SBS modified asphalt and preparation method thereof

By using a combination of linear styrene-butadiene-styrene block copolymer, furfural extracted oil and sulfur-containing stabilizer in SBS modified asphalt, the preparation process is optimized, and the insufficient performance of SBS modified asphalt at high and low temperatures is solved. The problem of this problem has achieved the effect of small dosage of modifier, short production cycle and excellent performance, and is suitable for road construction.

CN119081431APending Publication Date: 2024-12-06CHAMBROAD (HAINAN) ADVANCED MATERIAL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411369877.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing SBS modified asphalt has insufficient performance under high and low temperature conditions, making it difficult to meet the market's demand for better performance. At the same time, the modifier is used in large quantities, long production cycles, and poor economic performance.

Method used

Linear styrene-butadiene-styrene block copolymer is used as SBS modifier, combined with furfural extracted oil and sulfur-containing stabilizer, and SBS modified asphalt is prepared by heating premix, shear mixing and stirring development. Optimize the composition of the component to improve its physical and chemical stability over a wide temperature range.

Benefits of technology

It achieves excellent performance of SBS modified asphalt under high and low temperature conditions. It has small dosage of modifiers, short production cycle, good economy, suitable for industrial production, and meets high and low temperature performance requirements that even exceed industry standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005067295360000021
    Figure BDA0005067295360000021
  • Figure BDA0005067295360000022
    Figure BDA0005067295360000022
  • Figure BDA0005067295360000031
    Figure BDA0005067295360000031
Patent Text Reader

Abstract

The invention belongs to the field of petrochemical engineering, and particularly relates to SBS modified asphalt and a preparation method thereof. The SBS modified asphalt provided by the invention comprises the following components in parts by mass: 100 parts of matrix asphalt, 4-5 parts of an SBS modifier, 1-2 parts of a compatilizer and 0.2-0.3 part of a stabilizer, the SBS modifier is a linear styrene-butadiene-styrene block copolymer, and the mass ratio of a polystyrene chain segment to a polybutadiene chain segment in the copolymer is 30: 70; the compatilizer is furfural extract oil; the stabilizer is a sulfur-containing stabilizer. The composition of the SBS modified asphalt is optimally designed, and particularly, the specific SBS modifier is selected, so that the SBS modified asphalt can show excellent performance under high-temperature and low-temperature conditions, and can meet the use requirements under different weather conditions; and the SBS modified asphalt is small in modifier dosage, short in production period and good in economical efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of petrochemical industry, and in particular relates to an SBS modified asphalt and a preparation method thereof. Background Art

[0002] With the rapid development of my country's economy, highway transportation construction has also made remarkable achievements. Asphalt is an indispensable material in highway construction, and its performance directly affects the quality and service life of the highway. However, due to various complex environmental conditions and traffic loads, asphalt materials face many challenges, such as fatigue cracks, rutting, low-temperature cracks, etc. In order to improve the performance of asphalt materials, modified asphalt technology came into being, among which the use of styrene-butadiene-styrene block copolymer (SBS) modified asphalt has been widely studied and applied.

[0003] SBS is a thermoplastic elastomer with good chemical stability and mechanical properties. SBS has a two-phase structure, styrene is the dispersed phase, which is incompatible with each other and is in a phase-separated state, forming a high-strength physical crosslink; while butadiene is the continuous phase, which provides SBS modified asphalt with good elongation and viscoelasticity. By adding SBS copolymers to asphalt, a three-dimensional network structure is formed, thereby enhancing the viscosity of asphalt. SBS modified asphalt has high temperature resistance, low temperature resistance and rutting resistance, which has a significant effect on extending the service life of roads.

[0004] With the rapid development of SBS modified asphalt technology, the market has put forward higher and higher requirements on the performance of SBS modified asphalt. How to make SBS modified asphalt take into account better high and low temperature performance has become a research hotspot in this field. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an SBS modified asphalt and a preparation method thereof. The SBS modified asphalt provided by the present invention exhibits excellent performance under both high and low temperature conditions and can adapt to the use requirements under different climatic conditions; and the SBS modified asphalt has a small amount of modifier used, a short production cycle, and good economy.

[0006] The present invention provides an SBS modified asphalt, wherein the components of the SBS modified asphalt include, by weight:

[0007]

[0008] The SBS modifier is a linear styrene-butadiene-styrene block copolymer, and the mass ratio of the polystyrene segment to the polybutadiene segment in the copolymer is 30:70;

[0009] The compatibilizer is furfural extracted oil;

[0010] The stabilizer is a sulfur-containing stabilizer.

[0011] Preferably, the base asphalt is 70#A grade road petroleum asphalt.

[0012] Preferably, the number average molecular weight of the linear styrene-butadiene-styrene block copolymer is 80,000 to 120,000.

[0013] Preferably, the kinematic viscosity of the furfural extracted oil at 40° C. is 35 to 40 Pa·s.

[0014] Preferably, the sulfur content of the sulfur-containing stabilizer is ≥ 99 wt %.

[0015] Preferably, the components of the SBS modified asphalt include, by weight:

[0016]

[0017] The present invention provides a method for preparing the SBS modified asphalt described in the above technical solution, comprising the following steps:

[0018] The base asphalt, SBS modifier, compatibilizer and stabilizer are mixed to obtain SBS modified asphalt.

[0019] Preferably, the mixing process specifically includes:

[0020] a) premixing the base asphalt and the SBS modifier by heating, and then shearing and mixing to obtain an asphalt mixture;

[0021] b) mixing the asphalt mixture, compatibilizer and stabilizer, stirring and growing to obtain SBS modified asphalt.

[0022] Preferably, in step a), the temperature of the heated premix is ​​120-160° C.; the temperature of the shear mixing is 180-200° C., the shear speed of the shear mixing is 2000-4500 r / min, and the time of the shear mixing is 30-60 min.

[0023] Preferably, in step b), the stirring and developing temperature is 180-190° C., the stirring and developing speed is 600-1000 r / min, and the stirring and developing time is 3-6 h.

[0024] Compared with the prior art, the present invention provides an SBS modified asphalt and a preparation method thereof. In terms of mass fractions, the components of the SBS modified asphalt provided by the present invention include: 100 parts of base asphalt, 4 to 5 parts of SBS modifier, 1 to 2 parts of compatibilizer, and 0.2 to 0.3 parts of stabilizer; the SBS modifier is a linear styrene-butadiene-styrene block copolymer, and the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 30:70; the compatibilizer is furfural extracted oil; and the stabilizer is a sulfur-containing stabilizer. The present invention optimizes the composition of the SBS modified asphalt, especially by selecting a specific SBS modifier, so that the SBS modified asphalt can exhibit excellent physical and chemical stability in a wide temperature range, and at the same time has excellent high and low temperature performance. In addition, the amount of modifier used in the SBS modified asphalt is small, the development time during preparation is short, it has good economic benefits, and is suitable for industrial production. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] The present invention provides an SBS modified asphalt, wherein the components of the SBS modified asphalt include, by weight:

[0027]

[0028] In the modified asphalt provided by the present invention, the base asphalt is preferably 70#A grade road petroleum asphalt.

[0029] In the modified asphalt provided by the present invention, the SBS modifier is a linear styrene-butadiene-styrene block copolymer, and the mass ratio of the polystyrene segment to the polybutadiene segment in the copolymer is 30:70; the number average molecular weight of the linear styrene-butadiene-styrene block copolymer is preferably 80,000 to 120,000.

[0030] In the modified asphalt provided by the present invention, based on the content of base asphalt in the modified asphalt as 100 parts by mass, the content of the SBS modifier in the modified asphalt can specifically be 4 parts by mass, 4.1 parts by mass, 4.2 parts by mass, 4.3 parts by mass, 4.4 parts by mass, 4.5 parts by mass, 4.6 parts by mass, 4.7 parts by mass, 4.8 parts by mass, 4.9 parts by mass or 5 parts by mass.

[0031] In the modified asphalt provided by the present invention, the compatibilizer is furfural extracted oil; the kinematic viscosity of the furfural extracted oil at 40°C is preferably 35-40 Pa·s, specifically 35 Pa·s, 35.5 Pa·s, 36 Pa·s, 36.5 Pa·s, 37 Pa·s, 37.5 Pa·s, 38 Pa·s, 38.5 Pa·s, 39 Pa·s, 39.5 Pa·s or 40 Pa·s.

[0032] In the modified asphalt provided by the present invention, based on the content of base asphalt in the modified asphalt as 100 parts by mass, the content of the compatibilizer in the modified asphalt may specifically be 1 part by mass, 1.1 parts by mass, 1.2 parts by mass, 1.3 parts by mass, 1.4 parts by mass, 1.5 parts by mass, 1.6 parts by mass, 1.7 parts by mass, 1.8 parts by mass, 1.9 parts by mass or 2 parts by mass.

[0033] In the modified asphalt provided by the present invention, the stabilizer is a sulfur-containing stabilizer; the sulfur content of the sulfur-containing stabilizer is preferably ≥99wt%.

[0034] In the modified asphalt provided by the present invention, based on the content of base asphalt in the modified asphalt as 100 parts by mass, the content of the stabilizer in the modified asphalt may specifically be 0.2 parts by mass, 0.21 parts by mass, 0.22 parts by mass, 0.23 parts by mass, 0.24 parts by mass, 0.25 parts by mass, 0.26 parts by mass, 0.27 parts by mass, 0.28 parts by mass, 0.29 parts by mass or 0.3 parts by mass.

[0035] The present invention provides a method for preparing the SBS modified asphalt described in the above technical solution, comprising the following steps:

[0036] The base asphalt, SBS modifier, compatibilizer and stabilizer are mixed to obtain SBS modified asphalt.

[0037] In the preparation method provided by the present invention, the mixing process specifically includes:

[0038] a) premixing the base asphalt and the SBS modifier by heating, and then shearing and mixing to obtain an asphalt mixture;

[0039] b) mixing the asphalt mixture, compatibilizer and stabilizer, stirring and growing to obtain SBS modified asphalt.

[0040] In the above-mentioned mixing process provided by the present invention, step a) helps to further refine the dispersed phase of the modifier and improve the compatibility with asphalt. In step a), the temperature of the heated premix is ​​preferably 120-160°C, specifically 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C or 160°C; the temperature of the shear mixing is preferably 180-200°C, specifically 180°C, 185°C, 190°C, 195°C or 200°C; the shear speed of the shear mixing is preferably 2000-4500r / min, specifically 2000r / min, 2500r / min, 3000r / min, 3500r / min, 4000r / min or 4500r / min; the shear mixing time is preferably 30-60min, specifically 30min, 35min, 40min, 45min, 50min, 55min or 60min.

[0041] In the above-mentioned mixing process provided by the present invention, step b) helps to further promote the uniformity and stability of the modified asphalt. In step b), the stirring and developing temperature is preferably 180-190°C, specifically 180°C, 185°C or 190°C; the stirring and developing speed is preferably 600-1000r / min, specifically 600r / min, 650r / min, 700r / min, 750r / min, 800r / min, 850r / min, 900r / min, 950r / min or 1000r / min; the stirring and developing time is preferably 3-6h, specifically 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.

[0042] The technical solution provided by the present invention optimizes the composition of SBS modified asphalt, especially by selecting a specific SBS modifier, so that the SBS modified asphalt can exhibit excellent physical and chemical stability in a wide temperature range and have excellent high and low temperature performance. In addition, the amount of modifier used in the SBS modified asphalt is small, the development time during preparation is short, it has good economic benefits, and is suitable for industrial production.

[0043] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.

[0044] Example 1

[0045] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 29.4g of modifier, which is a linear styrene-butadiene-styrene block copolymer, the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 30:70, and the number average molecular weight is 80,000-120,000. Put it on the direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 10.2g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.5g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0046] Example 2

[0047] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 28.2g of modifier, which is a linear styrene-butadiene-styrene block copolymer, the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 30:70, and the number average molecular weight is 80,000-120,000. Put it on the direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 9g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.44g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0048] Example 3

[0049] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 27g of modifier, which is a linear styrene-butadiene-styrene block copolymer, the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 30:70, and the number average molecular weight is 80,000-120,000. Put it on the direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 7.8g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.38g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0050] Comparative Example 1

[0051] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 29.4g of modifier, which is a linear styrene-butadiene-styrene block copolymer, the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 20:80, and the number average molecular weight is 80,000-120,000. Put it on the direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 10.2g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.5g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0052] Comparative Example 2

[0053] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 28.2g of modifier, which is a linear styrene-butadiene-styrene block copolymer, the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 20:80, and the number average molecular weight is 80,000-120,000. Put it on the direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 9g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.44g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0054] Comparative Example 3

[0055] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 29.4g of modifier, which is a linear styrene-butadiene-styrene block copolymer, with a mass ratio of polystyrene segments to polybutadiene segments of 40:60 and a number average molecular weight of 80,000-120,000. Put it on a direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 10.2g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.5g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0056] Comparative Example 4

[0057] Melt 600g of 70#A-grade road petroleum asphalt at 130-140℃, add 28.2g of modifier, which is a linear styrene-butadiene-styrene block copolymer, the mass ratio of polystyrene segments to polybutadiene segments in the copolymer is 40:60, and the number average molecular weight is 80,000-120,000. Put it on the direct heating jacket for heating, and use a glass thermometer to continuously stir the modifier and immerse it in the asphalt during the preheating process. When the temperature rises to about 160℃, put it into the shearing machine for preheating. Turn the shearing machine manually, and when the shearing machine rotates smoothly, turn on the shearing machine, adjust the speed of the shearing machine to 2000r / min, and use a glass rod to stir the modifier on the wall of the cylinder into the cylinder. When the temperature rises to 158-165℃, adjust the speed of the shearing machine to 4500r / min, turn off the heating jacket, use residual heat to heat up, and control the temperature at about 180℃. The shearing time is 50min, and the temperature is controlled at about 180℃ during the process. After the shearing is completed, the cylinder is taken out and 9g of compatibilizer is added. The compatibilizer is furfural extracted oil with a kinematic viscosity of 38Pa·s (40°C). It is placed in a temperature-controlled heating jacket and the control temperature is set at 185°C. When the temperature rises to 173°C, 1.44g of stabilizer is added. The stabilizer contains more than 99wt% sulfur. The timing is started and the stirring speed is adjusted to 600r / min for 4h of development.

[0058] Performance Evaluation

[0059] The performance of the SBS modified asphalt prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was evaluated, and the results are shown in the following table:

[0060]

[0061] Comparison between Example 1 and Comparative Example 1, and between Example 2 and Comparative Example 2 shows that, at the same modifier dosage, the softening point of the modified asphalt prepared by the present invention is 13 to 22% higher than the softening point of the modified asphalt of the comparative example. This shows that the modified asphalt prepared by the present invention has better high temperature resistance. The softening point of the modified asphalt prepared by Examples 1 to 3 is much higher than the technical index of the modified asphalt ID in JTG F400-2004, which shows that the preparation method of the present invention can effectively improve the high temperature stability of asphalt, meeting or even exceeding the current industry standards. According to the results of Example 3, even when the modified asphalt dosage is reduced by 8%, the softening point is still 14°C higher than the technical index of the modified asphalt ID. This shows that the asphalt prepared by the present invention can still maintain excellent high temperature performance while reducing the amount of modifier used.

[0062] Comparison between Example 1 and Comparative Example 3, and Example 2 and Comparative Example 4 shows that, at the same modifier dosage, the ductility of the modified asphalt prepared by the present invention is 33-38% higher than that of the modified asphalt of the comparative example, which indicates that the modified asphalt prepared by the present invention has better plasticity. The ductility of the modified asphalt prepared by the present invention is 30-37% higher than that of the modified asphalt of the comparative example after aging, which indicates that the modified asphalt prepared by the present invention has better low-temperature performance. The aging ductility of the modified asphalt prepared by Examples 1 to 3 is much higher than the technical index of the modified asphalt ID in JTG F400-2004, which shows that the preparation method of the present invention can effectively improve the low-temperature performance of asphalt, meeting or even exceeding the current industry standards. According to the results of Example 3, even when the modified asphalt dosage is reduced by 8%, the softening point is still higher than the technical index of the modified asphalt ID. This shows that the asphalt prepared by the present invention can still maintain excellent low-temperature performance when the amount of modifier is reduced.

[0063] According to Examples 1 to 3, even when the modified asphalt dosage is reduced by 8%, the results of Example 3 show that the softening point and aging ductility are still higher than the technical indicators of the modified asphalt ID. This shows that the asphalt prepared by the present invention can still maintain excellent high and low temperature properties when the amount of modifier is reduced, which not only reduces costs but also improves resource utilization efficiency.

[0064] In summary, the modified asphalt preparation method of the present invention performs well in improving the high and low temperature performance of asphalt, can meet or even exceed industry standards, and also has advantages in terms of economy. These characteristics make the modified asphalt of the present invention have a wide range of application potentials in road construction.

[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A SBS modified asphalt, characterized in that: In parts by mass, the components of the SBS modified asphalt include: The SBS modifier is a linear styrene-butadiene-styrene block copolymer, and the mass ratio of the polystyrene segment to the polybutadiene segment in the copolymer is 30:70; The compatibilizer is furfural extracted oil; The stabilizer is a sulfur-containing stabilizer.

2. The SBS modified asphalt according to claim 1, characterized in that The base asphalt is 70#A grade road petroleum asphalt.

3. The SBS modified asphalt according to claim 1, characterized in that The number average molecular weight of the linear styrene-butadiene-styrene block copolymer is 80,000 to 120,000.

4. The SBS modified asphalt according to claim 1, characterized in that The kinematic viscosity of the furfural extracted oil at 40° C. is 35 to 40 Pa·s.

5. The SBS modified asphalt according to claim 1, characterized in that The sulfur content of the sulfur-containing stabilizer is ≥99wt%.

6. The SBS modified asphalt according to claim 1, characterized in that In parts by mass, the components of the SBS modified asphalt include:

7. A method for preparing the SBS modified asphalt according to any one of claims 1 to 6, characterized in that: The following steps are involved: The base asphalt, SBS modifier, compatibilizer and stabilizer are mixed to obtain SBS modified asphalt.

8. The preparation method according to claim 7, characterized in that: The mixing process specifically includes: a) premixing the base asphalt and the SBS modifier by heating, and then shearing and mixing to obtain an asphalt mixture; b) mixing the asphalt mixture, compatibilizer and stabilizer, stirring and growing to obtain SBS modified asphalt.

9. The preparation method according to claim 8, characterized in that: In step a), the temperature of the heated premix is ​​120-160° C.; the temperature of the shear mixing is 180-200° C., the shear speed of the shear mixing is 2000-4500 r / min, and the time of the shear mixing is 30-60 min.

10. The preparation method according to claim 8, characterized in that: In step b), the stirring and developing temperature is 180-190° C., the stirring and developing speed is 600-1000 r / min, and the stirring and developing time is 3-6 h.