Black conductive polymer material and application

By developing black organic electrochromic materials prepared by conjugated polymers, the problem of difficulty in achieving dark tones in traditional smart window technology is solved, low-cost and efficient optical performance and energy efficiency are achieved, and the application field is expanded.

CN119081078AActive Publication Date: 2024-12-06PEKING UNIV SHENZHEN GRADUATE SCHOOL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411482507.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-06
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

Traditional smart window technology relies on liquid crystal or metal oxide films, making it difficult to achieve dark tones such as black, limiting design and functional choices. At the same time, existing electrochromic materials are costly and have limited market applications.

Method used

Develop a black organic electrochromic material based on conjugated polymers. Through specific conjugated polymer structure and preparation process, it can achieve a reversible color change effect from black to transparent, with ultra-low driving voltage and ultra-long cycle stability. Sex and high tinting efficiency.

Benefits of technology

It achieves improved optical performance and energy efficiency at low cost, expands the application areas of smart window technology, and provides more aesthetic choices and energy-saving advantages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081078A_ABST
    Figure CN119081078A_ABST
Patent Text Reader

Abstract

The invention relates to the field of electrochromic materials, in particular to a black conductive polymer material. The black conductive polymer has a total absorption effect in a visible light region, and has ultra-low driving voltage, ultra-long cycle stability and high coloring efficiency. The super-long color changing effect from black to transparency can be achieved. The organic electrochromic material can be effectively used as a material of a color-changing layer of an organic electrochromic element. In addition, the performance and the like of the organic electrochromic device with the organic matter layer containing the compound disclosed by the invention are greatly improved in the aspects of color changing performance, driving voltage, service life, response time and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrochromic materials, and in particular to a black conductive polymer material and application thereof. Background Art

[0002] Traditional electrochromic materials have some limitations in color regulation, optical properties and stability. Conjugated polymers have a wide range of application potential in the field of electrochromism due to their unique electrical properties and structural characteristics. Therefore, it is necessary to provide an electrochromic material based on conjugated polymers to meet a wider range of application needs. Smart window technology, as an important component in modern architecture and the automotive industry, has always been a hot area of ​​research and development. This technology allows dynamic regulation of window transmittance, thereby providing optimization of energy efficiency, comfort and privacy. Traditional smart window technology relies on liquid crystals or metal oxide films, which are effective but have limitations in cost, durability and color selection. In particular, existing technologies have difficulty in achieving dark tones, such as black, which limits the choices of designers and architects in terms of aesthetics and functionality. In recent years, electrochromic (EC) technology has attracted attention as a new solution for smart windows. Electrochromic materials change their color by applying voltage, thereby regulating the transmittance of light. Although this technology shows great potential in energy efficiency and user control, most existing electrochromic materials are mainly based on inorganic compounds, which are usually transparent or light-colored and have high manufacturing costs, limiting their widespread application in the market. Therefore, the development of a new black organic electrochromic material is not only a technological innovation, but also meets the market's demand for more diverse and affordable smart window solutions.

[0003] Compared with traditional inorganic materials, organic electrochromic materials are more flexible in synthesis and can achieve a wide range of color adjustments through molecular design, including darker color tones such as black. In addition, the manufacturing process of these materials is more economical, which is expected to reduce the overall cost of smart windows and make them more popular. In addition, black organic electrochromic materials offer unique advantages in terms of visual effects and energy efficiency. Black not only provides more choices in aesthetics, but also excels in energy saving due to its excellent light-to-heat conversion efficiency. The development of such materials can significantly improve the energy efficiency of smart windows, while providing architects and designers with more innovative design space. Summary of the invention

[0004] In view of the above shortcomings of existing black organic electrochromic materials, the present invention provides a bismuth-containing compound, a preparation method and an application. The purpose of the present invention is to develop a new type of black organic electrochromic material that can not only provide improved optical properties and higher energy efficiency, but also be achieved at a lower cost, thereby making smart window technology feasible and economical in a wider range of application fields. Through the innovation of this material, the present invention is expected to promote the development of smart window technology and bring revolutionary changes to the construction and automotive industries.

[0005] The technical solution of the present invention is achieved by providing a black conductive polymer material, the molecular formula of which is as follows:

[0006]

[0007] Among them, y=1, x+z+w=1; x≥0, z≥0, w≥0; at most one of x, z, w is 0;

[0008] n is a natural number less than 100; R5 is a branched or straight alkyl chain of 1 to 20 carbon atoms.

[0009] R1=R2, R3=R4; R1 and R3 are each independently selected from hydroxyl, carbonyl, carboxyl, thioether group, ester group, ether group, nitro group, halogen, C1~C20 hydroxyl, C2~C20 carbonyl, C2~C40 carboxyl, C3~C20 thioether group, C1~C20 ester group, C2~C20 ether group, C2~C60 nitro, halogen-containing C1~C20 alkyl chain, silyl group, C1~C20 arylsilyl group.

[0010]

[0011] In one embodiment of the present invention, the polymer material is selected from the following:

[0012]

[0013]

[0014]

[0015] The invention also provides application of the black conductive polymer material in electrochromic devices.

[0016] The beneficial effects are as follows:

[0017] The black conductive polymer of the present invention has a full absorption effect in the visible light region, and the conductive polymer has an ultra-low driving voltage, ultra-long cycle stability and high coloring efficiency. It can achieve an ultra-long color change effect from black to transparent. It can be effectively used as a material for the color change layer of an organic electrochromic element. In addition, the organic electrochromic device whose organic layer contains the compound of the present invention greatly improves the performance of the device in terms of color change performance, driving voltage, life, response time, etc.

[0018] This material is mainly used in the fields of smart windows, high-end display technology and energy-saving buildings. The core of the invention is to use specific conjugated organic polymers, combined with advanced preparation processes, to achieve a reversible change from black to transparent under voltage excitation. The material adopts a unique conjugated polymer structure, which optimizes the light absorption characteristics of the material by precisely controlling the molecular arrangement and electronic conjugation length, so that it has a shorter response time under a specific voltage. The design of the conjugated polymer also takes into account its electrochemical stability and color retention ability under long-term use. The preparation method includes a series of organic synthesis steps for constructing a conjugated polymer with a specific molecular structure, as well as subsequent material processing technology to ensure the uniformity and functionality of the material. The black conjugated electrochromic material of this patent has a high adaptability and excellent performance, providing new possibilities for the use of electrochromic technology in various high-demand applications, especially in occasions where long-life and fast-response color control is required. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The schematic diagram is a structural diagram of an electrochromic device using the polymer material of the present invention.

[0020] Figure 2 The CV curve of the electrochromic device using the polymer material of the present invention is shown in FIG.

[0021] Figure 3 The figure is a comparison diagram of the electrochromic device using the polymer material of the present invention in the neutral state and the colored state. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0024] The electrochromic device of the present invention is mainly composed of an electrochromic layer, a conductive layer, an ion conductor (electrolyte), a counter electrode, a substrate and a power source. The electrochromic layer can be composed of a single or multiple mixed compounds and formed by a solution coating method, including but not limited to spin coating, dip coating, scraping, inkjet printing or thermal transfer. In addition, the type of substrate in the present invention is not particularly limited and may include silicon wafers, quartz, glass plates, metal plates, plastic films, etc.

[0025] Specific implementation plan:

[0026] Example 1: Synthesis of black conjugated polymer P1

[0027] P1 is a polar conductive polymer containing spirofluorene as the main component, and the general synthesis route thereof is shown below.

[0028]

[0029] A-1 (4.53 g, 4.66 mmol), A-2 (10 g, 18.63 mmol), A-3 (3.28 g, 11.18 mmol), A-4 (0.95 g, 2.79 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P1 polymer.

[0030] A-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0031] A-2: 1H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0032] A-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0033] A-4: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P1: 13 C NMR(400MHz,Chloroform-d)δ169.35,164.67,161.49,153.27,149.82,144.41,140.11,137.98,134.01,133.79,13 2.47,131.59,130.69,129.42,124.15,119.05,116.19,113.50,113.01,99.68,63.01,45.12,35.06,14.28,14.10.

[0034] Example 2: Synthesis of black conjugated polymer P2 as shown in the figure

[0035]

[0036] B-1 (4.53 g, 4.66 mmol), B-2 (10 g, 18.63 mmol), B-3 (2.73 g, 9.32 mmol), B-4 (1.51 g, 4.66 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N, N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P2 polymer.

[0037] B-1: 1H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0038] B-2: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0039] B-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0040] B-4: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P2: 13 C NMR(400MHz,Chloroform-d)δ169.35,164.67,161.49,153.27,149.82,144.41,140.11,137.98,134.01,133.79,13 2.47,131.59,130.69,129.42,124.15,119.05,116.19,113.50,113.01,99.68,63.01,45.12,35.06,14.28,14.10.

[0041] Example 3: Synthesis of black conjugated polymer P3

[0042]

[0043] C-1 (4.53 g, 4.66 mmol), C-2 (10 g, 18.63 mmol), C-3 (2.19 g, 7.45 mmol), C-4 (3.62 g, 11.18 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P3 polymer.

[0044] C-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0045] C-2: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0046] C-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0047] C-4: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P3: 13C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0048] Example 4: Synthesis of black conjugated polymer P4

[0049]

[0050] D-1 (5.43 g, 5.59 mmol), D-2 (10 g, 18.63 mmol), D-3 (2.19 g, 2.74 mmol), D-4 (1.21 g, 3.72 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P4 polymer.

[0051] D-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0052] D-2: 1H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0053] D-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0054] D-4: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P4: 13 C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0055] Example 5: Synthesis of black conjugated polymer P5

[0056]

[0057] E-1 (9.06 g, 9.32 mmol), E-2 (10 g, 18.63 mmol), D-3 (2.74 g, 9.32 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P5 polymer.

[0058] E-1: 1H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0059] E-2: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0060] E-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0061] P5: 13 C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0062] Example 6: Synthesis of black conjugated polymer P6

[0063]

[0064] F-1 (4.43 g, 5.59 mmol), F-2 (10 g, 18.63 mmol), F-3 (3.83 g, 13.04 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P6 polymer.

[0065] F-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0066] F-2: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0067] F-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0068] P6: 13C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0069] Example 7: Synthesis of black conjugated polymer P7

[0070]

[0071] G-1 (12.68 g, 13.04 mmol), G-2 (10 g, 18.63 mmol), G-3 (1.81 g, 5.59 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P7 polymer.

[0072] G-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0073] G-2: 1H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0074] G-3: 1 H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0075] P7: 13 C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0076] Example 8: Synthesis of black conjugated polymer P8

[0077]

[0078] H-1 (16.31 g, 16.77 mmol), H-2 (10 g, 18.63 mmol), H-3 (0.60 g, 1.86 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P8 polymer.

[0079] H-1: 1H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0080] H-2: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0081] H-3: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P8: 13 C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0082] Example 9: Synthesis of black conjugated polymer P9

[0083]

[0084] I-1 (10.97 g, 13.68 mmol), I-2 (10 g, 27.36 mmol), I-3 (4.43 g, 13.68 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N, N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P9 polymer.

[0085] I-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0086] I-2: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0087] I-3: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P9: 13C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0088] Example 10: Synthesis of black conjugated polymer P10

[0089]

[0090] J-1 (2.19 g, 2.74 mmol), J-2 (10 g, 27.36 mmol), J-3 (7.97 g, 24.62 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P10 polymer.

[0091] J-1: 1 H NMR(500MHz,Chloroform-d)δ7.58(d,J=8.2Hz,2H),7.54-7.49(m,2H),7.48(d,J=3.6Hz,2H), 7.43(d,J=1.8Hz,2H),7.18(dd,J=8.8,2.6Hz,2H),6.88(d,J=8.8Hz,2H),4.27(q,J=7.1Hz,4H) ,4.16(t,J=5.1Hz,4H),3.87(t,J=5.1Hz,4H),3.74(dd,J=5.9,3.7Hz,4H),3.67-3.62(m,9H),3 .57(dd,J=6.0,3.6Hz,4H),3.50(q,J=7.0Hz,5H),1.31(t,J=7.1Hz,7H),1.19(t,J=7.0Hz,6H).

[0092] J-2: 1H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0093] J-3: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P10: 13 C NMR(400MHz,Chloroform-d)δ167.36,164.67,156.80,153.27,149.80,144.41,139.66,137.98,137.84,137.38,134.01,132.47,130.69,130.4 2,128.93,124.15,119.05,118.76,114.79,113.01,99.68,93.03,92.63 ,91.93,63.65,63.01,62.08,60.86,45.12,35.06,15.23,14.28,14.10.

[0094] Example 11: Synthesis of black conjugated polymer P11

[0095]

[0096] K-2 (10) g, 13.68 mmol), K-3 (4.02 g, 13.68 mmol), K-4 (4.43 g, 13.68 mmol), Pd(OAC)2 (0.083 g, 0.37 mmol), PiVOH (0.57 g, 5.5 mmol) and K2CO3 (5.14 g, 37.27 mmol) were dissolved in N,N-dimethylacetamide (DMAc) (6 mL) and heated at 130 ° C in a nitrogen atmosphere for 48 hours. The polymer was precipitated in methanol and filtered to obtain P11 polymer.

[0097] K-1: 1 H NMR (400MHz, Chloroform-d) δ4.08 (s, 4H), 3.73-3.60 (m, 14H), 3.60-3.51 (m, 15H), 3.51 (d, J = 7.0Hz, 3H), 1.19 (t, J = 7.0Hz, 7H).

[0098] K-2: 1H NMR (400MHz, Chloroform-d) δ7.66 (s, 2H).

[0099] K-3: 1 H NMR(500MHz,Chloroform-d)δ3.99(q,J=5.1Hz,2H),1.29(t,J=5.0Hz,3H).P11:13C NMR(400MHz,Chloroform-d)δ164.67,153.27,144.41,137.98,134.01,130.69,113.01,99.68,63.01,45.12,35.06,14.10.

[0100] The present invention introduces a novel black conductive polymer, the device of which has ultra-low driving voltage, ultra-long cycle stability and high coloring efficiency. Specifically, a black high-performance conductive polymer is obtained by copolymerizing four monomers. In addition, the polymer has a highest occupied molecular orbital (HOMO) energy level of -4.21 to -4.47 eV and a lowest unoccupied molecular orbital (LUMO) energy level of -2.52 to -2.78 eV. The molecular weights of the polymer materials in the aforementioned embodiments are shown in Table 1 below.

[0101] Table 1. Polymer molecular weight

[0102]

[0103] Using this compound as a color-changing layer material in an organic electrochromic device can improve the device's life and coloring efficiency. Figure 1 As shown. Ion storage layer Prussian blue (1-50 mg / mL). The CV curve of the device made of black conjugated polymer P5 in Example 5 is as follows Figure 2 The device made of black conjugated polymer P5, the photo comparison of neutral black and colored transparent color, as shown in Figure 3 shown.

[0104] The polymer structures listed above are only partial representatives, and other black conductive polymer molecules containing the same concept are within the scope of protection of this patent.

[0105] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A black conductive polymer material, characterized in that: The molecular formula is as follows: Among them, y=1, x+z+w=1; x≥0, z≥0, w≥0; at most one of x, z, w is 0; n is a natural number less than 100; R5 is a branched or linear alkyl chain of 1 to 20 carbon atoms; R1=R2, R3=R4; R1 and R3 are each independently selected from hydroxyl, carbonyl, carboxyl, thioether group, ester group, ether group, nitro group, halogen, C1~C20 hydroxyl, C2~C20 carbonyl, C2~C40 carboxyl, C3~C20 thioether group, C1~C20 ester group, C2~C20 ether group, C2~C60 nitro, halogen-containing C1~C20 alkyl chain, silyl group, C1~C20 arylsilyl group.

2. The black conductive polymer material according to claim 1, characterized in that: R1 is selected from the following 3. The black conductive polymer material according to claim 1, characterized in that: Selected from:

4. Use of the black conductive polymer material according to any one of claims 1 to 3 in an electrochromic device.

Citation Information

Patent Citations

  • Green electrochromism macromolecule material as well as preparation method and application thereof

    CN107674185A

  • Black electrochromic polymer material and preparation method and application thereof

    CN107880253A

  • Black polymer material, and preparation method and application thereof

    CN110229312A

  • Black electrochromic polymer and preparation method thereof

    CN118255971A

  • Electrochromic polymer and synthesis and uses thereof

    US20190016852A1