Preparation method of photoactive layer film, organic solar cell and preparation method of organic solar cell

By adding amphiphilic additives to the photoactive layer material to regulate the interface tension, the problem of the volatility of low boiling point solvents is solved, and spontaneous diffusion is achieved in the atmospheric environment to form a uniform film, improving the efficiency and material utilization of organic solar cells .

CN119081190AActive Publication Date: 2024-12-06WESTLAKE UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411572150.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-06
Estimated Expiration
2044-11-06

AI Technical Summary

Technical Problem

In the prior art, low boiling point solvents such as chloroform volatilize too quickly in spontaneous diffusion film formation process, resulting in the photoactive layer being unable to form a uniform thin film, affecting the power conversion efficiency of organic solar cells.

Method used

By adding amphiphilic additives to the photoactive layer material, the interface tension between the droplets and the culture medium solvent liquid surface is regulated, and the spontaneous diffusion of high-quality uniform photoactive layer film is promoted in the atmospheric environment, and the recycling and reuse process is used to reduce the Waste of materials.

Benefits of technology

It realizes the preparation of uniform photoactive layer thin films in an atmospheric environment with a low cost and simple process, which reduces the manufacturing complexity of organic solar cells, improves the utilization rate of photoactive layer materials, and improves the power conversion efficiency of organic solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081190A_ABST
    Figure CN119081190A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a preparation method of a photoactive layer thin film, an organic solar cell and a preparation method thereof. The preparation method of the photoactive layer film comprises the following steps: blending a polymer donor and a small molecule receptor, and dissolving the mixture into an active layer solvent to form a first precursor solution; dissolving an amphiphilic additive into the active layer solvent to form a second precursor solution; mixing the second precursor solution and the first precursor solution according to a predetermined volume ratio to obtain a photoactive layer organic solution doped with an amphiphilic additive; and transferring liquid drops of the photoactive layer organic solution into an open container containing the culture medium solvent, so that the liquid drops spontaneously diffuse on the liquid level of the culture medium solvent to form a uniform photoactive layer film. The amphiphilic additive is doped into the photoactive layer material, so that the interfacial tension between solution droplets and the surface of the culture medium solvent can be regulated and controlled, and a spontaneously-diffused high-quality uniform photoactive layer film is formed on the surface of the culture medium solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of organic solar cell preparation, and more specifically, to a method for preparing a photoactive layer film, an organic solar cell and a method for preparing the same. Background Art

[0002] Photovoltaics is an important clean energy source, and organic photovoltaics have attracted widespread attention due to its outstanding advantages such as solution processability, flexibility, lightness, and transparency. The preparation of organic solar cells using a solution method under open-air conditions has become a low-cost clean energy technology. Traditional solution processing techniques mainly include spin coating, blade coating, slit coating, etc. Water transfer is another solution processing technology, which has become an ultra-fast, scalable and versatile spontaneous diffusion film-forming process. Compared with the above-mentioned traditional solution method, the spontaneous diffusion film-forming process has unique advantages and applications. First, the film-forming process does not require large equipment, but only an open container containing a solvent. Secondly, the entire process does not rely on a harsh nitrogen atmosphere, can be completed in the air, and is insensitive to air humidity. In addition, unlike the large loss of photoactive layer materials in the spin coating process, the spontaneous diffusion film-forming process can improve the utilization rate of materials and reduce the waste of expensive photoactive layer materials through strategies such as multiple transfers and recycling.

[0003] At present, the research on the selection of photoactive layer materials and the details of the spontaneous diffusion film-forming process in this field shows that this process is expected to achieve uniform thickness distribution and good phase separation morphology of the photoactive layer. On the one hand, the reported spontaneous diffusion film-forming processes all use high-boiling-point chlorobenzene (132°C) as the solvent. After the droplet contacts the water surface, while the chlorobenzene slowly evaporates, the photoactive layer material gradually spontaneously diffuses to form a uniform film. At the same time, with the self-assembly of the polymer main chain, a beneficial phase separation is gradually formed. On the other hand, the photoactive layer material based on the non-fullerene Y6 series acceptor has small and discrete oriented crystals in the chloroform system, so the power conversion efficiency of the organic solar cell prepared with the photoactive layer material dissolved in the chloroform system is higher than that of the chlorobenzene system. However, since the boiling point of chloroform is only 61°C, it evaporates very quickly in the spontaneous diffusion film-forming process. Before the photoactive layer material is completely diffused, the chloroform has completely evaporated, resulting in the inability of the photoactive layer to diffuse into a uniform film.

[0004] In summary, it is urgent to develop a spontaneous diffusion film-forming process for photoactive layer materials suitable for low-boiling point solvents (such as chloroform system). With the goal of improving the power conversion efficiency of organic solar cells, the spontaneous diffusion process is innovated to achieve the preparation of uniform photoactive layer films using a simple and low-cost process. Summary of the invention

[0005] In order to solve the above technical problems, the present disclosure provides a method for preparing a photoactive layer film, an organic solar cell and a method for preparing the same. By doping an amphiphilic additive into the photoactive layer material, the interfacial tension between the solution droplets and the surface of the culture medium solvent can be regulated, thereby forming a spontaneously diffused high-quality uniform photoactive layer film on the surface of the culture medium solvent. The photoactive layer obtained by the preparation method of the present disclosure in an atmospheric environment can be used to prepare an organic solar cell, which can reduce the complexity of the process and reduce the waste of expensive photoactive layer materials through a recycling and reuse process.

[0006] The first scheme of the present disclosure provides a method for preparing a photoactive layer film, which is used in an organic solar cell. The preparation method includes: blending a polymer donor and a small molecule acceptor and dissolving them in an active layer solvent to form a first precursor solution; dissolving an amphiphilic additive in the active layer solvent to form a second precursor solution; mixing the second precursor solution and the first precursor solution in a predetermined volume ratio to obtain a photoactive layer organic solution doped with the amphiphilic additive; and transferring a droplet of the photoactive layer organic solution into an open container containing a culture medium solvent so that it spontaneously diffuses on the liquid surface of the culture medium solvent to form a uniform photoactive layer film; wherein the boiling point of the material of the active layer solvent is lower than the boiling point of the culture medium solvent, and the surface tension of the active layer solvent is less than the surface tension of the culture medium solvent; wherein the material of the amphiphilic additive is selected so as to be able to interact with the culture medium solvent to promote the diffusion of the droplet on the liquid surface, and at the same time to interact with the active layer solvent to promote the continuity of the photoactive layer film.

[0007] The second scheme of the present disclosure provides an organic solar cell. The organic solar cell comprises a transparent conductive substrate layer, a hole transport layer, a photoactive layer, an electron transport layer and a top electrode layer; wherein the photoactive layer is obtained by using the photoactive layer film prepared by the preparation method described in the first scheme; wherein the material of the transparent conductive substrate layer is selected from any one of ITO, FTO, AZO, GZO conductive glass, metal nanowire substrate and highly transparent metal film substrate; the material of the hole transport layer is water-based PEDOT:PSS or MoO 3 ; The material of the electron transport layer is a combination of ZnO and PEIE; The material of the top electrode layer is selected from any one of Ag, Au, Al and Pt.

[0008] The third scheme of the present disclosure provides a method for preparing an organic solar cell. The preparation method includes the following steps: forming one of the hole transport layer and the electron transport layer on the transparent conductive substrate layer to obtain an intermediate substrate; using the preparation method described in the first scheme to obtain the photoactive layer film; performing transfer processing on the photoactive layer film: using a vacuum suction pen to suck the intermediate substrate, obliquely pressing the photoactive layer film on the water surface, dividing the film at the edge, obliquely lifting the intermediate substrate printed with the photoactive layer film, annealing, and forming the photoactive layer; and sequentially forming the other of the hole transport layer and the electron transport layer, and the top electrode layer above the photoactive layer.

[0009] The method for preparing the photoactive layer film, the organic solar cell and the method for preparing the same provided by the present disclosure have the following beneficial effects compared with the prior art: (1) By doping the amphiphilic additive into the photoactive layer material, the interfacial tension between the droplet and the medium solvent surface can be regulated, thereby promoting the thickness uniformity of the photoactive layer film formed by spontaneous diffusion film formation; at the same time, the amphiphilic additive can interact with the active layer solvent, thereby promoting the continuity of the photoactive layer film; (2) The photoactive layer prepared by the spontaneous diffusion film forming method in the atmospheric environment is used to prepare organic solar cells, which can reduce the complexity of the device process; the prepared photoactive layer film can be used to transfer the photoactive layers of multiple organic solar cells at the same time, thereby improving the utilization rate of the photoactive layer; (3) By re-dissolving the recovered solid mixture into the active layer solvent, the remaining photoactive layer material can be recycled, effectively avoiding the waste of photoactive layer materials and reducing manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. When appropriate, the same reference numerals are used in all drawings to refer to the same or similar parts. Such embodiments are illustrative and are not intended to be exhaustive or exclusive embodiments of the present device or method. In the drawings: Figure 1 is a schematic flow chart of a method for preparing a photoactive layer film according to an embodiment of the present disclosure; Figure 2 is a schematic flow chart of a method for preparing an organic solar cell according to an embodiment of the present disclosure; Figure 3 is a schematic structural diagram of an organic solar cell according to an embodiment of the present disclosure; Figure 4 is a JV curve of an organic solar cell according to another embodiment of the present disclosure; Figure 5 is a JV curve of an organic solar cell according to another embodiment of the present disclosure; Figure 6 is a JV curve of an organic solar cell according to another embodiment of the present disclosure; Figure 7 is a schematic flow chart of a method for preparing an organic solar cell according to another embodiment of the present disclosure. DETAILED DESCRIPTION

[0011] In order to make the purpose, technical solution and advantages of the embodiment of the present application clearer, the technical solution of the embodiment of the present application will be clearly and completely described in conjunction with the drawings of the embodiment of the present application. Obviously, the described embodiment is a part of the embodiment of the present application, not all of the embodiments. Based on the described embodiment of the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0012] Unless otherwise defined, the technical terms or scientific terms used in this application should be understood by people with ordinary skills in the field to which this application belongs. "First", "second" and similar words used in this application do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0013] In order to keep the following description of the embodiments of the present application clear and concise, the present application omits detailed descriptions of known functions and known components.

[0014] Figure 1 FIG. 1 is a schematic flow chart of a method 100 for preparing a photoactive layer thin film according to this embodiment. Figure 1 As shown, the preparation method 100 includes steps S110 to S140.

[0015] S110: blending a polymer donor and a small molecule acceptor, and dissolving them into an active layer solvent to form a first precursor solution.

[0016] S120: dissolving the amphiphilic additive into the active layer solvent to form a second precursor solution.

[0017] S130: Mixing the second precursor solution and the first precursor solution in a predetermined volume ratio to obtain a photoactive layer organic solution doped with the amphiphilic additive.

[0018] S140: Pipette droplets of the photoactive layer organic solution into an open container containing a culture medium solvent, so that the droplets spontaneously diffuse on the liquid surface of the culture medium solvent to form a uniform photoactive layer film.

[0019] S110 to S140 will be described in detail below.

[0020] As described above, this embodiment is dedicated to developing a spontaneous diffusion film-forming process for photoactive layer materials suitable for low-boiling point solvents in order to prepare organic solar cells with high power conversion efficiency. Therefore, the active layer solvent in this article should be selected from solvents with low boiling points, such as chloroform (boiling point 61°C), dichloromethane (boiling point 40°C), 2-methyltetrahydrofuran (boiling point 80°C) or tetrahydrofuran (boiling point 66°C), which can be any one of the above solvents or a combination of multiple thereof.

[0021] The blend of the polymer donor and the small molecule acceptor here can be PM6:Y6, PM6:BTP-eC9, PM6:Y6:PCBM or PM6:BTP-eC9:PCBM.

[0022] The material of the amphiphilic additive is selected so as to be able to interact with the culture medium solvent to promote the diffusion of the droplets on the liquid surface, and to interact with the active layer solvent to promote the continuity of the photoactive layer film. By adding the amphiphilic additive to the photoactive layer organic solution, the additive can interact with the culture medium solvent and the active layer solvent in the spontaneous diffusion film forming process, thereby obtaining a continuous photoactive layer film with uniform thickness and good phase separation effect.

[0023] Preferably, the amphiphilic additive may be a polymer, and more preferably, the amphiphilic additive may include poly (N-isopropylacrylamide, PNIPAM), polysorbate 20 (Polysorbate 20, Tween 20) or pluronic F127 (Pluronic F127, PF127).

[0024] It should be understood that the active layer solvent in S120 should be the same as the active layer solvent in S110, so that the polymer donor, the small molecule acceptor and the amphiphilic additive can be dissolved in the same solvent when mixed, ensuring the accuracy of the mixing ratio.

[0025] As can be understood by those skilled in the art, in the spontaneous diffusion film-forming process, the culture medium solvent should be selected to have a larger surface tension and a higher boiling point, and the boiling point of the material of the active layer solvent should be lower than the boiling point of the culture medium solvent, and the surface tension of the active layer solvent should be smaller than the surface tension of the culture medium solvent.

[0026] Preferably, the culture medium solvent may be any one or more combinations of pure water, imidazole ionic liquids, pyridinium ionic liquids, quaternary ammonium salt ionic liquids, perfluorooctane sulfonic acid and fluorocarbon compositions.

[0027] On the other hand, Figure 2 As shown, the present disclosure also provides a method 200 for preparing an organic solar cell. The structure of the prepared organic solar cell 300 is as shown in FIG. Figure 3 The preparation method 200 includes the following steps S210 to S240. Figure 2 and Figure 3 The above steps S210 to S240 are described in detail below.

[0028] S210 , forming one of the hole transport layer 320 and the electron transport layer 340 on the transparent conductive substrate layer 310 to obtain an intermediate substrate.

[0029] S220, obtaining a photoactive layer film by using the preparation method 100.

[0030] S230, transfer the photoactive layer film: use a vacuum pen to suck the intermediate substrate, obliquely press the photoactive layer film onto the liquid surface of the culture medium solvent, divide the film at the edge, obliquely lift the intermediate substrate printed with the photoactive layer film, anneal, and form a photoactive layer 330.

[0031] S240 , forming the other of the hole transport layer 320 and the electron transport layer 340 , and the top electrode layer 350 in sequence above the photoactive layer 330 .

[0032] In order to better explain the preparation of the organic solar cell 300 provided by the present disclosure, the following description will be given by taking the culture medium solvent as pure water, the active layer solvent as chloroform, and the polymer donor: small molecule acceptor group as PM6:Y6 as an example.

[0033] In S210, a hole transport layer 320 or an electron transport layer 340 can be formed on the transparent conductive substrate layer 310 by spin coating, that is, an intermediate substrate consisting of a transparent conductive substrate layer 310 + a hole transport layer 320 can be formed (correspondingly, an electron transport layer 340 is formed in the subsequent S240 to obtain an organic solar cell with a positive structure), or an intermediate substrate consisting of a transparent conductive substrate layer 310 + an electron transport layer 340 can be formed (correspondingly, a hole transport layer 320 is formed in the subsequent S240 to obtain an organic solar cell with an inverted structure), and the present invention is not limited here.

[0034] Optionally, the material of the transparent conductive substrate layer 310 is selected from any one of ITO, FTO, AZO, GZO conductive glass, metal nanowire substrate and highly transparent metal film substrate, and the material of the hole transport layer 320 is aqueous PEDOT:PSS or MoO 3 , the material of the electron transport layer 340 is a combination of ZnO and PEIE. Figure 3 In the preferred embodiment shown, the transparent conductive base layer 310 is a glass substrate with an ITO film, and the material of the hole transport layer 320 is aqueous PEDOT:PSS.

[0035] In S210, specifically, the ITO conductive substrate of the glass substrate is ultrasonically cleaned with a detergent, deionized water, and isopropyl alcohol in sequence, and then dried at high temperature or blown with airflow to complete the preparation of the transparent conductive substrate layer 310. Next, the hole transport layer 320 is spin-coated on the transparent conductive substrate layer 310 treated with oxygen plasma. The spin-coated material is 50% aqueous PEDOT:PSS (Al 4083), and the spin-coating conditions are 4 krpm, 30 s, and annealing at 120°C for 5 min to obtain an intermediate substrate.

[0036] Preferably, the material of the hole transport layer 320 is selected from Al 4083 as PEDOT:PSS, because Al 4083 has good photoelectric properties and helps to improve the photoelectric conversion efficiency of solar cells, and is the best choice for preparing the hole transport layer 320 by solution method in organic solar cells.

[0037] In S220, specifically, a PM6:Y6 solution is prepared, the mass ratio of the polymer donor and the small molecule acceptor is 1:1.2, the total concentration is 25 mg / mL, PM6:Y6 is dissolved in chloroform (active layer solvent), and stirred at 50°C for 1 hour to obtain a first precursor solution. PNIPMA (amphiphilic additive) is dissolved in chloroform at a concentration of 20 mg / mL to obtain a second precursor solution; the obtained second precursor solution and the first precursor solution are mixed according to a predetermined volume ratio; the spontaneous diffusion film forming process is carried out at 25°C and a relative humidity of about 40%, and a 1 / 2 volume of pure water solution (culture medium solvent) is placed in a culture dish with a diameter of 95 mm, and 18 μL of PM6:Y6 solution is taken with a pipette and dropped on the water surface.

[0038] In S230, specifically, after the thin film on the water surface is dried, the transfer is performed, and the intermediate substrate coated with the hole transport layer 320 is sucked with a vacuum pen, and the thin film on the water surface is tilted to avoid bubbles. After the thin film at the edge is cut, the substrate is lifted up at an angle. This process can be repeated multiple times to avoid material waste. After the transfer, the thin film is placed on a hot stage and annealed at 80°C for 2 minutes to obtain the photoactive layer 330.

[0039] In S240, ZnO solution and PEIE solution are sequentially spin-coated on the photoactive layer 330 as the electron transport layer 340. The function of PEIE is to improve the stability of the device. The spin coating conditions of the ZnO solution are 4 krpm, 30 s, and no annealing is required. The PEIE solution is prepared by dissolving PEIE in ethylene glycol monomethyl ether, with a concentration of 0.5 wt%. The spin coating conditions are 3 krpm, 30 s, and no annealing is required. Then, a top electrode layer 350 can be prepared on the electron transport layer 340 by an evaporation process. The material of the top electrode layer 350 can optionally be any one of Ag, Au, Al and Pt. Figure 3 In the preferred embodiment shown, the material of the top electrode layer 350 is preferably Ag.

[0040] It should be particularly noted that the transparent conductive substrate layer 310, hole transport layer 320, photoactive layer 330, and electron transport layer 340 of the organic solar cell disclosed in the present invention can all be prepared by a solution method under an atmospheric environment, without the need for a strict nitrogen or vacuum atmosphere, thereby reducing the manufacturing complexity of the organic solar cell.

[0041] In the embodiments provided in the present disclosure, in order to verify the effect of amphiphilic additives on the formation of a photoactive layer film of uniform thickness, the present disclosure designs different volume ratios of the second precursor solution and the first precursor solution, that is, the doping ratio of the amphiphilic additive is optimized, ranging from 0.1% to 10%. This is because increasing the doping ratio within a certain range is conducive to increasing the diffusion diameter of the film, but it will reduce the film thickness. The thickness of the undoped PM6:Y6 film is distributed at 115±82.6nm, with a large variance. Taking the amphiphilic additive as PNIPAM as an example, the thickness of the PM6:Y6 film doped with 2 vt% PNIPAM is 85.5±7.48nm, and the thickness distribution is relatively uniform. Continuing to increase the PNIPAM doping ratio, the spontaneous diffusion process has undergone some changes. Due to the excessive aggregation of amphiphilic molecules, agglomeration is easy to occur in the center of the droplet. After doping with 10 vt% PNIPAM, a 54.3±9.60 nm film is formed around, but a very thick film will be formed in the central area due to excessive aggregation. Similar phenomena were also observed in the doping system of Tween20 and PF127.

[0042] In addition, the present disclosure also verifies the effects of different types of amphiphilic additives on the diffusion of the photoactive layer into a thin film with uniform thickness.

[0043] Example 1 (unadopant amphiphilic additive): After accurately weighing 11.4 mg PM6 and 13.6 mg Y6, 1 mL chloroform was added and stirred at 50 °C in air for 1 h. PM6:Y6 thin film was prepared by spontaneous diffusion film-forming process. The spontaneous diffusion process was carried out at 25 °C and relative humidity of about 40%. A 1 / 2 volume of pure water solution was placed in a Petri dish with a diameter of 95 mm. 18 μL PM6:Y6 solution was taken with a pipette and dropped on the water surface at an angle of 45°. Before the PM6:Y6 droplet was completely diffused, the chloroform evaporated quickly, resulting in the inability of the photoactive layer to diffuse into a uniform film.

[0044] Example 2 [amphiphilic additive is poly (N-isopropylacrylamide) (PNIPAM)]: The other steps of Example 2 are the same as those of Example 1, except that 20 mg of PNIPAM is accurately weighed and then 1 mL of chloroform is added and shaken to mix; before use, 1 µL of PNIPAM solution is added to each 100 µL of PM6:Y6 solution to obtain a mixed solution with a PNIPAM doping ratio of 1 vt%. Subsequently, a PM6:Y6 film is prepared using a self-dispersive film-forming process. After the PM6:Y6 droplets are doped with 1 vt% PNIPAM, they can be diffused into a uniform photoactive layer film.

[0045] In Example 2, the PM6:Y6 thin film prepared by the spontaneous diffusion film forming process is applied to an organic solar cell, and the specific steps are as follows.

[0046] 1) Prepare the active layer solution: accurately weigh 11.4 mg PM6 and 13.6 mg Y6, add 1 mL chloroform and stir at 50 °C in air for 1 h.

[0047] 2) Accurately weigh 20 mg PNIPAM and add 1 mL chloroform to shake and mix. In the comparative example, the doping ratio of PNIPAM was optimized. The specific steps are as follows: 0.5, 1, 2, 5, and 10 μL PNIPAM solution were added to each 100 μL PM6:Y6 solution, and after stirring at room temperature for 10 min, photoactive layer solutions with PNIPAM doping ratios of 0.5, 1, 2, 5, and 10 vt% were obtained, corresponding to comparative examples 1-1, 1-2, 1-3, 1-4, and 1-5, respectively.

[0048] 3) Use detergent, deionized water, and isopropyl alcohol to ultrasonically clean the ITO conductive base of the glass substrate in sequence, and then dry it at high temperature or blow it with air flow to complete the preparation of the hard transparent bottom electrode.

[0049] 4) Before spin coating PEDOT:PSS, the ITO conductive substrate was treated with oxygen plasma for 2 min. The PEDOT:PSS solution was filtered with a 0.45 µm nylon filter and then spin coated. The spin coating conditions were static coating, 4 krpm, 30 s, the film thickness was about 10 nm, and annealing was performed at 120°C for 5 min.

[0050] 5) Prepare PM6:Y6 thin film using spontaneous diffusion film forming process. Place 1 / 2 volume of pure water solution in a culture dish with a diameter of 95 mm. Take 18 μL of the active layer solution prepared in step 1) with a pipette and drop it on the water surface at an angle of 45°.

[0051] 6) After the film on the water surface is dry, transfer printing is performed. Use a vacuum pen to suck the ITO conductive substrate coated with the hole transport layer, and tilt the film on the water surface to avoid bubbles. After cutting the film at the edge, lift the substrate at an angle. This process can be repeated multiple times to avoid material waste. After transfer printing, place the device on a hot stage and anneal at 80°C for 2 min.

[0052] 7) Spin coating of electron transport layer. Spin coating of ZnO solution, the spin coating conditions are dynamic coating, 4 krpm, 30 s; spin coating of PEIE solution, PEIE solution is obtained by dissolving PEIE in ethylene glycol monomethyl ether, the concentration is 0.5 wt%, the spin coating conditions are dynamic coating, 3 krpm, 30 s; the total film thickness is 20 nm.

[0053] 8) Place the prepared film substrate in a vacuum chamber and evacuate the chamber to a vacuum level as low as 5×10 -4 Pa, Ag electrode was evaporated on the upper surface of the electron transport layer with an evaporation rate of 0.5 Å / s and a film thickness of 60 nm.

[0054] The JV curve of the organic solar cell in Example 2 is as follows: Figure 4 As shown, the corresponding open circuit voltage ( V OC )、Short circuit current density( J SC ), fill factor (FF), and photoelectric conversion efficiency (PCE) values ​​are shown in Table 1. The results show that the best power conversion efficiency of organic solar cells prepared by PM6:Y6 thin films doped with 2 vt% PNIPAM is 15.2%. In addition, under the condition of doping with 2 vt% PNIPAM, the thickness of the film formed after the spontaneous diffusion of the droplets is the most uniform, and the film presents an interpenetrating network with a smoother surface, which is conducive to charge transfer, and the corresponding organic solar cell has a higher fill factor.

[0055] Table 1 JV curve values ​​of Example 2

[0056] Example 3 [Polysorbate 20 (Polysorbate 20, Tween 20)]: The other steps of Example 3 are the same as those of Example 1, except that 20 mg of Tween20 is accurately weighed and then 1 mL of chloroform is added and shaken to mix; before use, 1 µL of Tween20 solution is added to each 100 µL of PM6:Y6 solution to obtain a mixed solution with a Tween20 doping ratio of 1 vt%. Subsequently, a PM6:Y6 film is prepared using a self-dispersive film-forming process, and after the PM6:Y6 droplets are doped with Tween20, they can diffuse into a uniform film.

[0057] In Example 3, the PM6:Y6 film prepared by the spontaneous diffusion film forming process is applied to an organic solar cell. The specific steps are the same as those in Example 2, except that in step (2), 20 mg of Tween20 is accurately weighed and then 1 mL of chloroform is added and shaken to mix. In the comparative example, the doping ratio of Tween20 is optimized. The specific steps are as follows: 0.1, 0.5, 1, and 2 µL of Tween20 solution are added to each 100 µL of PM6:Y6 solution, and after stirring at room temperature for 10 min, a photoactive layer solution with a Tween doping ratio of 0.1, 0.5, 1, and 2 vt% is obtained, which corresponds to Comparative Examples 2-1, 2-2, 2-3, and 2-4, respectively.

[0058] The JV curve of the organic solar cell in Example 3 is as follows: Figure 5 As shown, the corresponding open circuit voltage ( V OC )、Short circuit current density( J SC ), fill factor (FF), and photoelectric conversion efficiency (PCE) values ​​are shown in Table 2. The results show that the optimal power conversion efficiency of organic solar cells prepared by PM6:Y6 doped with 0.5 vt% and 1 vt% Tween20 is 14.4%.

[0059] Table 2 JV curve values ​​of Example 3

[0060] Example 4 [Poloxamer F127 (Pluronic F127, PF127)]: The other steps of Example 4 are the same as those of Example 1, except that 20 mg of PF127 is accurately weighed and then 1 mL of chloroform is added and shaken to mix; before use, 1 µL of PF127 solution is added to each 100 µL of PM6:Y6 solution to obtain a mixed solution with a PF127 doping ratio of 1 vt%. Subsequently, a PM6:Y6 thin film is prepared using a self-dispersive film-forming process, and after the PM6:Y6 droplets are doped with PF127, they can diffuse into a uniform thin film.

[0061] In Example 4, the PM6:Y6 film prepared by the spontaneous diffusion film forming process is applied to an organic solar cell. The specific steps are the same as those in Example 2, except that in step (2), 20 mg of PF127 is accurately weighed and then 1 mL of chloroform is added and shaken to mix. In the comparative example, the doping ratio of PF127 is optimized. The specific steps are as follows: 0.1, 0.5, 1, and 2 µL of PF127 solution are added to each 100 µL of PM6:Y6 solution, and after stirring at room temperature for 10 min, photoactive layer solutions with PF127 doping ratios of 0.1, 0.5, 1, and 2 vt% are obtained, which correspond to comparative examples 3-1, 3-2, 3-3, and 3-4, respectively.

[0062] The JV curve of the organic solar cell in Example 4 is as follows: Figure 6 As shown, the corresponding open circuit voltage ( V OC )、Short circuit current density( J SC ), fill factor (FF), and photoelectric conversion efficiency (PCE) values ​​are shown in Table 3. The results show that the best power conversion efficiency of organic solar cells prepared by PM6:Y6 doped with 0.5 vt% PF127 is 14.9%.

[0063] Table 3 JV curve values ​​of Example 4

[0064] The results of Examples 1-4 show that PM6:Y6 cannot form a uniform spontaneous diffusion film in a chloroform system; however, the doping of amphiphilic polymers such as PNIPAM, Tween20, and PF127 can promote the spontaneous diffusion of droplets. High-quality PM6:Y6 photoactive layers with different doping systems were successfully prepared using the spontaneous diffusion film-forming process and applied to organic solar cells.

[0065] In one embodiment, Figure 7 As shown, in order to further improve the utilization rate of the photoactive material, the preparation method 200 provided in the present disclosure further includes steps S250 to S280.

[0066] S250, scraping the photoactive layer film remaining on the liquid surface with a scraper.

[0067] S260, using the active layer solvent to clean the scraper, transferring the cleaned solution to a container, and drying to obtain a solid mixture of the polymer donor, the small molecule receptor and the amphiphilic additive.

[0068] S270, re-dissolving the recovered solid mixture into a corresponding volume of the active layer solvent to obtain the photoactive layer organic solution again.

[0069] S280, dropping the photoactive layer organic solution onto the liquid surface of the active layer solvent, so that the organic solution diffuses spontaneously on the liquid surface to form the photoactive layer thin film.

[0070] For example, a scraper can be used to pass over the water surface, and all PM6:Y6 film fragments scattered on the water surface after transfer can be collected on the plate surface; the scraper can be cleaned with chloroform, and the cleaned solution can be collected into a sample bottle, and the sample bottle can be placed in an oven and dried at 100°C for 2 hours to evaporate the chloroform and the small amount of residual water to obtain a mixed solid of PM6 and Y6. This process does not involve the separation of donors, acceptors, and additives, and does not involve any purification or filtration operations; the recovered solid PM6:Y6 is accurately weighed, and the corresponding volume of chloroform is added to dissolve it, and a PM6:Y6 solution with an accurate concentration is prepared; the recovered solid object contains PM6, Y6, and additives at the same time, and there is no need to re-dope the amphiphilic polymer during the re-dissolution process. After only adding chloroform to dissolve, a spontaneously diffusing photoactive layer film can be directly formed on the water surface.

[0071] By repeating the above steps S250 to S280 in a loop, waste of photoactive layer materials can be effectively avoided.

[0072] Compared with the prior art, the present disclosure provides a method for spontaneous diffusion film formation and recycling of the photoactive layer of an organic solar cell, including the steps of film formation, transfer, collection, cleaning, dissolution, etc. By repeating these steps, the spontaneous diffusion film formation and recycling and reuse of the photoactive layer in the chloroform system can be achieved. In the process of spontaneous diffusion of droplets, by doping amphiphilic additives into the photoactive layer material, the interfacial tension between the droplets and the liquid surface of the culture medium solvent can be regulated, thereby promoting the uniformity of the liquid surface film. The photoactive layer prepared by the spontaneous diffusion film formation method in an atmospheric environment is used to prepare an organic solar cell, which can reduce the complexity of the device process and effectively avoid the waste of the photoactive layer material.

[0073] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of disclosure involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the above disclosed concept. For example, the above features are replaced with the technical features with similar functions disclosed in this application (but not limited to) by each other to form a technical solution.

[0074] In addition, although each operation is described in a specific order, this should not be construed as requiring these operations to be performed in the specific order shown or in a sequential order. Under certain circumstances, multitasking and parallel processing may be advantageous. Similarly, although some specific implementation details are included in the above discussion, these should not be construed as limiting the scope of the present invention. Some features described in the context of a separate embodiment can also be implemented in a single embodiment in combination. On the contrary, the various features described in the context of a single embodiment can also be implemented in multiple embodiments individually or in any suitable sub-combination mode.

[0075] Although the subject matter has been described in language specific to structural features and / or methodological logical actions, it should be understood that the subject matter defined in the appended claims is not necessarily limited to the specific features or actions described above. On the contrary, the specific features and actions described above are merely example forms of implementing the claims.

[0076] Several embodiments of the present application have been described in detail above, but the present application is not limited to these specific embodiments. Those skilled in the art can make various variations and modifications to the embodiments based on the concept of the present application, and these variations and modifications should all fall within the scope of protection claimed by the present application.

Claims

1. A method for preparing a photoactive layer film, wherein the photoactive layer film is used for an organic solar cell, It is characterized in that The preparation method comprises the following steps: The polymer donor and the small molecule acceptor are mixed and dissolved in an active layer solvent to form a first precursor solution; dissolving the amphiphilic additive into the active layer solvent to form a second precursor solution; mixing the second precursor solution and the first precursor solution in a predetermined volume ratio to obtain a photoactive layer organic solution doped with the amphiphilic additive; and Pipetting a drop of the photoactive layer organic solution into an open container containing a culture medium solvent, so that the droplet spontaneously diffuses on the liquid surface of the culture medium solvent to form a uniform photoactive layer film; Wherein, the boiling point of the material of the active layer solvent is lower than the boiling point of the culture medium solvent, and the surface tension of the active layer solvent is lower than the surface tension of the culture medium solvent; The material of the amphiphilic additive is selected so as to be able to interact with the culture medium solvent to promote the spreading of the droplets on the liquid surface, and to interact with the active layer solvent to promote the continuity of the photoactive layer film.

2. The preparation method according to claim 1, It is characterized in that The active layer solvent is any one or more combinations of chloroform, dichloromethane, 2-methyltetrahydrofuran and tetrahydrofuran.

3. The preparation method according to claim 2, It is characterized in that The culture medium solvent is any one or more combinations of pure water, imidazole ionic liquids, pyridine ionic liquids, quaternary ammonium salt ionic liquids, perfluorooctane sulfonic acid and fluorocarbon compounds.

4. The preparation method according to claim 3, It is characterized in that The amphiphilic additive includes poly (N-isopropylacrylamide), polysorbate 20 or poloxamer F127.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The blend of the polymer donor and the small molecule acceptor includes PM6:Y6, PM6:BTP-eC9, PM6:Y6:PCBM or PM6:BTP-eC9:PCBM.

6. The preparation method according to any one of claims 1 to 4, It is characterized in that When the active layer solvent is chloroform and the culture medium solvent is pure water, the concentration of the first precursor solution is 5 mg / mL, the concentration of the second precursor solution is 20 mg / mL, and the predetermined volume ratio is 0.1% to 10%.

7. The preparation method according to claim 6, It is characterized in that The predetermined volume ratio is 1%.

8. An organic solar cell, It is characterized in that It includes a transparent conductive substrate layer, a hole transport layer, a photoactive layer, an electron transport layer and a top electrode layer; Wherein, the photoactive layer is obtained by using the photoactive layer thin film prepared by the preparation method according to any one of claims 1 to 7; Wherein, the material of the transparent conductive substrate layer is selected from any one of ITO, FTO, AZO, GZO conductive glass, metal nanowire substrate and highly transparent metal film substrate; The material of the hole transport layer is aqueous PEDOT:PSS or MoO 3 ; The material of the electron transport layer is a combination of ZnO and PEIE; The material of the top electrode layer is selected from any one of Ag, Au, Al and Pt.

9. A method for preparing an organic solar cell, It is characterized in that The following steps are involved: forming one of a hole transport layer and an electron transport layer on the transparent conductive substrate layer to obtain an intermediate substrate; The photoactive layer film is obtained by the preparation method according to any one of claims 1 to 7; The photoactive layer film is subjected to transfer processing: the intermediate substrate is sucked by a vacuum pen, and the photoactive layer film is obliquely pressed onto the liquid surface of the culture medium solvent, the film at the edge is divided, and the intermediate substrate printed with the photoactive layer film is obliquely lifted, and annealed to form the photoactive layer; as well as The other of the hole transport layer and the electron transport layer, and a top electrode layer are sequentially formed above the photoactive layer.

10. The preparation method according to claim 9, It is characterized in that The preparation method further comprises: Using a scraper to scrape off the photoactive layer film remaining on the liquid surface; The scraper is cleaned with the active layer solvent, the cleaned solution is transferred to a container, and a solid mixture of the polymer donor, the small molecule receptor and the amphiphilic additive is obtained after drying; re-dissolving the recovered solid mixture into a corresponding volume of the active layer solvent to obtain the photoactive layer organic solution again; and The photoactive layer organic solution is dropped onto the liquid surface of the active layer solvent so as to be spontaneously diffused on the liquid surface to form the photoactive layer thin film.

Citation Information

Patent Citations

  • Liquid composition for deposition of organic electroactive materials

    CN103262278A

  • Method for preparation of quick dissolving thin films containing bioactive material with enhanced thermal stability

    CN109475508A

  • Efficient organic solar cell and preparation method thereof

    CN111584718A

  • Organic solar cell produced by spontaneous orientation film forming method and production method thereof

    CN113644202A

  • Rapid, large volume, dead layer-free 3D printing

    CN113727828A