High polymer material for powder puff and preparation method thereof
By forming the front of the texture or protrusion or fluff on the surface of the puff material, combined with the optimization of the permeable template and peeling liquid, the problem of irregular and insufficient softness of the existing puff material is solved, and the regular surface and goodness of the polymer material are achieved The sense of use.
Patent Information
- Application Number
- CN202411589102.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-08
- Publication Date
- 2024-12-06
AI Technical Summary
The surface of the existing puff material is difficult to form a regular surface during foaming, and the softness is insufficient, resulting in poor use.
The foam layer resin is coated and cured with a water-permeable template to form a front surface with patterns or protrusions or fluffs. The peeling strength and material combination are optimized through the peeling liquid to ensure the surface is integrally formed and regular.
The regular surface of the puff material is realized, the softness and mechanical properties are improved, the weather resistance is enhanced, and the user experience is provided.
Smart Images

Figure CN119081394A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymers, and more particularly to a polymer material for a powder puff. Background Art
[0002] A powder puff is a kind of makeup tool. Generally, loose powder and powder compact boxes contain a powder puff, which is used to pick up foundation and modify makeup. In the prior art, powder puffs are generally made of sponge material. The sponge material powder puff is generally soft, but delicate, and has a poor texture, and is gradually being eliminated. Now a powder puff made of polyurethane foam material has been developed. The polyurethane powder puff is mainly coated on the outer layer of the sponge, and the outer layer is used to pick up powder and modify makeup. However, during the foaming process of the polyurethane foam material, the surface is randomly foamed, and it is difficult to form a regular surface. The softness is not ideal, which makes the feeling when using it poor. Summary of the invention
[0003] In view of the shortcomings of the prior art, the object of the present invention is to provide a polymer material for a powder puff.
[0004] To achieve the above object, the present invention provides the following technical solutions: A polymer material for powder puffs. The invention comprises a foaming layer, wherein the foaming layer has a front side and a back side, the front side has lines, bulges or villi, and the lines, bulges or villi are integrally formed with the foaming layer.
[0005] As another object of the present invention, a method for preparing a polymer material for a powder puff is provided. The method comprises the following steps: Step 1: Take the permeable template, cover one side of the permeable template with a stripping liquid and dry it; Step 2: prepare a foaming layer resin, apply the foaming layer resin on the side of the permeable template covered with the stripping liquid, place it in a solidification tank for solidification, and wash and dry it after solidification to obtain a substrate; Step 3: Tear off the water-permeable template on the back of the substrate to obtain the polymer material.
[0006] As a further improvement of the present invention, The stripping solution is an organic silicon or organic fluorine solution.
[0007] As a further improvement of the present invention, The step 1 is specifically as follows: The permeable template is immersed in the stripping liquid, and then taken out to complete the covering of the permeable template; or The step 1 specifically comprises: coating one side of the permeable template with a layer of stripping liquid; or The step 1 specifically comprises: spraying a stripping liquid on one side of the permeable template.
[0008] As a further improvement of the present invention, The foaming resin in step 2 comprises: Solvents, polyurethane resins, water-soluble bio-based powders.
[0009] As a further improvement of the present invention, The water-soluble bio-based powder is cyclodextrin, English gum, white dextrin, maltodextrin and yellow dextrin.
[0010] As a further improvement of the present invention, The water-soluble bio-based powder absorbs 50% to 200% of its own weight of water to swell, and absorbs more than 100% to 400% of its own weight of water to dissolve.
[0011] As a further improvement of the present invention, The solvent is DMF.
[0012] As a further improvement of the present invention, The mass ratio of the polyurethane resin to the water-soluble bio-based powder is 20-40:30-150.
[0013] As a further improvement of the present invention, The permeable template is Textured base fabric or Base fabric with fleece or Permeable polymer template Or a water-permeable polymer template with holes.
[0014] As a further improvement of the present invention, the peeling force between the back side of the substrate and the water-permeable template is controlled at 0.2-0.5 N / cm.
[0015] The beneficial effect of the present invention is that the present invention mainly forms a front side with lines, protrusions or fluff on the surface of the foaming material through an intermediary, and integrally forms it, so that the powder puff material has a regular front side, and the front side is used for powdering and contacting the human body, so there is no need to post-process the powder puff material to obtain a regular surface.
[0016] In the present invention, the surface regularity of the foamed material is mainly achieved through the permeable template. The foamed material is coated on the permeable template. After the foaming is completed, the side that fits the permeable template will be printed with regular patterns. For example, when the permeable template uses a plain woven base cloth, the front side will be a plain woven checkered pattern. When a fluffy base cloth is selected, there will be a fluffy surface. The surface of the polymer material produced in this way will be easier to control.
[0017] In actual use, we found that sometimes when the peeling strength between the permeable template and the foam material is high, the front side of the foam layer will be damaged when peeling the permeable template. At this time, we found that covering the permeable template with peeling liquid first will make it easier to peel off the permeable template without damaging the front texture.
[0018] The stripping solution is preferably an organic fluorine or organic silicon solution with a mass fraction of 0.2% to 0.5%. If the stripping strength is too small, the water-permeable template will detach during the foaming process.
[0019] Polyurethane material is preferred in the selection of foaming materials, and in the preferred embodiment of the present invention, polyurethane resin, solvent, and soluble bio-based powder are mixed and used. The addition of soluble bio-based powder can obtain dense bubbles, and in the subsequent water washing process, the bubbles can be directly washed out, and have better mechanical properties and weather resistance while maintaining good softness. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the overall structure of the polymer material according to an embodiment of the present invention.
[0021] Figure numerals: 1, front; 2, back. DETAILED DESCRIPTION Example
[0022] Step 1: Take a plain woven base fabric, soak the plain woven base fabric in a stripping solution and dry it, the stripping solution is a 0.3% organic fluorine aqueous solution; Step 2: Prepare the resin mixture: Take weight parts: Polyurethane resin with 30% solid content: 100 parts Wood powder: 40 parts DMF: 140 parts. Take appropriate weight portions of DMF to make the viscosity of the resin mixture at about 5000 cps, which is a suitable coating viscosity.
[0023] The polyurethane resin, DMF and yellow dextrin powder are stirred and mixed to obtain a resin mixture.
[0024] The resin mixture is applied to the front of the permeable template, placed in a solidification tank for solidification, and washed and dried after solidification to obtain the base material; Step 3: Peel off the substrate and the plain woven base fabric to obtain the polymer material.
[0025] The polymer material comprises a foaming layer, the foaming layer has a front side and a back side, the front side has a plain woven base fabric pattern, and the plain woven base fabric pattern is integrally formed with the foaming layer. Example
[0026] Step 1: Take a plain woven base fabric, soak the plain woven base fabric in a stripping solution and dry it, the stripping solution is a 0.3% organic fluorine aqueous solution; Step 2: Prepare the resin mixture: Take weight parts: Polyurethane resin with 30% solid content: 100 parts Yellow dextrin powder: 120 parts DMF: 140 parts. Take appropriate weight portions of DMF to make the viscosity of the resin mixture at about 5000 cps, which is a suitable coating viscosity.
[0027] The yellow dextrin powder has been tested and it has been found that 1 part of yellow dextrin can absorb 1 part of water by weight during the swelling stage and can dissolve after absorbing 2 parts of water.
[0028] The polyurethane resin, DMF and yellow dextrin powder are stirred and mixed to obtain a resin mixture.
[0029] The resin mixture is applied to the front of the permeable template, placed in a solidification tank for solidification, and washed and dried after solidification to obtain the base material; Step 3: Peel off the substrate and the plain woven base fabric to obtain the polymer material.
[0030] The polymer material comprises a foaming layer, the foaming layer has a front side and a back side, the front side has a plain woven base fabric pattern, and the plain woven base fabric pattern is integrally formed with the foaming layer. Example
[0031] Step 1: Take a plain woven base fabric, soak the plain woven base fabric in a stripping solution and dry it, the stripping solution is a 0.3% organic fluorine aqueous solution; Step 2: Prepare the resin mixture: Take weight parts: Polyurethane resin with solid content of 28-32%: 100 parts Calcium powder: 20 parts Yellow dextrin powder: 120 parts DMF: 140 parts. Take appropriate weight portions of DMF to make the viscosity of the resin mixture at about 5000 cps, which is a suitable coating viscosity.
[0032] The yellow dextrin powder has been tested and it has been found that 1 part of yellow dextrin can absorb 1 part of water by weight during the swelling stage and can dissolve after absorbing 2 parts of water.
[0033] The polyurethane resin, DMF and yellow dextrin powder are stirred and mixed to obtain a resin mixture.
[0034] The resin mixture is applied to the front of the permeable template, placed in a solidification tank for solidification, and washed and dried after solidification to obtain the base material; Step 3: Peel off the substrate and the plain woven base fabric to obtain the polymer material.
[0035] The polymer material comprises a foaming layer, the foaming layer has a front side and a back side, the front side has a plain woven base fabric pattern, and the plain woven base fabric pattern is integrally formed with the foaming layer. Example
[0036] Step 1: Take a fluff base fabric, spray a stripping solution on one side of the plain woven base fabric and dry it. The stripping solution is a 0.3% silicone aqueous solution; Step 2: Prepare the resin mixture: Take weight parts: Polyurethane resin with 30% solid content: 100 parts Yellow dextrin powder: 120 parts DMF: 140 parts. Take appropriate weight portions of DMF to make the viscosity of the resin mixture at about 5000 cps, which is a suitable coating viscosity.
[0037] The yellow dextrin powder has been tested and it has been found that 1 part of yellow dextrin can absorb 1 part of water by weight during the swelling stage and can dissolve after absorbing 2 parts of water.
[0038] The polyurethane resin, DMF and yellow dextrin powder are stirred and mixed to obtain a resin mixture.
[0039] The resin mixture is applied to the front of the permeable template, placed in a solidification tank for solidification, and washed and dried after solidification to obtain the base material; Step 3: Peel off the substrate and the plain woven base fabric to obtain the polymer material.
[0040] The polymer material comprises a foaming layer, the foaming layer has a front side and a back side, the front side has a plain woven base fabric pattern, and the plain woven base fabric pattern is integrally formed with the foaming layer.
[0041] Comparative Example 1: Step 1: Take the plain woven base fabric. Step 2: Prepare the resin mixture: Take weight parts: Polyurethane resin with 30% solid content: 100 parts Wood powder: 40 parts DMF: 140 parts. Take appropriate weight portions of DMF to make the viscosity of the resin mixture at about 5000 cps, which is a suitable coating viscosity.
[0042] The polyurethane resin, DMF and yellow dextrin powder are stirred and mixed to obtain a resin mixture.
[0043] The resin mixture is applied to the front of the permeable template, placed in a solidification tank for solidification, and washed and dried after solidification to obtain the base material; Step 3: Peel off the substrate and the plain woven base fabric to obtain the polymer material.
[0044] Ingredients:
[0045] Contrast effect: test: 1. Peel strength test: GB / T 2791-1995 2. Softness test: GB / T 39371-2020 3. Tear strength: GB / T10808-2006
[0046] Examples 1 to 4 adopt a process of first covering the permeable template with a release agent, wherein the peel strength test is the peel strength between the substrate and the base fabric, so that the peel strength is greatly reduced compared with the control example, and the permeable template can be kept from detaching during the foaming process.
[0047] In terms of softness, Examples 2, 3, and 4 are also greatly improved compared to Example 1, and the tear strength is also greatly improved, indicating that the addition of yellow dextrin improves the softness while also ensuring the tear strength compared to wood powder. And the weather resistance is improved, because wood powder is easy to rot and deteriorate, and cannot be washed out during the washing process, which leads to the problem of poor weather resistance. The powder puff polymer material of the present invention has a very soft, delicate, and skin-friendly effect, and has a good comfortable experience when applying powder on the face, and is a very good high-end powder puff material.
[0048] The beneficial effect of the present invention is that the present invention mainly forms a front side with lines, protrusions or fluff on the surface of the foaming material through an intermediary, and integrally forms it, so that the powder puff material has a regular front side, and the front side is used for powdering and contacting the human body, so there is no need to post-process the powder puff material to obtain a regular surface.
[0049] In the present invention, the surface regularity of the foamed material is mainly achieved through the permeable template. The foamed material is coated on the permeable template. After the foaming is completed, the side that fits the permeable template will be printed with regular patterns. For example, when the permeable template uses a plain woven base cloth, the front side will be a plain woven checkered pattern. When a fluffy base cloth is selected, there will be a fluffy surface. The surface of the polymer material produced in this way will be easier to control.
[0050] In actual use, we found that sometimes when the peeling strength between the permeable template and the foam material is high, the front side of the foam layer will be damaged when peeling the permeable template. At this time, we found that covering the permeable template with peeling liquid first will make it easier to peel off the permeable template without damaging the front texture.
[0051] The stripping solution is preferably an organic fluorine or organic silicon solution with a mass fraction of 0.2% to 0.5%. If the stripping strength is too small, the water-permeable template will detach during the foaming process.
[0052] Polyurethane material is preferred in the selection of foaming materials, and in the preferred embodiment of the present invention, polyurethane resin, solvent, and soluble bio-based powder are mixed and used. The addition of soluble bio-based powder can obtain dense bubbles, and in the subsequent water washing process, the bubbles can be directly washed out, and have better mechanical properties and weather resistance while maintaining good softness.
[0053] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A polymer material for a powder puff, characterized in that: It comprises a foaming layer (1), the foaming layer having a front side (2) and a back side (3), the front side having lines or protrusions or fluff, and the lines or protrusions or fluff are integrally formed with the foaming layer.
2. A method for preparing a polymer material for a powder puff, Features: The method comprises the following steps: Step 1: Take the permeable template, cover the permeable template with stripping liquid and dry it; Step 2: prepare a resin mixture, apply the resin mixture on a permeable template, place it in a solidification tank for solidification, and wash and dry it after solidification to obtain a base material; Step 3: Peeling off the substrate and the water-permeable template to obtain a polymer material.
3. The method for preparing a polymer material for a powder puff according to claim 2, characterized in that: The stripping solution is an organic silicon or organic fluorine solution.
4. The method for preparing a polymer material for a powder puff according to claim 2, characterized in that: The step 1 is specifically as follows: The permeable template is immersed in the stripping liquid, and then taken out to complete the covering of the permeable template; or The step 1 specifically comprises: coating one side of the permeable template with a layer of stripping liquid; or The step 1 specifically comprises: spraying a stripping liquid on one side of the permeable template.
5. The method for preparing a polymer material for a powder puff according to claim 2, characterized in that: The foaming resin in step 2 comprises: Solvents, polyurethane resins, water-soluble bio-based powders.
6. The method for preparing a polymer material for a powder puff according to claim 5, characterized in that: The water-soluble bio-based powder is cyclodextrin, English gum, white dextrin, maltodextrin and yellow dextrin.
7. The method for preparing a polymer material for a powder puff according to claim 5, characterized in that: The water-soluble bio-based powder absorbs 50% to 200% of its own weight of water to swell, and absorbs more than 100% to 400% of its own weight of water to dissolve.
8. The method for preparing a polymer material for a powder puff according to claim 5, characterized in that: The solvent is DMF.
9. The method for preparing a polymer material for a powder puff according to claim 5, characterized in that: The mass ratio of the polyurethane resin to the water-soluble bio-based powder is 20-40:30-150.
10. The method for preparing a polymer material for a powder puff according to claim 2, characterized in that: The permeable template is Non-textured fabric or Textured base fabric or Base fabric with fleece or Permeable polymer template Or a water-permeable polymer template with holes.
11. The method for preparing a polymer material for a powder puff according to claim 2, characterized in that: The peeling strength between the back of the substrate and the permeable template is controlled at 0.2-0.5N / cm.
Citation Information
Patent Citations
Novel waterproof air previous polyurethane artificial leather and preparation thereof
CN101440578A
Ultra-soft protein synthetic leather and preparing method thereof
CN106436342A
Manufacture method of stripping leather for soft air cushion powder puffs
CN106436345A
Method for continuously manufacturing sponge sheet for powder puff
CN107428976A
High-durability antibacterial and anti-mildew polyurethane synthetic leather and preparation method thereof
CN111501372A