared in Example 1, Example 2 and Comparative Example 1 are made into test pieces to measure their DMA curves. Figure 3 As shown, the abscissa is temperature and the ordinate is loss tangent. The glass transition temperatures (Tg) of the shape memory polymers prepared in Example 1, Example 2 and Comparative Example 1 are 88.1°C, 81.2°C and 90.3°C, respectively. It can be seen that compared with Comparative Example 1 using divinylbenzene as a crosslinking agent, Examples 1 and 2 of the present invention using polyethylene glycol diacrylate as a crosslinking agent can reduce the glass transition temperature (Tg) of the shape memory polymer.

[0064] The present invention makes the shape memory polymers prepared in Example 1, Example 2 and Comparative Example 1 into test pieces (size 6*80*2mm) to measure the deformation capacity of the shape memory polymers (gauge length section 40mm, stretching rate 4mm / min), as shown in FIG. Figure 4 As shown, the ordinate in the figure is strain (elongation at break). The elongation at break of the shape memory polymers prepared in Example 1, Example 2 and Comparative Example 1 at the deformation temperature (Tg-20°C) is 370.74%, 337.47% and 242.55%. It can be seen that compared with Comparative Example 1 using divinylbenzene as a cross-linking agent, Examples 2 and 3 of the present invention using polyethylene glycol diacrylate as a cross-linking agent can significantly improve the deformation ability of the shape memory polymer.

[0065] The present invention conducts thermogravimetric analysis test on the shape memory polymers prepared in Example 1, Example 2 and Comparative Example 1. Figure 5 As shown, the shape memory polymer has a very low weight loss at 300°C and has good temperature resistance.

[0066] Example 3

[0067] A method for preparing a thermosetting shape memory polymer comprises: placing 75 parts of styrene, 25 parts of butyl acrylate, 3 parts of polyethylene glycol diacrylate 200, and 2 parts of benzoyl peroxide in a beaker, stirring for 30 minutes, ensuring uniform mixing, and obtaining a premix. Applying a release agent to the surface of the mold and drying it, repeating the operation three times. Pour the premix into the mold, and heat cure according to the following curing procedure: first keep it at 70°C for 2 hours, then keep it at 90°C for 2 hours, and finally keep it at 120°C for 3 hours, to obtain a thermosetting shape memory polymer.

[0068] Example 4

[0069] A method for preparing a thermosetting shape memory polymer comprises: placing 67 parts of styrene, 33 parts of butyl acrylate, 3 parts of polyethylene glycol diacrylate 200, and 2 parts of benzoyl peroxide in a beaker, stirring for 30 minutes, ensuring uniform mixing, and obtaining a premix. Applying a release agent to the surface of the mold and drying it, repeating the operation three times. Pour the premix into the mold, and heat cure according to the following curing procedure: first keep it at 70°C for 2 hours, then keep it at 90°C for 2 hours, and finally keep it at 120°C for 3 hours, to obtain a thermosetting shape memory polymer.

[0070] Depend on Figure 6 It can be seen that the glass transition temperatures (Tg) of the shape memory polymers prepared in Example 1, Example 3 and Example 4 of the present invention are 77.5°C, 69.7°C and 57.6°C respectively. It can be seen that with the increase of the butyl acrylate content in the polymerized monomer, the glass transition temperature decreases significantly. It should be noted that the horizontal axis in the figure is temperature and the vertical axis is heat flow. It should be noted that, Figure 3 and Figure 6 The glass transition temperatures corresponding to Example 1 are different due to different testing methods.

[0071] Example 5

[0072] A method for preparing a thermosetting shape memory composite material, comprising: placing 80 parts of styrene, 20 parts of butyl acrylate, 3 parts of polyethylene glycol diacrylate, and 2 parts of benzoyl peroxide in a beaker, stirring for 30 minutes, ensuring uniform mixing, and obtaining a premix. Apply a release agent to the surface of the mold and dry it, and repeat the operation three times. Lay a spandex-nylon blended fiber mesh cloth in the mold and fix it, wherein the laying angles of the fibers in the spandex-nylon blended fiber mesh cloth are -45° and +45° (i.e., the warp and weft directions are perpendicular), wherein the spandex in the spandex-nylon blended fiber mesh cloth accounts for 13.6wt% and the nylon accounts for 83.4wt%.

[0073] The premix is ​​poured into a mold with a spandex-nylon blended fiber mesh cloth, and thermally cured according to the following curing procedure: first, heat preservation at 70°C for 2 hours, then heat preservation at 90°C for 2 hours, and finally heat preservation at 120°C for 3 hours, to obtain a thermosetting shape memory polymer composite material, wherein the spandex-nylon blended fiber mesh cloth accounts for 9.6% of the volume fraction of the composite material;

[0074] like Figure 7 As shown, the thermosetting shape memory composite material prepared in this embodiment has two phases, the shape memory polymer matrix and the elastic fiber, so that the curve shows two peaks, but the deformation ability of the shape memory composite material is limited by the shape memory polymer matrix. Therefore, the peak corresponding to the shape memory polymer matrix (i.e., 76.4°C) is taken as the Tg of the shape memory composite material. It should be noted that Figure 7The middle abscissa is temperature, and from left to right, the ordinates are storage modulus (black) and loss tangent (blue). The elongation at break of the thermosetting shape memory composite material prepared in this embodiment can reach 376% (the gauge length is 10 mm) at the deformation temperature (56°C). Figure 4 .

[0075] like Figure 8 As shown, the shape fixation rate and shape recovery rate of the thermosetting shape memory composite material prepared in this embodiment can still reach 99% after four shape memory cycles, and has good shape memory performance. It should be noted that Figure 8 The horizontal axis in the middle is time, and from left to right, the vertical axes are temperature (black), strain (red), and stress (blue).

[0076] Comparative Example 2

[0077] It is basically the same as Example 5, except that the spandex-nylon blended fiber mesh cloth is replaced by a glass fiber-carbon fiber blended fiber mesh cloth.

[0078] The use of glass fiber-carbon fiber blended fiber mesh severely limits the deformation capacity of the composite material.

[0079] Comparative Example 3

[0080] The method is basically the same as Example 5, except that the spandex-nylon blended fiber mesh cloth accounts for 50% of the composite material by volume. Due to the excessive fiber content, the polymer matrix resin can only immerse the fibers, and after curing, some fibers are exposed, which affects the continuity of the matrix and thus cannot show shape memory properties.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A thermosetting shape memory polymer, characterized in that: The thermosetting shape memory polymer is obtained by thermally curing a mixture of styrene, acrylate monomers, a free radical initiator and polyethylene glycol diacrylate.

2. The thermosetting shape memory polymer according to claim 1, characterized in that: In parts by weight, the amount of styrene is 20 to 90 parts, the amount of acrylate monomer is 10 to 80 parts, the amount of free radical initiator is 0.5 to 3 parts, and the amount of polyethylene glycol diacrylate is 0.5 to 10 parts.

3. The thermosetting shape memory polymer according to claim 1, characterized in that: The acrylic acid ester monomers include but are not limited to one or more of methyl acrylate, butyl acrylate, methyl methacrylate, hexyl acrylate, hexyl methacrylate, cyclohexyl acrylate, and octadecyl acrylate; The free radical initiator includes but is not limited to one or more of azobisisobutyronitrile, benzoyl peroxide, tert-butyryl peroxide, dibenzoyl peroxide, and azobisisoheptylnitrile; and / or The number average molecular weight of polyethylene glycol diacrylate is 100-3,000.

4. A thermosetting shape memory composite material, characterized in that: The invention comprises the thermosetting shape memory polymer according to any one of claims 1 to 3 and an elastic fiber material. 5 . The thermosetting shape memory composite material according to claim 4 , wherein the volume fraction of the elastic fiber material in the thermosetting shape memory composite material is not greater than 30%.

6. The thermosetting shape memory composite material according to claim 4, characterized in that: The elastic fiber material is one or more of an elastic fiber layer and an elastic fiber fabric; preferably, the elastic fiber in the elastic fiber material is selected from one or more of spandex fiber, nylon fiber, polypropylene fiber, polyethylene fiber and polyurethane fiber.

7. A method for preparing the thermosetting shape memory composite material according to any one of claims 4 to 6, characterized in that: The preparation method comprises: Mix styrene, acrylate monomers, free radical initiator, and polyethylene glycol diacrylate to obtain a premix; The elastic fiber material is layered and mixed with the premix, and then thermally cured to obtain the thermosetting shape memory composite material.

8. The preparation method according to claim 7, characterized in that: The laying angle of the elastic fibers in the elastic fiber material is -180° to 180°, preferably -45° to 45°.

9. The preparation method according to claim 7, characterized in that: The thermal curing temperature is 60-120° C. and the time is 7-24 hours.

10. An application of the thermosetting shape memory composite material according to any one of claims 4 to 6, characterized in that: Used in the field of intelligent core molds.

Citation Information

Patent Citations

  • Fiber enhanced composite material of shape memory, and application

    CN101003652A

  • Shaped memory polymer and its production

    CN101029103A

  • Dual-multiple shape-memory styrenic-based polymer and preparation method thereof

    CN105859972A

  • Shape memory resin-forming composition and shape memory resin molded article molded from the composition

    JP2002220536A

  • Shape Memory Copolymer