Water-based ink

By using specific resin units in aqueous inks, the wetting and fixing properties of the resin film are improved, and the problem of insufficient fixing properties of aqueous inks on the resin film is solved, and better printing material and storage properties are achieved.

CN119081474APending Publication Date: 2024-12-06KAO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411398168.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-11-27
Filing Date
2021-11-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The fixing properties of aqueous ink on the resin film are insufficient, resulting in the coating film being easily peeled off, affecting the aesthetics of the printed matter and food preservation.

Method used

A resin containing (meth)acrylic acid, cycloalkyl (meth)acrylic acid and an alkyl (meth)acrylic acid whose glass transition temperature is 0°C or less when the homopolymer is made is used as the fixing resin. Ensure the wetting and fixing properties of the resin film.

Benefits of technology

The fixing property of aqueous ink on the resin film is significantly improved, and the wipe resistance and storage properties of the printed matter are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005074407530000071
    Figure BDA0005074407530000071
  • Figure BDA0005074407530000211
    Figure BDA0005074407530000211
  • Figure BDA0005074407530000261
    Figure BDA0005074407530000261
Patent Text Reader

Abstract

The present invention relates to a water-based ink containing a pigment, a fixing resin, and water, the fixing resin contains a structural unit derived from a (meth) acrylic acid (A), a structural unit derived from a cycloalkyl (meth) acrylate (B), and a structural unit derived from an alkyl (meth) acrylate (C) having a glass transition temperature (Tg) of 0 DEG C or less when made into a homopolymer. The content of the structural unit derived from the (meth) acrylic acid (A) is 6-25 mass% of the total structural units of the fixing resin, and the content of the structural unit derived from the cycloalkyl (meth) acrylate (B) is 30-90 mass% of the total structural units of the fixing resin.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is filed on November 25, 2021 、Application No. 202180079280.8 、The name of the invention is Water-based Ink A divisional application for a patent application. Technical Field

[0002] The invention relates to a water-based ink. Background Art

[0003] In the industrial printing market such as packaging printing, resin films are mainly used as printing media from the perspective of durability. When the printing medium is a resin film, unlike paper media, the resin film does not absorb ink, the ink has poor wettability, and the constituent resin of the resin film has low polarity. As a problem, the fixability of the ink can be cited. Insufficient fixability of the ink to the resin film means that the ink coating film is easily peeled off from the resin film. The peeling of the ink will damage the aesthetics of the printed matter and reduce the storage of the contents such as food. Therefore, the fixability of the ink to the resin film is required.

[0004] In the past, the fixation to the resin film was possible by using solvent ink or UV ink, but the volatile organic solvent and residual monomer have a heavy load on the environment and human body. Therefore, the use of water-based ink with a small environmental load is being promoted. However, the fixation of water-based ink to the resin film is a big issue, and a new fixation technology for water-based ink is needed.

[0005] For example, as an inkjet aqueous ink capable of recording images having excellent fixability and abrasion resistance, Japanese Patent Application Laid-Open No. 2017-210604 (Patent Document 1) discloses an aqueous ink containing resin particles having: a first layer (inner side) formed by a first resin containing a specific amount of units derived from an ethylenically unsaturated monomer containing a cyclic aliphatic group, and a second layer (outer side) formed by a second resin having a specific amount of units derived from an ethylenically unsaturated monomer containing an ionic group. Summary of the invention

[0006] The present invention relates to an aqueous ink, wherein the aqueous ink contains a pigment, a fixing resin and water, wherein the fixing resin contains a structural unit derived from (meth)acrylic acid (A), a structural unit derived from a cycloalkyl (meth)acrylate (B), and a structural unit derived from an alkyl (meth)acrylate (C) having a glass transition temperature (Tg) of 0°C or less when forming a homopolymer, wherein the content of the structural unit derived from the (meth)acrylic acid (A) is 6% by mass or more and 25% by mass or less in all the structural units of the fixing resin, and the content of the structural unit derived from the cycloalkyl (meth)acrylate (B) is 30% by mass or more and 90% by mass or less in all the structural units of the fixing resin. DETAILED DESCRIPTION

[0007] When printing on a resin film using an aqueous ink, the aqueous ink needs to be sufficiently fixed to the resin film. However, in the technique of Patent Document 1, the fixing property of the ink is insufficient.

[0008] The present invention relates to an aqueous ink having excellent fixability to a resin film.

[0009] The present inventors have found that the above-mentioned problems can be solved by using a resin containing a structural unit derived from (meth)acrylic acid, a structural unit derived from a cycloalkyl (meth)acrylate, and a structural unit derived from an alkyl (meth)acrylate having a glass transition temperature of 0° C. or less when forming a homopolymer as a fixing resin.

[0010] That is, the present invention relates to an aqueous ink comprising a pigment, a fixing resin and water.

[0011] The fixing resin comprises a structural unit derived from (meth)acrylic acid (A), a structural unit derived from a cycloalkyl (meth)acrylate (B), and a structural unit derived from an alkyl (meth)acrylate (C) having a glass transition temperature (Tg) of 0° C. or less when forming a homopolymer.

[0012] The content of the structural unit derived from (meth)acrylic acid (A) is 6% by mass or more and 25% by mass or less in the total structural units of the fixing resin,

[0013] The content of the structural unit derived from the cycloalkyl (meth)acrylate (B) is 30% by mass or more and 90% by mass or less in the total structural units of the fixing resin.

[0014] According to the present invention, it is possible to provide an aqueous ink having excellent fixability to a resin film.

[0015] [Water-based ink]

[0016] The water-based ink of the present invention is a water-based ink containing a pigment, a fixing resin and water.

[0017] The fixing resin comprises a structural unit derived from (meth)acrylic acid (A), a structural unit derived from a cycloalkyl (meth)acrylate (B), and a structural unit derived from an alkyl (meth)acrylate (C) having a glass transition temperature (Tg) of 0° C. or less when forming a homopolymer.

[0018] The content of the structural unit derived from (meth)acrylic acid (A) is 6% by mass or more and 25% by mass or less in the total structural units of the fixing resin,

[0019] The content of the structural unit derived from the cycloalkyl (meth)acrylate (B) is 30% by mass or more and 90% by mass or less in the total structural units of the fixing resin.

[0020] It should be noted that "aqueous" means that water accounts for the largest proportion in the medium.

[0021] According to the present invention, it is possible to provide an aqueous ink having excellent fixability to a resin film. The reason for this is not necessarily clear, but it is considered to be as follows.

[0022] The fixing resin contained in the water-based ink of the present invention contains a structural unit derived from a cycloalkyl (meth)acrylate (B). It is believed that the cycloalkyl ester portion of the cycloalkyl (meth)acrylate (B) closely interacts with the resin film, thereby improving the fixing property.

[0023] Furthermore, since the fixing resin contains a structural unit derived from an alkyl (meth)acrylate (C) having a glass transition temperature (Tg) of 0°C or less when forming a homopolymer, it is considered that the Tg of the fixing resin can be lowered, thereby improving wettability to the resin film and improving fixing properties.

[0024] <Water-based ink>

[0025] The aqueous ink of the present invention contains at least a pigment, a fixing resin and water, and exhibits excellent fixing properties in inkjet printing. Therefore, it is preferably used for inkjet printing.

[0026] Preferred forms of the pigment used in the water-based ink of the present invention include: (i) a pigment that can maintain a dispersed state without a dispersant, i.e., a self-dispersible pigment; (ii) a pigment particle form in which the pigment is dispersed with a low-molecular or high-molecular surfactant; (iii) a polymer particle form containing the pigment. Among them, the polymer particle form containing the pigment is preferred from the viewpoint of the dispersion stability and fixability of the pigment.

[0027] Here, "pigment-containing polymer particles" (hereinafter also referred to as "pigment-containing polymer particles") refer to particles in which a polymer contains a pigment, particles in which a part of the pigment is exposed on the surface of particles composed of a polymer and a pigment, particles in which a polymer is adsorbed to a part of the pigment, and may be a mixture thereof. Among them, particles in which a polymer contains a pigment are more preferred.

[0028] [pigment]

[0029] The pigment used in the present invention may be any of an inorganic pigment and an organic pigment.

[0030] Examples of inorganic pigments include carbon black and metal oxides. In black ink, carbon black is preferred. Examples of carbon black include furnace black, lamp black, acetylene black, and channel black. Examples of white ink include metal oxides such as titanium dioxide, zinc oxide, silicon dioxide, aluminum oxide, and magnesium oxide.

[0031] Examples of the organic pigment include azo pigments, diazo pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, dioxazine pigments, perylene pigments, perinone pigments, thioindigo pigments, anthraquinone pigments, and quinophthalone pigments.

[0032] The color tone is not particularly limited, and in the case of chromatic ink, any color pigment such as yellow, magenta, cyan, red, blue, orange, green, etc. can be used.

[0033] The above-mentioned pigments may be used alone or in combination of two or more.

[0034] [Polymer particles containing pigment]

[0035] The polymer constituting the pigment-containing polymer particles (hereinafter also referred to as "polymer a") is not particularly limited as long as it has at least a pigment dispersibility.

[0036] As polymer a, vinyl resins, polyester resins, polyurethane resins, etc. obtained by addition polymerization of vinyl monomers can be cited. Among them, from the viewpoint of dispersion stability and fixability of the pigment, at least one selected from vinyl resins and polyester resins is preferred, and vinyl resins are more preferred.

[0037] As the polymer a, a synthetic product synthesized appropriately may be used, or a commercially available product may be used.

[0038] The pigment-containing polymer particles are more preferably pigment-containing crosslinked polymer particles obtained by further crosslinking the pigment-containing polymer particles with a crosslinking agent (hereinafter also referred to as "pigment-containing crosslinked polymer particles"), and are even more preferably pigment-containing crosslinked vinyl polymer particles.

[0039] The polymer a before crosslinking may be a water-soluble polymer or a water-insoluble polymer, but is more preferably a water-insoluble polymer. Even if the polymer used is a water-soluble polymer, the polymer becomes a water-insoluble polymer as long as it is crosslinked.

[0040] In this specification, the "water-insoluble" of a polymer means that when a constant amount of the polymer is dissolved in 100 g of water at 25°C after drying at 105°C for 2 hours, the amount of the polymer dissolved is less than 10 g. In the case of an anionic polymer, the amount of the polymer dissolved is the amount of the polymer dissolved when the anionic groups of the polymer are 100% neutralized with sodium hydroxide.

[0041] [Vinyl resin]

[0042] When polymer a is a vinyl resin, from the viewpoint of improving the dispersion stability of the pigment, the vinyl resin preferably contains a structural unit derived from an (a-1) ionic monomer, and further preferably has a structural unit derived from a (a-2) hydrophobic monomer and / or a (a-3) nonionic monomer.

[0043] [(a-1) Ionic monomer]

[0044] As the (a-1) ionic monomer, an anionic monomer is preferred, and examples thereof include a carboxylic acid monomer and a sulfonic acid monomer, and a carboxylic acid monomer is more preferred.

[0045] Examples of the carboxylic acid monomer include at least one selected from (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid and citraconic acid, preferably (meth)acrylic acid. "(Meth)acrylic acid" refers to at least one selected from acrylic acid and methacrylic acid.

[0046] [(a-2) Hydrophobic monomer]

[0047] (a-2) The "hydrophobicity" of the hydrophobic monomer means that when the monomer is dissolved to saturation in 100 g of ion-exchanged water at 25°C, the dissolved amount is less than 10 g.

[0048] As specific examples of (a-2) hydrophobic monomers, hydrophobic monomers described in paragraphs

[0020] to

[0022] of Japanese Patent Publication No. 2018-83938 can be cited. Among them, preferably, an alkyl (meth)acrylate having an alkyl group with a carbon number of 1 to 18, particularly 1 to 10, an aromatic group-containing monomer having an aromatic group with a carbon number of 6 to 22, a macromonomer having a polymerizable functional group at one end, and more preferably one or more selected from styrene, α-methylstyrene and benzyl (meth)acrylate.

[0049] The macromonomer having a polymerizable functional group at one end is a compound having a number average molecular weight of 500 to 100,000, preferably 1,000 to 10,000, and examples of the polymerizable functional group include an acryloyloxy group and a methacryloyloxy group.

[0050] The macromonomer is preferably an aromatic group-containing monomer-based macromonomer, and examples of the aromatic group-containing monomer constituting the macromonomer include the above-mentioned aromatic group-containing monomers.

[0051] Specific examples of commercially available styrene-based macromonomers include AS-6(S), AN-6(S), and HS-6(S) manufactured by Toagosei Co., Ltd.

[0052] [(a-3) Nonionic monomer]

[0053] The (a-3) nonionic monomer is a monomer having a high affinity for water or a water-soluble organic solvent, and is, for example, a monomer containing a hydroxyl group or a polyalkylene glycol chain.

[0054] Specific examples of the component (a-3) include the nonionic monomers described in paragraph

[0018] of Japanese Patent Application Publication No. 2018-83938, wherein preferably at least one selected from methoxy polyethylene glycol (n=1 to 30) (meth)acrylate and polypropylene glycol (n=2 to 30) (meth)acrylate.

[0055] The above-mentioned components (a-1) to (a-3) may be used alone or in combination of two or more monomer components contained in the components.

[0056] (Content of each structural unit in vinyl resin)

[0057] From the viewpoint of improving the dispersion stability of the pigment, the content of the structural unit derived from the components (a-1) to (a-3) in the vinyl resin is as follows.

[0058] The content of the component (a-1) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 12% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less.

[0059] The content of the component (a-2) is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, further preferably 70% by mass or less.

[0060] When component (a-3) is contained, its content is preferably 2 mass % or more, more preferably 5 mass % or more, further preferably 10 mass % or more, and is preferably 45 mass % or less, more preferably 40 mass % or less, further preferably 35 mass % or less.

[0061] The mass ratio of the component (a-1) to the component (a-2) [component (a-1) / component (a-2)] is preferably 0.15 or more, more preferably 0.2 or more, further preferably 0.25 or more, and is preferably 1.2 or less, more preferably 0.8 or less, further preferably 0.5 or less.

[0062] (Manufacture of vinyl resin)

[0063] The vinyl resin can be produced by copolymerizing a monomer mixture using a known polymerization method. As the polymerization method, a solution polymerization method is preferred.

[0064] The solvent used in the solution polymerization method is not limited, but polar solvents such as water, aliphatic alcohols, ketones, ethers, and esters are preferred, and water, methanol, ethanol, acetone, methyl ethyl ketone, and the like are more preferred.

[0065] During the polymerization, a polymerization initiator or a polymerization chain transfer agent may be used. Examples of the polymerization initiator include persulfates such as ammonium persulfate and potassium persulfate, and water-soluble azo polymerization initiators, and examples of the polymerization chain transfer agent include mercaptans.

[0066] The polymerization temperature varies depending on the types of polymerization initiator, monomer, solvent, etc. used, but is preferably 30° C. or higher, more preferably 50° C. or higher, and is preferably 95° C. or lower, more preferably 80° C. or lower.

[0067] The polymerization atmosphere is preferably a nitrogen or inert gas atmosphere.

[0068] The vinyl resin is preferably neutralized with a neutralizing agent as described later.

[0069] From the viewpoint of dispersion stability and fixability, the weight average molecular weight of the vinyl resin is preferably 5,000 or more, more preferably 8,000 or more, and even more preferably 10,000 or more, and is preferably 150,000 or less, more preferably 100,000 or less, and even more preferably 80,000 or less.

[0070] From the same viewpoints as above, the acid value of polymer a is preferably 50 mgKOH / g or more, more preferably 70 mgKOH / g or more, and further preferably 90 mgKOH / g or more, and is preferably 400 mgKOH / g or less, more preferably 300 mgKOH / g or less, and further preferably 200 mgKOH / g or less.

[0071] The weight average molecular weight and acid value of the polymer can be measured by the method described in Examples.

[0072] [Polyester resin]

[0073] When the polymer a is a polyester resin, the polyester resin contains a structural unit derived from an alcohol component and a structural unit derived from a carboxylic acid.

[0074] (Alcohol component)

[0075] Examples of the alcohol component of the raw material monomer of the polyester resin include polyols such as aromatic polyols and aliphatic polyols, and preferably contain aromatic diols.

[0076] As the aromatic diol, an alkylene oxide adduct of bisphenol A is preferred.

[0077] Specifically, the alkylene oxide adduct of bisphenol A is preferably a compound represented by the following general formula (I-1).

[0078]

[0079] In the general formula (I-1), OR 1 , R 2 O is an oxyalkylene group, and each independently is preferably an oxyalkylene group having 1 to 4 carbon atoms, and more preferably an oxyethylene group or an oxypropylene group.

[0080] x and y are the added mole numbers of alkylene oxide, and the average value of the sum of x and y is preferably 2 or more and preferably 7 or less, more preferably 5 or less, and further preferably 3 or less from the viewpoint of reactivity with the carboxylic acid component.

[0081] In addition, x OR 1 and y R 2 O may be the same or different, but are preferably the same from the viewpoint of fixability to print media. The alkylene oxide adduct of bisphenol A is preferably a propylene oxide adduct or an ethylene oxide adduct, and more preferably a propylene oxide adduct of bisphenol A.

[0082] From the viewpoint of improving fixability, the content of the alkylene oxide adduct of bisphenol A in the alcohol component is preferably 50 mol % or more, more preferably 60 mol % or more, further preferably 70 mol % or more and 100 mol % or less.

[0083] As the alcohol component of the raw material monomer of the polyester resin, other alcohol components may be used in addition to the alkylene oxide adduct of bisphenol A. Examples of other alcohol components include ethylene glycol, propylene glycol (1,2-propylene glycol), glycerol, pentaerythritol, trimethylolpropane, hydrogenated bisphenol A, sorbitol, or alkylene oxide (having a carbon number of 2 or more and 4 or less) adducts thereof (average addition mole number of 1 or more and 16 or less).

[0084] (Carboxylic acid component)

[0085] The carboxylic acid component as a raw material monomer of the polyester resin includes carboxylic acids, acid anhydrides thereof, and alkyl (having 1 to 3 carbon atoms) esters thereof.

[0086] Examples of the carboxylic acid component include aromatic dicarboxylic acids, aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and trivalent or higher polycarboxylic acids. Preferably, it is at least one selected from aromatic dicarboxylic acids and aliphatic dicarboxylic acids.

[0087] As the aromatic dicarboxylic acid, phthalic acid, isophthalic acid and terephthalic acid are preferred, and terephthalic acid is more preferred.

[0088] As the aliphatic dicarboxylic acid, unsaturated aliphatic dicarboxylic acid and saturated aliphatic dicarboxylic acid can be mentioned, as the unsaturated aliphatic dicarboxylic acid, fumaric acid and maleic acid are preferred, and fumaric acid is more preferred, as the saturated aliphatic dicarboxylic acid, adipic acid and succinic acid are preferred. As the alicyclic dicarboxylic acid, cyclohexane dicarboxylic acid, decalin dicarboxylic acid, and tetrahydrophthalic acid are preferred, and as the polycarboxylic acid with a valence of more than 3, trimellitic acid and pyromellitic acid are preferred.

[0089] The above carboxylic acid components can be used alone or in combination of two or more.

[0090] Among the above carboxylic acid components, aromatic dicarboxylic acids and aliphatic dicarboxylic acids are preferred, aliphatic dicarboxylic acids are more preferred, unsaturated aliphatic dicarboxylic acids are further preferred, and fumaric acid is further preferred. In addition, it is also preferred to use aromatic dicarboxylic acids and / or alicyclic dicarboxylic acids in combination with unsaturated aliphatic dicarboxylic acids.

[0091] The content of the unsaturated aliphatic dicarboxylic acid in the carboxylic acid component is preferably 25 mol% or more, more preferably 40 mol% or more, further preferably 60 mol% or more, further preferably 70 mol% or more, and is 100 mol% or less.

[0092] (Manufacture of polyester resin)

[0093] The polyester resin can be obtained by polycondensing at least an alcohol component and a carboxylic acid component. For example, it can be produced by polycondensing the alcohol component and the carboxylic acid component at a temperature of 180° C. to 250° C. in an inert gas atmosphere using an esterification catalyst as needed. The preferred embodiments and preferred contents of the alcohol component and the carboxylic acid component are as described above.

[0094] In the polycondensation reaction of the polyester resin, it is preferred to use an esterification catalyst.

[0095] As the esterification catalyst, there can be mentioned tin catalysts, titanium catalysts, metal compounds such as antimony trioxide, zinc acetate, germanium dioxide, etc., and from the viewpoint of esterification reaction efficiency, tin catalysts are preferred. As the tin catalyst, dibutyltin oxide, di(2-ethylhexanoate)tin(II), or salts thereof are preferred, and di(2-ethylhexanoate)tin(II) is more preferred.

[0096] Furthermore, if necessary, an esterification co-catalyst such as 3,4,5-trihydroxybenzoic acid may be further used, and a radical polymerization inhibitor such as 4-tert-butylcatechol or hydroquinone may be used in combination.

[0097] From the viewpoint of improving fixability, the acid value of the polyester resin is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, further preferably 15 mgKOH / g or more, and is preferably 70 mgKOH / g or less, more preferably 50 mgKOH / g or less, further preferably 40 mgKOH / g or less.

[0098] From the viewpoint of improving fixability, the weight average molecular weight of the polyester resin is preferably 8,000 or more, more preferably 10,000 or more, and further preferably 12,000 or more, and from the viewpoint of dispersion stability of the pigment, it is preferably 200,000 or less, more preferably 100,000 or less, and further preferably 50,000 or less.

[0099] The acid value and weight average molecular weight of the polyester resin can be prepared by appropriately adjusting the type of monomers used, the mixing ratio, the polycondensation temperature, and the reaction time to obtain a desired resin. The acid value and weight average molecular weight of the polyester resin can be measured by the method described in the Examples.

[0100] [Preparation of Pigment-Containing Polymer Particles]

[0101] The pigment-containing polymer particles can be efficiently produced as a pigment aqueous dispersion by a method having the following steps 1 and 2.

[0102] Step 1: A step of dispersing a pigment mixture containing a pigment, a polymer a, an organic solvent, and water to obtain a dispersed product

[0103] Step 2: A step of removing the organic solvent from the dispersion obtained in step 1 to obtain an aqueous dispersion of polymer particles A containing a pigment (hereinafter also referred to as "aqueous pigment dispersion (i)").

[0104] When the polymer a is a vinyl resin, it is preferred to further perform the following step 3.

[0105] Step 3: A step of adding a crosslinking agent to the pigment aqueous dispersion (i) obtained in step 2 to crosslink the pigment-containing polymer particles to obtain an aqueous dispersion (I) of pigment-containing crosslinked polymer particles (hereinafter also referred to as "pigment aqueous dispersion (I)").

[0106] The pigment-containing polymer particles according to the present invention also include the pigment-containing cross-linked polymer particles obtained in step 3.

[0107] (Process 1)

[0108] The pigment mixture in step 1 is preferably obtained by dissolving the polymer a in an organic solvent, and then adding the pigment, water, and, if necessary, a neutralizing agent, a surfactant, etc. to the obtained organic solvent solution and mixing them to obtain an oil-in-water dispersion.

[0109] The organic solvent used in step 1 is not limited, and is preferably ketones, ethers, esters, aliphatic alcohols having 1 to 3 carbon atoms, etc., and is more preferably ketones having 4 to 8 carbon atoms from the viewpoint of improving wettability to the pigment and adsorption of the polymer a to the pigment, more preferably methyl ethyl ketone and methyl isobutyl ketone, and even more preferably methyl ethyl ketone. When a vinyl resin is synthesized as the polymer a by a solution polymerization method, the solvent used in the polymerization may be used as it is.

[0110] When the polymer a has an acid group, it is preferred that at least a portion of the acid group is neutralized using a neutralizer. This is believed to increase the charge repulsion that is manifested after neutralization, thereby suppressing the aggregation of pigment particles in the aqueous ink and improving the dispersion stability of the pigment.

[0111] In the case of neutralization, it is preferable to perform neutralization so that the pH becomes 7 or more and 11 or less.

[0112] Examples of the neutralizing agent include bases such as sodium hydroxide, potassium hydroxide, ammonia, and various amines, and sodium hydroxide and ammonia are preferred.

[0113] Alternatively, the polymer a may be neutralized in advance.

[0114] From the viewpoint of improving dispersion stability, the usage equivalent of the neutralizer is preferably 20 mol % or more, more preferably 30 mol % or more, further preferably 40 mol % or more, and is preferably 150 mol % or less, more preferably 120 mol % or less, further preferably 100 mol % or less.

[0115] Here, the usage equivalent of the neutralizing agent can be calculated by the following formula, when the polymer a before neutralization is referred to as "polymer a'".

[0116] Equivalent amount of neutralizer used (mol %) = [{neutralizer added mass (g) / equivalent amount of neutralizer} / [{acid value of polymer a' (mgKOH / g) × mass of polymer a' (g)} / (56 × 1,000)]] × 100

[0117] The dispersion treatment in step 1 may be performed by only main dispersion using shear stress to micronize the pigment particles to a desired particle size. However, from the viewpoint of obtaining a uniform pigment aqueous dispersion, it is preferred to preliminarily disperse the pigment mixture and then perform main dispersion.

[0118] As a disperser for preliminary dispersion, a commonly used mixing and stirring device such as an anchor blade and a dispersion blade can be used.

[0119] As a device for providing shear stress for main dispersion, for example, a kneading machine such as a roll mill and a kneader, a high-pressure homogenizer such as a microfluidizer, a paint stirrer, a media disperser such as a bead mill, etc. Among them, from the viewpoint of reducing the particle size of the pigment, a high-pressure homogenizer and a bead mill are preferably used.

[0120] When a high-pressure homogenizer is used for dispersion treatment, the pigment can be controlled to have a desired particle size by controlling the number of passes at a dispersion pressure of 20 MPa or more, and the average particle size of the pigment aqueous dispersion (I) described below can also be adjusted.

[0121] (Process 2)

[0122] The removal of the organic solvent in step 2 can be performed by a known method. The organic solvent in the obtained pigment aqueous dispersion (i) is preferably substantially removed, but may remain in an amount of, for example, 0.1% by mass or less, as long as the purpose of the present invention is not impaired.

[0123] In order to remove coarse particles, it is preferred that the aqueous dispersion from which the organic solvent has been removed is further centrifuged, the liquid layer is filtered through a filter, etc., and the product passed through the filter is obtained as the pigment aqueous dispersion (i).

[0124] (Process 3)

[0125] Step 3 is optional, and a crosslinking agent is added to the pigment water dispersion (i) obtained in step 2 to crosslink a part of the carboxyl groups of the polymer a constituting the pigment-containing polymer particles, thereby forming a crosslinked structure on the surface of the pigment-containing polymer particles to obtain a pigment water dispersion (I) of crosslinked polymer particles containing the pigment. It is believed that the polymer formed by crosslinking the polymer a is firmly adsorbed or fixed on the surface of the pigment, and the aggregation of the pigment is suppressed, and as a result, the dispersion stability of the obtained ink is further improved.

[0126] The crosslinking agent is preferably a polyfunctional epoxy compound having two or more epoxy groups in the molecule, more preferably a compound having two or more glycidyl ether groups, and still more preferably a polyglycidyl ether compound of a polyol having a hydrocarbon group having 3 to 4 carbon atoms.

[0127] From the viewpoint of improving the easiness of reaction, etc., the molecular weight of the cross-linking agent is preferably 120 or more, more preferably 150 or more, and is preferably 2,000 or less, more preferably 1,500 or less.

[0128] The epoxy equivalent of the crosslinking agent is preferably 90 or more, more preferably 100 or more, and is preferably 300 or less, more preferably 200 or less.

[0129] Preferred examples of the crosslinking agent include polyglycidyl ethers such as trimethylolpropane polyglycidyl ether (water-soluble: 27% by mass) and pentaerythritol polyglycidyl ether (water-soluble: 0% by mass).

[0130] From the viewpoint of improving fixability, etc., the crosslinking rate in step 3 is preferably 15 mol% or more, more preferably 20 mol% or more, and further preferably 25 mol% or more, in terms of the ratio of the molar equivalent number of the crosslinking functional groups of the crosslinking agent to the molar equivalent number of the carboxyl groups of the polymer a, and is preferably 80 mol% or less, more preferably 60 mol% or less, and further preferably 50 mol% or less.

[0131] From the same viewpoint as described above, the temperature of the cross-linking treatment is preferably 40° C. or higher, more preferably 50° C. or higher, and is preferably 90° C. or lower, more preferably 80° C. or lower.

[0132] In the pigment water dispersion (I) of the pigment-containing cross-linked polymer particles obtained by step 3, from the viewpoint of ensuring the storage stability of the pigment water dispersion (I) when used in the water-based ink of the present invention, the acid value of the polymer constituting the pigment-containing cross-linked polymer particles having a cross-linked structure is preferably 40 mgKOH / g or more, more preferably 60 mgKOH / g or more, and further preferably 80 mgKOH / g or more, and is preferably 160 mgKOH / g or less, more preferably 130 mgKOH / g or less, and further preferably 100 mgKOH / g or less. In the present invention, the acid value of the polymer having a cross-linked structure can be calculated by multiplying the acid value of the polymer a before cross-linking by the cross-linking ratio.

[0133] From the viewpoint of improving the dispersion stability of the pigment aqueous dispersion, the non-volatile component concentration (solid content concentration) of the obtained pigment aqueous dispersion (I) is preferably 10% by mass or more, more preferably 15% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less.

[0134] The solid content concentration was measured by the method described in Examples.

[0135] From the viewpoint of dispersion stability, the content of the pigment in the aqueous pigment dispersion (I) is preferably 5% by mass or more, more preferably 10% by mass or more, further preferably 12% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less.

[0136] The mass ratio of the (cross-linked) polymer to the pigment constituting the (cross-linked) polymer particles containing the pigment in the aqueous pigment dispersion (I) [(cross-linked) polymer / pigment] is preferably 0.08 or more, more preferably 0.1 or more, and is preferably 0.8 or less, more preferably 0.7 or less.

[0137] From the viewpoint of dispersion stability, the average particle size of the pigment-containing (cross-linked) polymer particles is preferably 50 nm or more, more preferably 70 nm or more, further preferably 80 nm or more, and is preferably 400 nm or less, more preferably 300 nm or less, further preferably 200 nm or less.

[0138] The average particle size is measured by the method described in Examples.

[0139] <Fixing resin>

[0140] The aqueous ink of the present invention contains a fixing resin from the viewpoint of improving the fixing property and improving the scratch resistance of the obtained printed matter.

[0141] The fixing resin more preferably contains a structural unit derived from (meth)acrylic acid, a structural unit derived from a cycloalkyl (meth)acrylate, and a structural unit derived from an alkyl (meth)acrylate having a glass transition temperature (Tg) of 0° C. or less when forming a homopolymer, and is composed only of resin. That is, the fixing resin is preferably in the form of resin particles (hereinafter also referred to as "resin particles B") that do not contain a pigment.

[0142] The structure of the resin particles B may be a structure in which the composition changes from the center of the resin particles toward the outer shell, such as a core-shell structure, or a structure in which the composition is substantially uniform from the center of the resin particles toward the outer shell, and a uniform structure is more preferred.

[0143] The fixing resin is preferably used as an aqueous dispersion in which the resin particles B are dispersed in water.

[0144] The (meth)acrylic acid (A) constituting the fixing resin is one or more selected from acrylic acid and methacrylic acid. Among them, acrylic acid is preferred.

[0145] The number of carbon atoms of the cycloalkyl group of the (meth)acrylate cycloalkyl ester (B) constituting the fixing resin is preferably 4 or more and 12 or less, and more preferably 5 or more and 8 or less. Preferred examples of the (meth)acrylate cycloalkyl ester include at least one selected from cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and cycloheptyl (meth)acrylate. Among them, at least one selected from cyclopentyl acrylate, cyclohexyl acrylate, and cycloheptyl acrylate is preferred, and cyclohexyl acrylate is more preferred.

[0146] As the (meth)acrylic acid alkyl ester (C) having a glass transition temperature (Tg) of 0°C or less when forming a homopolymer, preferably, there can be mentioned an alkyl (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 10, more preferably a carbon number of 2 to 8. As a preferred example thereof, there can be mentioned one or more selected from the group consisting of ethyl (meth)acrylate, (iso)propyl (meth)acrylate, (iso)butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, and preferably one or more selected from the group consisting of ethyl acrylate, butyl acrylate, isobutyl acrylate, and hexyl acrylate.

[0147] The monomers (A) to (C) components may be used alone or in combination of two or more.

[0148] The fixing resin may contain structural units derived from other monomers other than the above-mentioned monomers A to C within a range not impairing the effects of the present invention. Examples of other monomers include ionic monomers other than the above-mentioned monomers A to C, hydrophobic monomers having an aromatic group, and nonionic monomers.

[0149] (Content of Each Structural Unit in Fixing Resin)

[0150] From the viewpoint of improving the fixing property to the printing medium, the content of the structural unit derived from each monomer in the fixing resin is as follows.

[0151] The content of the structural unit derived from (meth)acrylic acid (A) is 6 mass % or more, preferably 7 mass % or more, more preferably 8 mass % or more, and further preferably 9 mass % or more, and is 25 mass % or less, preferably 24 mass % or less, more preferably 23 mass % or less, and further preferably 22 mass % or less.

[0152] The content of the structural unit derived from the cycloalkyl (meth)acrylate (B) is 30% by mass or more, preferably 35% by mass or more, more preferably 40% by mass or more, and further preferably 45% by mass or more, and is 90% by mass or less, preferably 85% by mass or less, more preferably 80% by mass or less, and further preferably 75% by mass or less.

[0153] The content of the structural unit derived from the alkyl (meth)acrylate (C) is preferably 2% by mass or more, more preferably 4% by mass or more, and even more preferably 6% by mass or more, and is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less.

[0154] The fixing resin can be produced by copolymerizing a monomer mixture containing the above-mentioned monomer (A), monomer (B), monomer (C) and the like by a known polymerization method or the like.

[0155] From the viewpoint of improving fixability, the weight average molecular weight of the fixing resin is preferably 20,000 or more, more preferably 40,000 or more, further preferably 80,000 or more, and is preferably 2 million or less, more preferably 1 million or less, further preferably 500,000 or less, and further preferably 200,000 or less.

[0156] From the viewpoint of improving the fixing property, the acid value of the fixing resin is preferably 20 mgKOH / g or more, more preferably 30 mgKOH / g or more, further preferably 40 mgKOH / g or more, and is preferably 200 mgKOH / g or less, more preferably 180 mgKOH / g or less, further preferably 150 mgKOH / g or less, and further preferably 120 mgKOH / g or less.

[0157] The weight average molecular weight and acid value of the fixing resin are measured by the method described in Examples.

[0158] From the viewpoint of improving the fixing property, the glass transition temperature (Tg) of the fixing resin is preferably -20°C or higher, more preferably -15°C or higher, further preferably -10°C or higher, further preferably -5°C or higher, and is preferably 50°C or lower, more preferably 40°C or lower, further preferably 30°C or lower, further preferably 20°C or lower.

[0159] The glass transition temperature of the fixing resin can be calculated from the mass ratio of the monomers in each polymer part according to the following Fox equation.

[0160] 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+···+(W m / Tg m )

[0161] W1+W2+···W m =1

[0162] In the above Fox formula, Tg is the glass transition temperature of the polymer, Tg1, Tg2, ···, Tg m is the glass transition temperature of the homopolymer of each polymerizable monomer. The unit of temperature is K. In addition, W1, W2, ..., W m It represents the mass ratio of each monomer.

[0163] As the glass transition temperature of the homopolymer of each monomer in the above Fox formula, for example, the value described in Polymer Handbook Third Edition (Wiley-Interscience 1989) can be used.

[0164] From the viewpoint of storage stability of the ink, the average particle size of the resin particles B in the aqueous ink is preferably greater than 10 nm, more preferably greater than 20 nm, further preferably greater than 30 nm, and is preferably less than 300 nm, more preferably less than 200 nm, further preferably less than 150 nm.

[0165] The water-based ink of the present invention may contain various additives commonly used in water-based inks, such as a water-soluble organic solvent, a surfactant, a humectant, a wetting agent, a viscosity modifier, a defoaming agent, a preservative, a mildew preventive, and a rust preventive.

[0166] (Water-soluble organic solvent)

[0167] Examples of the water-soluble organic solvent include glycol ethers, polyols, nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, and alkanolamines. Among them, at least one selected from glycol ethers and polyols is preferred.

[0168] As the glycol ether, alkylene glycol monoalkyl ether and alkylene glycol dialkyl ether are preferred, and alkylene glycol monoalkyl ether is more preferred. Preferred examples of the alkylene glycol monoalkyl ether include ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, and diethylene glycol monobutyl ether.

[0169] Examples of the polyol include alkylene glycols having 2 to 6 carbon atoms, such as propylene glycol, diethylene glycol, and 1,2-hexanediol, and glycerin.

[0170] (Surfactant)

[0171] As the surfactant, a nonionic surfactant is preferred, and at least one selected from acetylene glycol-based surfactants and silicone-based surfactants is more preferred.

[0172] Examples of the acetylene glycol surfactant include acetylene glycols such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, 3,5-dimethyl-1-hexyn-3-ol, and 2,4-dimethyl-5-hexyn-3-ol, and ethylene oxide adducts thereof.

[0173] Examples of commercially available products of the acetylene glycol-based surfactants include "Surfynol" series and "OLFINE" series manufactured by Nissin Chemical Industry Co., Ltd.

[0174] As the silicone surfactant, polyether-modified silicone is preferred. Examples of commercially available products thereof include KF series manufactured by Shin-Etsu Chemical Co., Ltd.: KF-353, KF-355A, KF-642, KF-6011, etc., Silface SAG series manufactured by Nissin Chemical Co., Ltd., BYK series manufactured by BYK-Chemie Japan KK, and the like.

[0175] The water-based ink of the present invention can be efficiently produced by mixing a pigment, a fixing resin, water, and, if necessary, a water-soluble organic solvent, a surfactant, and other additives, etc. The mixing method is not particularly limited.

[0176] <Contents of each component in water-based ink>

[0177] From the viewpoint of improving the fixing property to the printing medium, the content of each component in the aqueous ink of the present invention and the ink properties are as follows.

[0178] (Pigment content)

[0179] The content of the pigment in the aqueous ink is preferably 2% by mass or more, more preferably 3% by mass or more, further preferably 4% by mass or more, and is preferably 15% by mass or less, more preferably 12% by mass or less, further preferably 10% by mass or less.

[0180] (Content of Pigment-Containing Polymer Particles)

[0181] The content of the pigment-containing polymer particles in the aqueous ink is preferably 3% by mass or more, more preferably 4% by mass or more, further preferably 5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 12% by mass or less.

[0182] (Content of fixing resin)

[0183] The content of the fixing resin in the aqueous ink is preferably 0.5% by mass or more, more preferably 1% by mass or more, and further preferably 2% by mass or more, and is preferably 10% by mass or less, more preferably 8% by mass or less, and further preferably 6% by mass or less.

[0184] The mass ratio of the fixing resin to the pigment-containing polymer particles [fixing resin / pigment-containing polymer particles] is preferably 0.1 or more, more preferably 0.2 or more, and is preferably 2 or less, more preferably 1 or less.

[0185] The content of the water-soluble organic solvent in the aqueous ink is preferably 10% by mass or more, more preferably 20% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less.

[0186] The total content of surfactants in the aqueous ink is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and further preferably 0.8% by mass or more, and is preferably 5% by mass or less, more preferably 4% by mass or less, and further preferably 3% by mass or less.

[0187] The water content in the aqueous ink is preferably 30% by mass or more, more preferably 40% by mass or more, and further preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and further preferably 70% by mass or less.

[0188] (Physical properties of water-based ink)

[0189] From the viewpoint of fixability, the viscosity of the aqueous ink at 32°C is preferably 2 mPa·s or more, more preferably 3 mPa·s or more, further preferably 4 mPa·s or more, and is preferably 20 mPa·s or less, more preferably 15 mPa·s or less, further preferably 12 mPa·s or less.

[0190] From the viewpoint of fixability, the pH of the aqueous ink at 20°C is preferably 5.5 or more, more preferably 6.0 or more, and further preferably 6.5 or more, and from the viewpoint of component tolerance and skin irritation, it is preferably 11.0 or less, more preferably 10.5 or less, and further preferably 10.0 or less.

[0191] The aqueous ink of the present invention is loaded in a known inkjet printing device and can be ejected as ink droplets onto a printing medium such as a resin film to print an image, etc. The ink droplets can be ejected by any of piezoelectric, thermal, and electrostatic methods.

[0192] As the resin film, transparent synthetic resin films can be mentioned, for example, polyester films, vinyl chloride films, polypropylene films, polyethylene films, nylon films, etc. These films can be biaxially stretched films, uniaxially stretched films, and non-stretched films. Among them, polyester films and stretched polypropylene films are preferred, and polyethylene terephthalate (PET) films treated with corona discharge, biaxially stretched polypropylene (OPP) films treated with corona discharge, etc. are more preferred.

[0193] Example

[0194] In the following Production Examples, Preparation Examples, Examples and Comparative Examples, "parts" and "%" mean "parts by mass" and "mass %" unless otherwise specified. The measurement and calculation methods of various physical properties are as follows.

[0195] (1) Determination of number average molecular weight and weight average molecular weight of polymer

[0196] Phosphoric acid and lithium bromide were dissolved in N,N-dimethylformamide to concentrations of 60 mmol / L and 50 mmol / L, respectively, and the resulting liquid was used as an eluent for measurement by gel permeation chromatography [GPC apparatus (HLC-8320GPC) manufactured by Tosoh Corporation, chromatographic columns (TSKgel SuperAWM-H, TSKgel SuperAW3000, TSKgelguardcolum Super AW-H) manufactured by Tosoh Corporation, flow rate: 0.5 mL / min], using a monodisperse polystyrene kit with a known molecular weight [PStQuick B (F-550, F-80, F-10, F-1, A-1000), PStQuick C (F-288, F-40, F-4, A-5000, A-500), manufactured by Tosoh Corporation] as a standard substance.

[0197] The measurement sample used was a sample prepared by mixing 0.1 g of the polymer and 10 mL of the above eluent in a glass bottle, stirring the mixture with a magnetic stirrer at 25° C. for 10 hours, and filtering the mixture with a syringe filter (DISMIC-13HP, made of PTFE, 0.2 μm, made by ADVANTEC Co., Ltd.).

[0198] (2) Measurement of Average Particle Size of Pigment-Containing Polymer Particles in Aqueous Dispersion

[0199] The average particle size was measured by cumulative analysis using a laser particle analysis system "ELS-8000" (manufactured by Otsuka Electronics Co., Ltd.). The particles were diluted with water to a concentration of 5 × 10 -3 The measurement conditions are as follows: temperature 25°C, angle between incident light and detector 90°, cumulative number 100 times, refractive index of water (1.333) as the refractive index of the dispersion solvent, and the obtained cumulative average particle size is taken as the average particle size of the polymer particles containing the pigment.

[0200] (3) Determination of solid content concentration of aqueous dispersion

[0201] Using an infrared moisture meter "FD-230" (manufactured by Kett Electric Laboratory Co., Ltd.), 5 g of the measurement sample was dried under the conditions of a drying temperature of 150°C and measurement mode 96 (monitoring time 2.5 minutes / variation range 0.05%), and the moisture content (%) of the measurement sample was measured. The solid content concentration was calculated by the following formula.

[0202] Solid content concentration (%) = 100 - water content of the sample (%)

[0203] (4) Determination of Acid Value of Polymer

[0204] The resin was dissolved in a titration solvent of a mixture of toluene and acetone (2:1) in a potentiometric automatic titrator (manufactured by Kyoto Electronics Co., Ltd., automatic burette, model: APB-610), and titrated with a 0.1N potassium hydroxide / ethanol solution using a potentiometric titration method, with the inflection point on the titration curve being the end point. The acid value (mgKOH / g) was calculated from the titration amount to the end point of the potassium hydroxide solution.

[0205] Production Example 1 (Production of Fixing Resin Emulsion 1)

[0206] (1) Into a reaction vessel equipped with a stirrer, a reflux condenser and a dropping tank, 0.96 parts of acrylic acid, 4.80 parts of cyclohexyl acrylate, 2.24 parts of isobutyl acrylate, 5.89 parts of methyl ethyl ketone (MEK) and 0.65 parts of water were charged as initial charges, and the temperature of the reaction vessel was maintained at 77° C. and stirred for 10 minutes.

[0207] Next, a mixture of monomers and the like described in Table 1, namely 8.64 parts of acrylic acid, 43.2 parts of cyclohexyl acrylate, 20.16 parts of isobutyl acrylate, 53.0 parts of MEK, 5.89 parts of water, and 2.64 parts of 4,4'-azobis(4-cyanovaleric acid) as a polymerization initiator, was continuously added to the reaction container over 5 hours. After the addition was completed, the polymerization reaction was continued for 1 hour, and the reaction was cooled to room temperature to terminate the polymerization reaction.

[0208] (2) 4.2 parts of MEK were added to 15.8 parts of the copolymer obtained above so that the solid content concentration of the polymer solution became 40 wt % to dilute it. Then, 1.6 parts of 5N sodium hydroxide aqueous solution were added and stirred well at 25° C. Then, 70.8 parts of water were added over 1 hour. After the addition was completed, MEK was evaporated by an evaporator to obtain a fixing resin emulsion 1.

[0209] Preparation Examples 2 to 9, 11, 12 and Comparative Preparation Examples 1 to 4

[0210] Except that the monomer composition constituting the fixing resin in Preparation Example 1 was changed to the conditions shown in Table 1, the same operation as in Preparation Example 1 was carried out to obtain fixing resin emulsions 2 to 9, 11, 12, and 21 to 24.

[0211] Production Example 10 (Production of Fixing Resin Emulsion 10)

[0212] (1) Into a reaction vessel equipped with a stirrer, a reflux condenser and a dropping tank, 0.36 parts of acrylic acid, 1.80 parts of cyclohexyl acrylate, 0.84 parts of isobutyl acrylate, 4.29 parts of an emulsifier (sodium polyoxyethylene alkyl ether sulfate, manufactured by Kao Corporation, LATEMULE-118B), 7.44 parts of a polymerization initiator (potassium persulfate), and 98.11 parts of water were charged as initial charges, and the temperature of the reaction vessel was maintained at 80° C. and stirred for 30 minutes.

[0213] Next, a mixture of monomers and the like described in Table 1, namely 6.84 parts of acrylic acid, 34.2 parts of cyclohexyl acrylate, 15.96 parts of isobutyl acrylate, 2.63 parts of the above-mentioned emulsifier (LATEMULE-118B), 4.56 parts of a polymerization initiator (potassium persulfate), and 24.89 parts of water, was continuously added to the reaction vessel over 3 hours. After the addition was completed, the polymerization reaction was continued for 3 hours, and the reaction was terminated by cooling to room temperature.

[0214] (2) To 10.0 parts of the emulsified copolymer obtained above was added 1.35 parts of a 5N sodium hydroxide aqueous solution, and the mixture was sufficiently stirred at 25° C. to obtain a fixing resin emulsion 10 .

[0215]

[0216] Preparation Example 1 (Preparation of aqueous dispersion of pigment-containing polymer particles 1)

[0217] (1) Synthesis of water-insoluble polymers

[0218] 16 parts of methacrylic acid, 44 parts of styrene, 30 parts of styrene macromonomer (manufactured by Toagosei Co., Ltd., trade name: AS-6S, number average molecular weight 6,000, solid content 50%), and 25 parts of methoxy polyethylene glycol methacrylate (manufactured by NOF Corporation, trade name: Blemmer PME-200) were mixed to prepare 115 parts of a monomer mixed solution.

[0219] 18 parts of MEK, 0.03 parts of a chain transfer agent (2-mercaptoethanol), and 10% (11.5 parts) of the above-mentioned monomer mixed solution were added to a reaction container and mixed, and the atmosphere was fully purged with nitrogen.

[0220] On the other hand, a mixed solution of the remaining 90% (103.5 parts) of the monomer mixed solution, 0.27 parts of the chain transfer agent, 42 parts of MEK, and 3 parts of a polymerization initiator (2,2'-azobis(2,4-dimethylvaleronitrile), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: V-65) was placed in a dropping funnel, and the mixed solution in the reaction container was heated to 75°C while being stirred under a nitrogen atmosphere, and the mixed solution in the dropping funnel was added dropwise over 3 hours. Then, after 2 hours at 75°C, a solution obtained by dissolving 3 parts of the polymerization initiator in 5 parts of MEK was added, and the mixture was further aged at 75°C for 2 hours and at 80°C for 2 hours, and 50 parts of MEK was further added to obtain a solution (solid content concentration: 45%) of a water-insoluble polymer (weight average molecular weight: 50,000, acid value: 104 mgKOH / g).

[0221] (2) Preparation of aqueous dispersion of pigment-containing polymer particles 1

[0222] 95.2 parts of the water-insoluble polymer solution obtained in the above (1) were dissolved in 53.7 parts of MEK, and 13.7 parts of a 5N sodium hydroxide aqueous solution, 0.5 parts of a 25% ammonia water and 341.8 parts of ion exchange water were added thereto as a neutralizing agent, and 100 parts of a cyan pigment (manufactured by DIC Corporation, trade name: Fastogen Blue CA5380 15:3) was further added to obtain a pigment mixed solution (polymer neutralization degree: 72 mol %).

[0223] The obtained pigment mixture was mixed using a dispersing blade at 7000 rpm and 20° C. for 1 hour, and then further dispersed using a microfluidizer (manufactured by Microfluidics, high pressure homogenizer, trade name: M-140K) at a pressure of 180 MPa for 15 passes.

[0224] The obtained dispersion of pigment-containing polymer particles was subjected to reduced pressure at 60°C to remove MEK, further remove a portion of water, and centrifuge, and the liquid layer was filtered using a membrane filter (manufactured by Sartorius, trade name: Minisart syringe filter, pore size: 5 μm, material: cellulose acetate) to remove coarse particles, thereby obtaining an aqueous dispersion of pigment-containing polymer particles (solid content concentration: 22%).

[0225] 0.45 parts of a crosslinking agent (trimethylolpropane polyglycidyl ether, trade name: Denacol EX321L, epoxy equivalent: 130) and 15.23 parts of ion exchange water were added to 100 parts of the obtained aqueous dispersion of the pigment-containing polymer particles (equivalent to a crosslinking ratio of 30 mol%), and the mixture was heated at 70°C for 3 hours while stirring (solid content concentration: 22%). After cooling to room temperature, the liquid layer was filtered with a membrane filter (trade name: Minisart syringe filter) to remove coarse particles, thereby obtaining an aqueous dispersion of the pigment-containing polymer particles 1 (solid content concentration: 22%, pigment: 15.2%, polymer: 6.8%, average particle size: 110 nm).

[0226] Preparation Example 2 (Preparation of aqueous dispersion of pigment-containing polymer particles 2)

[0227] (1) Production of polyester resin

[0228] Polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane was used as the alcohol component, fumaric acid as the carboxylic acid component, di(2-ethylhexanoate)tin(II) as the esterification catalyst, and 3,4,5-trihydroxybenzoic acid as the esterification co-catalyst, and the mixture was reacted at 210°C for 10 hours to obtain a polyester resin having an acid value of 22.4 mgKOH / g and a weight average molecular weight of 13700 (molar ratio of [carboxylic acid component / alcohol component]: 1.04).

[0229] (2) Production of Aqueous Dispersion of Pigment-Containing Polymer Particles 2

[0230] In a container with an internal volume of 2 L, 66.7 g of the polyester resin obtained in (1) above was dissolved in 198.6 g of MEK, and a 5N sodium hydroxide aqueous solution was added thereto to neutralize 85 mol % of the acid value of the polyester resin. Further, 390.5 g of ion exchange water was added dropwise over 30 minutes, and the mixture was stirred and mixed at 10 to 15° C. at 1,500 r / min for 15 minutes using a dispersing blade.

[0231] Next, 100 g of CI Pigment Blue 15:3 (manufactured by Dainichi Seika Industries, Ltd., trade name: CFB6338JC) was added, and the mixture was stirred and mixed at 10 to 15° C. at 6,500 r / min for 2 hours using a dispersing blade to obtain a preliminary dispersion.

[0232] The obtained pre-dispersion was filtered through 200 mesh, diluted by adding 36.1 g of ion exchange water, and then dispersed 15 times at a pressure of 150 MPa using a microfluidizer (manufactured by Microfluidics, high-pressure homogenizer, trade name: M-110EH-30XP) to obtain an aqueous dispersion of pigment-containing polymer particles 2.

[0233] The whole amount of the obtained pigment aqueous dispersion was added to a 2L eggplant-shaped flask, ion exchange water was added in a manner such that the solid content concentration was 15%, and a rotary distillation apparatus (Tokyo Rika Instruments Co., Ltd., rotary evaporator, trade name: N-1000S) was used to remove the organic solvent at a speed of 50 r / min in a warm bath adjusted to 32° C. and a pressure of 0.09 MPa (abs) for 3 hours. Furthermore, the warm bath was adjusted to 62° C., the pressure was reduced to 0.07 MPa (abs), and the mixture was concentrated to a solid content concentration of 25% to obtain a concentrate.

[0234] The obtained concentrate was placed in a 500 mL angle rotor and centrifuged at 3,660 r / min for 20 minutes using a high-speed cooling centrifuge (manufactured by Hitachi Koki Co., Ltd., trade name: himac CR22G, set temperature 20°C). The liquid layer was then filtered using a membrane filter (trade name: Minisart syringe filter) and diluted with water so that the solid content concentration became 22% to obtain an aqueous dispersion of pigment-containing polymer particles 2 (solid content concentration: 22%, pigment: 13.2%, polymer: 8.8%, average particle size: 95 nm).

[0235] Example 1 (Preparation of water-based ink 1)

[0236] To the ink composition described in Table 2 (total 100 parts), an aqueous dispersion of the pigment-containing polymer particles 1 (8.17 parts in terms of solid content), 2.83 parts of the fixing resin emulsion obtained in Preparation Example 1, 32 parts of propylene glycol, 2 parts of diethylene glycol monoisobutyl ether (iBDG), and an acetylene glycol surfactant (manufactured by Nissin Chemical Industry Co., Ltd., trade name: Surfynol 440 (average EO addition mole number: 3.5)), 1 part of a polyether-modified silicone surfactant (manufactured by Shin-Etsu Chemical Co., Ltd., trade name: KF-6011), 0.25 parts of a polyether-modified silicone surfactant (manufactured by Shin-Etsu Chemical Co., Ltd., trade name: KF-353A), and ion-exchanged water were added and stirred thoroughly, and filtered with a membrane filter (trade name: Minisart syringe filter) to obtain an aqueous ink 1 (solid content concentration: 11%, pigment: 5.6%, polymer: 5.4%).

[0237] Examples 2 to 14 and Comparative Examples 1 to 4

[0238] Except that the conditions in Example 1 were changed to those shown in Table 2, the same procedure as in Example 1 was carried out to obtain water-based inks 2 to 14 and 21 to 24.

[0239] It should be noted that water dispersion 1 described in Table 2 is a water dispersion of pigment-containing polymer particles 1, water dispersion 2 is a water dispersion of pigment-containing polymer particles 2, and the self-dispersible pigment is a cyan pigment manufactured by Cabot Corporation (trade name: CAB-O-JET 450C).

[0240] Using the water-based inks 1-14 and 21-24 obtained in the above Examples and Comparative Examples, printed materials were prepared by the method described in (1) below, and the peel strength and cellophane tape peeling were evaluated by the methods described in (2) and (3) below. The results are shown in Table 2.

[0241] It should be noted that the numerical values ​​in Table 2 are the amounts of effective ingredients (solid content).

[0242] (1) Production of printed materials

[0243] A table-top coater (manufactured by Mitsui Electric Seiki Co., Ltd., trade name: TC-1 model) and a rod coater No. 3 were used to apply water-based ink on the corona discharge treated surface of a PET film (manufactured by FUTAMURA CHEMICAL Co., Ltd., trade name: FE2001#25) and an OPP film (manufactured by FUTAMURA CHEMICAL Co., Ltd., trade name: FOR-AQ#25), and dried at 50°C for 3 minutes to produce printed materials.

[0244] In addition, as a substitute for the inkjet printing test, a table coater test was performed as a simple evaluation method. The table coater test is considered to be correlated with the inkjet printing test in terms of fixability.

[0245] (2) Determination of peel strength

[0246] A double-sided tape (Nichiban Co., Ltd., trade name: Nice Tack, No. 4) was attached to the obtained printed material, and a T-type peel test was performed using a Tensilon universal testing machine (A&D Co., Ltd., trade name: RTC-1150A) to measure the peel strength (N / 15 mm).

[0247] The peel strength is preferably 1.5 N / 15 mm or more, more preferably 2 N / 15 mm or more.

[0248] (3) Measurement of transparent tape peeling

[0249] A transparent tape (manufactured by NICHIBAN Co., Ltd., trade name: CT-18) was attached to the obtained printed matter and then rapidly peeled off. The peeled sample was visually observed and evaluated based on the following criteria.

[0250] (Evaluation Criteria)

[0251] ○: There is no peeling of ink.

[0252] △: There is a portion where the ink peels off.

[0253] ×: The ink was completely peeled off.

[0254] If the evaluation is 0 or △, there is no practical problem.

[0255] It should be noted that no strong correlation was found between the above (2) peel strength and (3) transparent tape peeling. It is preferred that the (2) peel strength is 1.5 N / 15 mm or more and the transparent tape peeling evaluation is 0 or △.

[0256]

[0257] As can be seen from Table 2, the water-based inks 1 to 14 obtained in Examples have better fixability than the water-based inks 21 to 24 obtained in Comparative Examples, and thus can provide printed materials having excellent peel strength.

[0258] Possibility of industrial application

[0259] According to the present invention, it is possible to provide an aqueous ink having excellent fixability to a resin film. The aqueous ink for inkjet printing of the present invention is particularly useful for forming an image on a resin film by inkjet printing.

Claims

1. A water-based ink, wherein: The water-based ink contains a pigment, a fixing resin and water. The fixing resin comprises a structural unit derived from (meth)acrylic acid (A), a structural unit derived from a cycloalkyl (meth)acrylate (B), and a structural unit derived from an alkyl (meth)acrylate (C) having a glass transition temperature Tg of 0° C. or less when forming a homopolymer. The content of the structural unit derived from (meth)acrylic acid (A) is 6% by mass or more and 25% by mass or less in the total structural units of the fixing resin, The content of the structural unit derived from the cycloalkyl (meth)acrylate (B) is 30% by mass or more and 90% by mass or less in the total structural units of the fixing resin, The glass transition temperature Tg of the fixing resin is -20°C or higher and 40°C or lower.

2. The water-based ink according to claim 1, wherein: The cycloalkyl (meth)acrylate (B) is one or more selected from the group consisting of cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and cycloheptyl (meth)acrylate.

3. The aqueous ink according to claim 1 or 2, wherein: The (meth)acrylic acid alkyl ester (C) is at least one selected from the group consisting of ethyl acrylate, butyl acrylate, isobutyl acrylate and hexyl acrylate.

4. The aqueous ink according to any one of claims 1 to 3, wherein The content of the structural unit derived from the alkyl (meth)acrylate (C) is 4% by mass or more and 60% by mass or less in the total structural units of the fixing resin.

5. The aqueous ink according to any one of claims 1 to 4, wherein The acid value of the fixing resin is 20 mgKOH / g or more and 200 mgKOH / g or less.

6. The aqueous ink according to any one of claims 1 to 5, wherein The weight average molecular weight of the fixing resin is 20,000 or more and 1,000,000 or less.

7. The aqueous ink according to any one of claims 1 to 6, wherein The fixing resin is in the form of resin particles, and the average particle diameter of the resin particles is 10 nm or more and 300 nm or less.

8. The water-based ink according to claim 7, wherein: The resin particles have a homogeneous structure.

9. The aqueous ink according to any one of claims 1 to 8, wherein The content of the fixing resin in the aqueous ink is 0.5% by mass or more and 10% by mass or less.

10. The aqueous ink according to any one of claims 1 to 9, wherein The aqueous ink further contains a water-soluble organic solvent.

11. The water-based ink according to claim 10, wherein: The water-soluble organic solvent is one or more selected from glycol ethers and polyols.

12. The aqueous ink according to claim 10 or 11, wherein: The content of the water-soluble organic solvent in the aqueous ink is 10% by mass or more and 50% by mass or less.

13. The aqueous ink according to any one of claims 1 to 12, wherein The aqueous ink further contains a surfactant.

14. The water-based ink according to claim 13, wherein: The surfactant is one or more selected from acetylene glycol-based surfactants and silicone-based surfactants.

15. The aqueous ink according to claim 13 or 14, wherein: The total content of the surfactants in the aqueous ink is 0.1% by mass or more and 5% by mass or less.

16. The aqueous ink according to any one of claims 1 to 5, wherein The pigment is in the form of polymer particles containing the pigment.

17. The water-based ink according to claim 16, wherein: The polymer constituting the pigment-containing polymer particles is a vinyl resin.

18. The water-based ink according to claim 17, wherein: The vinyl resin has a structural unit derived from (a-1) an ionic monomer, and a structural unit derived from (a-2) a hydrophobic monomer and / or (a-3) a nonionic monomer.

19. The aqueous ink according to claim 18, wherein: The content of the component (a-1) in the vinyl resin is 5% by mass or more and 45% by mass or less.

20. The aqueous ink according to claim 18 or 19, wherein: The content of the component (a-2) in the vinyl resin is 30% by mass or more and 90% by mass or less.

21. The aqueous ink according to any one of claims 18 to 20, wherein The mass ratio of the component (a-1) to the component (a-2) is (component (a-1) / component (a-2)) of 0.15 to 1.

2.

22. The aqueous ink according to any one of claims 18 to 21, wherein The weight average molecular weight of the vinyl resin is 5,000 or more and 150,000 or less.

23. The aqueous ink according to any one of claims 16 to 22, wherein The acid value of the polymer constituting the pigment-containing polymer particles is 50 mgKOH / g or more and 400 mgKOH / g or less.

24. The aqueous ink according to any one of claims 16 to 23, wherein The pigment-containing polymer particles are pigment-containing cross-linked polymer particles obtained by further cross-linking the pigment-containing polymer particles with a cross-linking agent.

25. The aqueous ink according to claim 16, wherein: The polymer constituting the pigment-containing polymer particles is a polyester resin containing a structural unit derived from an alcohol component and a structural unit derived from a carboxylic acid.

26. The aqueous ink according to claim 25, wherein: The structural unit derived from the alcohol component contains an aromatic diol.

27. The aqueous ink according to claim 25, wherein: The structural unit derived from a carboxylic acid contains one or more selected from aromatic dicarboxylic acids and aliphatic dicarboxylic acids.

28. The aqueous ink according to any one of claims 16 to 27, wherein As a mass ratio of the fixing resin to the pigment-containing polymer particles, the fixing resin / pigment-containing polymer particles is 0.1 or more and 2 or less.

29. The aqueous ink according to any one of claims 1 to 28, wherein The content of water in the aqueous ink is 30% by mass or more and 90% by mass or less.

30. The aqueous ink according to any one of claims 1 to 29, wherein For resin films.

31. The aqueous ink according to any one of claims 1 to 30, wherein For inkjet printing.

Citation Information

Patent Citations

  • Aqueous ink, ink cartridge and inkjet recording method

    JP2017210604A

  • Aqueous gravure ink

    JP2018083938A