Electrolyte-resistant lithium battery wrapping adhesive tape and preparation process thereof

By using a combination of polyimide film and electrolyte-resistant acrylate adhesive in lithium battery-wrapped tape, combining baking process and non-silicon oil release film layer, the lithium battery-wrapped tape is solved in high and low temperature environments. Adhesive performance issues ensure the stability and reworkability of the tape in the electrolyte, extend battery life and improve safety.

CN119081568AInactive Publication Date: 2024-12-06CROWN NEW MATERIALS TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411195454.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The adhesive properties of existing lithium battery-wrapped tapes are affected in high-temperature and low-temperature environments and are prone to fall off. They tear off the residual glue in high-temperature environments, and there is a risk of loss of stickiness and falling off after long-term contact with the electrolyte.

Method used

Polyimide film is used as the base film layer, and the adhesion performance is enhanced by corona treatment; electrolyte-resistant acrylate adhesive is used as the adhesive layer, and bake it in the oven to form a structure, combined with non-silicon oil release The film layer forms a laminated structure from top to bottom to ensure the adhesive performance of the tape in extreme environments and the corrosion performance of the electrolyte.

Benefits of technology

Maintain good bonding performance in extreme environments, prevent the tape from falling off, and immerse in the electrolyte for a long time without fading or falling off, extending the battery life, improving battery performance and safety, while avoiding residual glue problems, and having reworkable characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081568A_ABST
    Figure CN119081568A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery wrapping adhesive tapes, and particularly relates to an electrolyte-resistant lithium battery wrapping adhesive tape and a preparation process thereof.The lithium battery wrapping adhesive tape comprises a second base film layer, a second bonding layer, a first base film layer, a first bonding layer and a release film layer which are stacked from top to bottom, the polyimide films are adopted as the first base film layer and the second base film layer, so that the adhesive tape has excellent high-temperature resistance and low-temperature resistance, can keep good adhesive performance in an extreme environment, effectively prevents the adhesive tape from falling off, and can avoid residual glue left on the surface of a battery by sol due to high temperature resistance, and reworking can be realized; an electrolyte-resistant acrylate adhesive is adopted as the first adhesive layer and the second adhesive layer, the first base film layer and the second base film layer are coated with the first adhesive layer and the second adhesive layer respectively, and then a baking process is adopted, so that the adhesive tape has excellent electrolyte corrosion resistance and can be soaked in electrolyte for a long time without fading or falling off, and the service life of the adhesive tape is prolonged. And the appearance and performance safety of the battery are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention belongs to the technical field of battery wrapping tapes, and in particular relates to an electrolyte-resistant lithium battery wrapping tape and a preparation process thereof. [Background technology]

[0002] As the global demand for environmental protection and new energy grows, lithium batteries, as an efficient and clean energy storage method, are widely used in electric vehicles, electric bicycles, energy storage systems and other fields. In these applications, the safety and reliability of lithium batteries are crucial, among which the battery packaging materials play a key role. Lithium battery wrapping tape is a commonly used battery packaging material.

[0003] The adhesive properties of existing lithium battery wrapping tapes may be affected in high and low temperature environments, resulting in the problem of tape falling off during use, and in high temperature environments, there will be residual adhesive left after tearing it off, and the reworkability is poor. The existing patent with publication number CN217535887U discloses a new energy battery tape, including a tape pressing base layer, a rubber anti-stretching layer is arranged at the top of the tape pressing base layer, a PE anti-stretching layer is arranged at the end of the rubber anti-stretching layer away from the tape pressing base layer, a scratch-resistant layer is arranged at the top of the PE anti-stretching layer, a flame-retardant layer is arranged at the end of the tape pressing base layer away from the rubber anti-stretching layer, and an adhesive layer is arranged at the bottom of the flame-retardant layer. The product prepared using this method can have a flame-retardant effect and effectively prevent safety problems caused by battery heating, but the product prepared by this method has the risk of losing adhesion and falling off due to long-term contact with electrolyte. [Summary of the invention]

[0004] The object of the present invention is to provide an electrolyte-resistant lithium battery wrapping tape and a preparation process thereof, which has high temperature resistance, low temperature resistance, and electrolyte corrosion resistance, ensures bonding performance, is convenient for rework, and prevents the tape from falling off.

[0005] The present invention is achieved by the following technical solutions:

[0006] A process for preparing an electrolyte-resistant lithium battery wrapping tape comprises the following steps:

[0007] S1. Prepare a first base film layer: use a polyimide film as the first base film layer, and perform corona treatment on the upper surface and the lower surface of the first base film layer using a power of 1.2kw-2.0kw;

[0008] S2. preparing a first adhesive layer: using an electrolyte-resistant acrylic adhesive as the first adhesive layer;

[0009] S3, preparing a release film layer: using PET as a substrate and coating a non-silicone release agent on its surface;

[0010] S4, uniformly coating the first adhesive layer on the lower surface of the first base film layer, and sending it into an oven, and after coming out of the oven, laminating the first adhesive layer with the upper surface of the release film layer to form a semi-finished tape with a structure of first base film layer-first adhesive layer-release film layer;

[0011] S5. Prepare a second base film layer: use a polyimide film as the second base film layer, and perform corona treatment on the upper surface and the lower surface of the second base film layer using a power of 1.2kw-2.0kw;

[0012] S6. preparing a second adhesive layer: using an electrolyte-resistant acrylic adhesive as the second adhesive layer;

[0013] S7. Evenly apply the second adhesive layer on the lower surface of the second base film layer and send it into an oven. After coming out of the oven, adhere the second adhesive layer to the upper surface of the first base film layer in the semi-finished tape to form a finished tape with a structure of second base film layer-second adhesive layer-first base film layer-first adhesive layer-release film layer.

[0014] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S1, the thickness of the first base film layer is 25-38 μm.

[0015] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S2, the thickness of the first adhesive layer is 25-30 μm.

[0016] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S3, the thickness of the release film layer is 25-50 μm, and the release force is ≤100 g / 24 mm.

[0017] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S4, the first base film layer coated with the first adhesive layer is fed into the oven at a speed of 35-45 m / min, the oven length is 40 m, and the oven temperature is 70-130°C.

[0018] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S5, the thickness of the second base film layer is 20-38 μm.

[0019] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S6, the thickness of the second adhesive layer is 14-25 μm.

[0020] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, in step S7, the second base film layer coated with the second adhesive layer is fed into the oven at a speed of 35-45 m / min, the oven length is 40 m, and the oven temperature is 70-130°C.

[0021] In the above-mentioned process for preparing an electrolyte-resistant lithium battery wrapping tape, the peeling force of the first adhesive layer is ≥10N / 24mm, the peeling force of the second adhesive layer is ≥5N / 24mm, and the peeling force of the first adhesive layer is greater than the peeling force of the second adhesive layer.

[0022] An electrolyte-resistant lithium battery wrapping tape is prepared using the electrolyte-resistant lithium battery wrapping tape preparation process as described above, and includes a second base film layer, a second adhesive layer, a first base film layer, a first adhesive layer, and a release film layer stacked from top to bottom.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] The present invention provides an electrolyte-resistant lithium battery wrapping tape and a preparation process thereof. The lithium battery wrapping tape comprises a second base film layer, a second adhesive layer, a first base film layer, a first adhesive layer, and a release film layer which are stacked from top to bottom. A polyimide film is used as the first base film layer and the second base film layer, so that the tape has excellent high and low temperature resistance, can maintain good adhesive performance in extreme environments, effectively prevent the tape from falling off, and the high temperature resistance can prevent the sol from leaving residual adhesive on the battery surface, which can be reworked; an electrolyte-resistant acrylic adhesive is used as the first adhesive layer and the second adhesive layer, and the first adhesive layer and the second adhesive layer are respectively coated on the first base film layer and the second base film layer and then a baking process is adopted, so that the tape has excellent electrolyte corrosion resistance, can be immersed in the electrolyte for a long time without fading or falling off, and ensures the appearance and performance safety of the battery.

Brief Description of the Drawings

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below.

[0026] Figure 1 It is a process flow chart of a process for preparing an electrolyte-resistant lithium battery wrapping tape in a specific embodiment of the present invention;

[0027] Figure 2 It is a schematic diagram of the structure of an electrolyte-resistant lithium battery wrapping tape in a specific embodiment of the present invention. [Specific implementation method]

[0028] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0029] When the embodiments of the present invention mention ordinal numbers such as "first" and "second", unless they do express the meaning of order according to the context, they should be understood as being merely for the purpose of distinction.

[0030] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0031] Specific embodiments, such as Figure 1-2 The process for preparing an electrolyte-resistant lithium battery wrapping tape shown includes the following steps:

[0032] Step S1, preparing a first base film layer: using a polyimide film as the first base film layer, and performing corona treatment on the upper and lower surfaces of the first base film layer using a power of 1.2kw-2.0kw, preferably 1.5kw, so that the base film and the adhesive can be better bonded. The polyimide film has excellent high and low temperature resistance and can maintain good bonding performance in an environment of -40°C to 200°C;

[0033] Step S2, preparing a first adhesive layer: using an electrolyte-resistant acrylic adhesive as the first adhesive layer, so that the prepared lithium battery wrapping tape has excellent electrolyte corrosion resistance, can be permanently immersed in the electrolyte at room temperature without falling off, and can be immersed at high temperature of 80° C. for 24 hours without fading or falling off, thereby extending the service life of the battery and improving the performance of the battery;

[0034] Step S3, preparing a release film layer: using PET as a substrate and coating a non-silicone oil release agent on its surface. The release film layer uses high-cleanliness PET as a substrate and a non-silicone oil release agent on its surface, and has environmental protection and stable release performance;

[0035] Step S4, uniformly coating the first adhesive layer on the lower surface of the first base film layer, and sending the layer into an oven, and after the layer comes out of the oven, laminating the first adhesive layer with the upper surface of the release film layer to form a semi-finished tape having a structure of the first base film layer-the first adhesive layer-the release film layer;

[0036] Step S5, preparing a second base film layer: using a polyimide film as the second base film layer, and performing corona treatment on the upper and lower surfaces of the second base film layer using a power of 1.2kw-2.0kw, preferably 1.5kw, so that the base film and the adhesive can be better bonded. The polyimide film has excellent high and low temperature resistance and can maintain good bonding performance in an environment of -40°C to 200°C;

[0037] Step S6, preparing a second adhesive layer: using an electrolyte-resistant acrylic adhesive as the second adhesive layer, so that the prepared lithium battery wrapping tape has excellent electrolyte corrosion resistance, can be permanently immersed in the electrolyte at room temperature without falling off, and can be immersed at high temperature of 80° C. for 24 hours without fading or falling off, thereby extending the service life of the battery and improving the performance of the battery;

[0038] Step S7, evenly apply the second adhesive layer on the lower surface of the second base film layer and send it into the oven. After coming out of the oven, adhere the second adhesive layer to the upper surface of the first base film layer in the semi-finished tape to form a finished tape with a structure of second base film layer-second adhesive layer-first base film layer-first adhesive layer-release film layer. The lithium battery wrapping tape includes a second base film layer, a second adhesive layer, a first base film layer, a first adhesive layer, and a release film layer stacked from top to bottom. Polyimide film is used as the first base film layer and the second base film layer, so that the tape has excellent high and low temperature resistance, can maintain good adhesion performance in extreme environments, effectively prevent the tape from falling off, and high temperature resistance can prevent the sol from leaving residual glue on the battery surface, which can be reworked; electrolyte-resistant acrylic adhesive is used as the first adhesive layer and the second adhesive layer, and the first adhesive layer and the second adhesive layer are respectively coated on the first base film layer and the second base film layer and then a baking process is adopted, so that the tape has excellent electrolyte corrosion resistance, can be immersed in the electrolyte for a long time without fading or falling off, and ensures the appearance and performance safety of the battery.

[0039] The first adhesive layer and the second adhesive layer of the present invention are the same acrylic adhesive layer, and different color pastes such as blue, yellow, black or white can be added to achieve the required color effect, and the addition ratio is controlled at 1%-5%.

[0040] The lithium battery wrapping tape of the present invention avoids adding chemicals that may pollute the environment during the preparation process, which is more environmentally friendly and also avoids problems that may affect the adhesive performance of the tape. In addition, the present invention performs special post-processing on the tape to make it reworkable, that is, if the battery needs to be readjusted or replaced after bonding, the tape can be easily torn off without leaving residual glue on the battery surface, which is convenient for operation and improves work efficiency.

[0041] Specifically, in step S1, the thickness of the first base film layer is 25-38 μm, preferably 25 μm.

[0042] In addition, in step S2, the thickness of the first adhesive layer is 25-30 μm, preferably 25 μm.

[0043] Furthermore, in step S3, the thickness of the release film layer is 25-50 μm, preferably 25 μm, and the release force is ≤100 g / 24 mm.

[0044] More specifically, in step S4, the first base film layer coated with the first adhesive layer is fed into the oven at a speed of 35-45 m / min, the oven length is 40 m, and the oven temperature is 70-130°C.

[0045] Further, in step S5, the thickness of the second base film layer is 20-38 μm, preferably 36 μm.

[0046] Furthermore, in step S6, the thickness of the second adhesive layer is 14-25 μm, preferably 14 μm.

[0047] Specifically, in step S7, the second base film layer coated with the second adhesive layer is fed into the oven at a speed of 35-45 m / min, the oven length is 40 m, and the oven temperature is 70-130°C.

[0048] More specifically, the peeling force of the first adhesive layer is ≥10N / 24mm, the peeling force of the second adhesive layer is ≥5N / 24mm, and the peeling force of the first adhesive layer is greater than the peeling force of the second adhesive layer.

[0049] The electrolyte-resistant lithium battery wrapping tape of the present invention comprises a second base film layer 3, a second adhesive layer 4, a first base film layer 1, a first adhesive layer 2, and a release film layer 5 which are stacked from top to bottom.

[0050] The manufacturing process of the present invention:

[0051] A transparent polyimide film with a thickness of 25 μm is used as the first base film layer. The film has excellent high and low temperature resistance and can maintain good bonding performance in an environment of -40°C to 200°C. The upper and lower surfaces of the second base film layer are treated with a power of 1.5 kW to treat the surface of the base film so that the base film and the adhesive can be better bonded.

[0052] The first adhesive layer is evenly coated on the lower surface of the first base film layer. The first adhesive layer is an electrolyte-resistant acrylic adhesive with a thickness of 25μm. Then, the first base film layer and the first adhesive layer are sent into an oven at a speed of 35-45m / min. The oven length is 40 meters, the minimum temperature is set to 70°C, and the maximum temperature is set to 130°C. After coming out of the oven, the first adhesive layer is bonded to the upper surface of the release film layer to form a semi-finished product with a structure of "first base film layer + first adhesive layer + release film layer". The release film layer is based on high-clean PET, and a non-silicone oil release agent is coated on its surface, which has environmental protection and stable release performance.

[0053] A transparent polyimide film with a thickness of 36 μm is used as the second base film layer. The film has excellent high and low temperature resistance and can maintain good bonding performance in an environment of -40°C to 200°C. The upper and lower surfaces of the second base film layer are treated with corona at a power of 1.5 kW to treat the base film surface.

[0054] A second adhesive layer is evenly coated on the lower surface of the second base film layer. The second adhesive layer is an electrolyte-resistant acrylic adhesive with a thickness of 14 μm. The second base film layer and the second adhesive layer are then sent into an oven at a speed of 35-45 m / min. The oven length is 40 meters, the minimum temperature is set to 70°C, and the maximum temperature is set to 130°C. After coming out of the oven, the second adhesive layer is bonded to the upper surface of the semi-finished first base film layer to form a finished product with a structure of "second base film layer + second adhesive layer + first base film layer + first adhesive layer + release film layer".

[0055] The above is an implementation method provided in combination with specific content, and it is not considered that the specific implementation of the present invention is limited to these descriptions. At the same time, due to different industry naming, it is not limited to the above naming, nor is it limited to English naming. Any similarity or similarity with the method, structure, etc. of the present invention, or a number of technical deductions or substitutions made under the premise of the concept of the present invention, shall be regarded as the protection scope of the present invention.

Claims

1. A process for preparing an electrolyte-resistant lithium battery wrapping tape, characterized in that: The steps include: S1. Prepare a first base film layer: use a polyimide film as the first base film layer, and perform corona treatment on the upper surface and the lower surface of the first base film layer using a power of 1.2kw-2.0kw; S2. preparing a first adhesive layer: using an electrolyte-resistant acrylic adhesive as the first adhesive layer; S3, preparing a release film layer: using PET as a substrate and coating a non-silicone release agent on its surface; S4, uniformly coating the first adhesive layer on the lower surface of the first base film layer, and sending it into an oven, and after coming out of the oven, laminating the first adhesive layer with the upper surface of the release film layer to form a semi-finished tape with a structure of first base film layer-first adhesive layer-release film layer; S5. Prepare a second base film layer: use a polyimide film as the second base film layer, and perform corona treatment on the upper surface and the lower surface of the second base film layer using a power of 1.2kw-2.0kw; S6. preparing a second adhesive layer: using an electrolyte-resistant acrylic adhesive as the second adhesive layer; S7. Evenly apply the second adhesive layer on the lower surface of the second base film layer and send it into an oven. After coming out of the oven, adhere the second adhesive layer to the upper surface of the first base film layer in the semi-finished tape to form a finished tape with a structure of second base film layer-second adhesive layer-first base film layer-first adhesive layer-release film layer.

2. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S1, the thickness of the first base film layer is 25-38 μm.

3. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S2, the thickness of the first adhesive layer is 25-30 μm.

4. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S3, the release film layer has a thickness of 25-50 μm and a release force of ≤100 g / 24 mm.

5. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S4, the first base film layer coated with the first adhesive layer is fed into the oven at a speed of 35-45 m / min, the oven length is 40 m, and the oven temperature is 70-130°C.

6. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S5, the thickness of the second base film layer is 20-38 μm.

7. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S6, the thickness of the second adhesive layer is 14-25 μm.

8. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: In step S7, the second base film layer coated with the second adhesive layer is fed into the oven at a speed of 35-45 m / min, the oven length is 40 m, and the oven temperature is 70-130°C.

9. The process for preparing an electrolyte-resistant lithium battery wrapping tape according to claim 1, characterized in that: The peeling force of the first adhesive layer is ≥10N / 24mm, the peeling force of the second adhesive layer is ≥5N / 24mm, and the peeling force of the first adhesive layer is greater than the peeling force of the second adhesive layer.

10. An electrolyte-resistant lithium battery wrapping tape, characterized in that: The adhesive tape is prepared by the electrolyte-resistant lithium battery wrapping tape preparation process as described in any one of claims 1 to 9, and includes a second base film layer, a second adhesive layer, a first base film layer, a first adhesive layer, and a release film layer stacked from top to bottom.

Citation Information

Patent Citations

  • Adhesive tape

    CN104159987A

  • Novel flame-retardant PI compound single-sided adhesive tape

    CN106947407A

  • Tab electrolyte-resistant pressure-sensitive adhesive, preparation method thereof and electrolyte-resistant tab tape

    CN109355025A

  • Battery-packaging material

    US20160301040A1

  • Adhesive, adhesive for packaging material for battery, laminate, packaging material for battery, container for battery, and battery

    WO2020246243A1