Sealing sheet, display, and method for manufacturing the same

By using a resin composition layer sealing sheet of specific thickness and composition in a micro LED display, the problems of insufficient resin flowability and bare chip displacement are solved, excellent buriedness and light control are achieved, and the visual recognition of the display is improved and productivity.

CN119081572AActive Publication Date: 2024-12-06아티엔스가부시키가이샤 +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411213003.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-11-30
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

In the progressive miniaturization LED elements, insufficient fluidity of the resin causes light to refract and reflect in the void, affecting the visual recognition of the display, and due to the uneven flow of the resin, the micro LEDs undergo bare-film shift, increasing production time and cost.

Method used

A sealing sheet is adopted, which consists of a first film, a resin composition layer and a second film. The thickness of the resin composition layer is between 2 μm and 100 μm and the thickness of the second film is between 12 μm and 188 μm, which satisfies a specific thickness ratio relationship. It has appropriate dynamic viscoelasticity and Young's modulus and contains specific resin compositions such as methacrylic resin, urethane resin and epoxy resin for sealing microLEDs.

Benefits of technology

It effectively suppresses the bare-film shift of micro LED and the refractive reflection of light, improves the visual recognition and production efficiency of the display, and provides excellent buriedness and light control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081572A_ABST
    Figure CN119081572A_ABST
Patent Text Reader

Abstract

Provided are a sealing sheet, a display, and a method for manufacturing the same, the sealing sheet having excellent embeddability and suppression of die displacement when applied to the sealing of a micro LED of a display in which the micro LED is used as a light source. The problem is solved by a sealing sheet in which a first film, a resin composition layer, and a second film are arranged in this order, the first film having a release layer on the surface facing the resin composition layer, the resin composition layer having a thickness Ta of 2-100 [mu] m, the second film having a thickness Th of 12-188 [mu] m, Ta and Th satisfying the relational expression 0.1 < = Ta / Thh < = 2, and Ta / Thh satisfies the relational expression 0.1 < = Ta / Thh < = 2. The maximum value (tan [delta] maximum value) of the loss tangent in the range of-50 DEG C to 80 DEG C obtained by dynamic viscoelasticity measurement of the resin composition layer is 0.6 to 2.2.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority based on Japanese patent application No. 2023-202350, filed on November 30, 2023, and all the contents disclosed therein are incorporated herein by reference. Technical Field

[0002] The present disclosure relates to a sealing sheet, and more particularly to a sealing sheet including a resin composition layer for sealing a micro LED used in a display using the micro LED as a light source, and also to a display equipped with the resin composition layer and a method for manufacturing the same. Background Art

[0003] In recent years, with regard to displays, with the goal of further high performance, the development of various light-emitting elements is being actively carried out. Specifically, various display specifications such as backlit displays using liquid crystals or quantum dots, displays using self-luminous elements such as mini / micro light emitting diodes (LED) or organic electroluminescence (EL), plasma displays, and electrophoretic displays have been studied, and the wide range of applications from large displays such as signage or televisions to small-sized uses such as tablets, personal computers, smart phones, and wearable devices has been studied. In particular, the development of displays using LEDs is progressing day by day, and a thermosetting resin composition for sealing LED elements is described in Japanese Patent Laid-Open No. 2023-12051 (Patent Document 1) and International Publication No. 2021 / 200035 (Patent Document 2). Japanese Patent Laid-Open No. 2021-111774 (Patent Document 3) describes a method for manufacturing a micro LED light emitting device in which a barrier layer is pressurized to deform the barrier layer, thereby sealing the micro LED. As a next-generation display technology, the micro LED display is the most popular. Summary of the invention

[0004] [Problems to be solved by the invention]

[0005] In the LED elements that have been miniaturized in recent years, the intervals between LED elements or the distance from the substrate have become narrower. The resin sheets for sealing optical semiconductor elements described in Patent Documents 1 and 2 have excellent heat resistance or handling properties. On the other hand, the resin has insufficient fluidity and is not sufficient to fill the void space (embeddedness) of the micro-sized LED elements. When there is a gap between the LED element and the sealing resin composition, light is refracted and reflected in the gap, and the light is mixed, which has an adverse effect on the visibility of the display.

[0006] On the other hand, when the micro-LED is embedded using the sealing sheet described in Patent Document 3, the uneven flow of the resin applies stress to one direction of the micro-LED, causing the micro-LED to shift from the substrate (die displacement). When die displacement occurs, the micro-LED emits light poorly, requiring a repair process for the defective part, thus increasing production time and cost.

[0007] The present disclosure is made in view of the above-mentioned problems, and its object is to provide a sealing sheet having excellent embedding properties and suppression of die shifting (die shifting properties) even when applied to a display using micro LEDs as light sources, a display having a resin composition layer, and a method for manufacturing the same.

[0008] Furthermore, as a further object, there is provided a sealing sheet having excellent light controllability, a display having a resin composition layer, and a method for producing the same, so as to prevent the visibility of the display from being reduced due to refraction or reflection of light.

[0009] [Technical means to solve the problem]

[0010] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by the sealing sheet described below, thereby completing the present inventions [1] to [8] described below.

[0011] [1]: A sealing sheet for sealing a micro-LED used in a display using the micro-LED as a light source, the sealing sheet being sequentially provided with a first film, a resin composition layer and a second film, the first film having a peeling layer on a surface facing the resin composition layer, the thickness Ta of the resin composition layer being 2 μm to 100 μm, the thickness Th of the second film being 12 μm to 188 μm, Ta and Th satisfying formula (1), and the maximum value of the loss tangent of the resin composition layer obtained by dynamic viscoelasticity measurement in the range of -50°C to 80°C being 0.6 to 2.2.

[0012] Formula (1) 0.1 ≦ Ta / Th ≦ 2

[0013] [2]: The sealing sheet according to [1], wherein the Young's modulus of the second film is 1 GPa to 6 GPa.

[0014] [3]: The sealing sheet according to [1] or [2], wherein a ratio of a root mean square height Sq of a surface of the first film in contact with the resin composition layer as specified in ISO 25178 to a thickness Ta of the resin composition layer is 30% or less.

[0015] [4]: The sealing sheet according to any one of [1] to [3], wherein the pencil hardness of the resin composition layer is 5B to 2H.

[0016] [5]: The sealing sheet according to any one of [1] to [4], wherein the resin composition layer contains a resin (A),

[0017] The resin (A) includes at least one selected from the group consisting of acrylic resin (a1), urethane resin (a2), and epoxy resin (a3).

[0018] [6]: The sealing sheet according to any one of [1] to [5], wherein the resin composition layer contains a colorant (B).

[0019] [7]: The sealing sheet according to any one of [1] to [6], wherein the resin composition layer contains a polymerization initiator (C).

[0020] [8]: A display using a micro LED having a resin composition layer of the sealing sheet according to any one of [1] to [7] as a light source.

[0021] [9]: A method for manufacturing a display using micro LEDs as light sources, comprising the following steps (1) to (6).

[0022] (1) a step of preparing a sealing sheet according to any one of [1] to [4], in which a first film, a resin composition layer for forming a sealing layer, and a second film are sequentially arranged;

[0023] (2) a step of preparing a sealing object in which a plurality of micro LEDs are arranged at intervals from each other on one surface of a substrate;

[0024] (3) a step of peeling the first film from the sealing sheet to expose the resin composition layer for forming a sealing layer;

[0025] (4) a step of placing the exposed resin composition layer for forming a sealing layer so as to cover the plurality of micro-LEDs;

[0026] (5) a step of flowing a resin composition layer for forming a sealing layer and filling the space between the plurality of micro-LEDs;

[0027] (6) A step of peeling off the second film.

[0028] [Effects of the Invention]

[0029] According to the present disclosure, it is possible to provide a sealing sheet having excellent embedding properties and suppression of die displacement even when applied to a display using micro LEDs as light sources, a display having a resin composition layer, and a method for producing the same.

[0030] Furthermore, according to the present disclosure, in addition to the above contents, a sealing sheet having excellent light controllability, a display having a resin composition layer, and a method for producing the same can be provided to prevent the visibility of the display from being reduced due to refraction and reflection of light. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic cross-sectional view showing an example of a laminated structure of a sealing sheet.

[0032] Figure 2 (a)~ Figure 2 (c-2) is a schematic cross-sectional view showing a step of sealing a light-emitting element on a substrate having the light-emitting element.

[0033] Figure 3 This is a cross-sectional view showing an example of a test substrate that imitates a micro-LED substrate.

[0034] Explanation of symbols

[0035] 1: Sealing sheet

[0036] 2: Resin composition layer

[0037] 2': Sealing layer

[0038] 3: First film

[0039] 4: Second film

[0040] 5: Light-emitting element (micro LED)

[0041] 6: Substrate

[0042] 7: Glass substrate DETAILED DESCRIPTION

[0043] Hereinafter, the present disclosure will be described in detail. In addition, the embodiment described below is an example of the present disclosure. The present disclosure is not limited to the following embodiment, and also includes modified examples implemented within the scope of the gist of the present disclosure.

[0044] In this specification, the numerical range specified by "to" is a range that includes the numerical values ​​recorded before and after "to" as the lower limit and upper limit. (Meth) acrylic acid refers to acrylic acid and methacrylic acid. In addition, as for the various components appearing in this specification, unless otherwise specified, they can be used alone or in combination of two or more. In addition, when two or more are used in combination, the content rate uses the total value.

[0045] [Form of sealing sheet]

[0046] An example of the sealing sheet disclosed in the present invention is shown in Figure 1 .like Figure 1As shown, the sealing sheet 1 is sequentially provided with a first film 3, a resin composition layer 2 and a second film 4. A plurality of resin composition layers may be provided. Figure 1 In the case of the three-layer structure shown above, a production method is preferably used in which the resin composition layer is formed on the second film and then the first film is bonded to the second film.

[0047] After manufacturing the sealing sheet, or while manufacturing the sealing sheet, the sealing sheet is wound around a core in a roll, thereby obtaining a sealing sheet roll. The length of the roll can be designed according to the purpose. From the perspective of improving productivity, it is preferably more than 50m, and more preferably more than 100m. From the perspective of manufacturing yield, the length of the roll is preferably set to less than 10000m. When the sealing sheet is set in a roll form, it is preferred that the first film is arranged outside the roll.

[0048] The sealing sheet disclosed in the present invention is used to seal the micro LED used in the display using the micro LED as a light source. The resin composition layer is preferably directly in close contact with the micro LED for sealing. The micro LED is not particularly limited, and is preferably arranged on a substrate of acrylic acid, urethane, polycarbonate, epoxy, polyimide, glass, paper, cloth, aluminum, ceramic or polyethylene terephthalate, and has an electrode portion. The micro LED can be arranged alone or in multiples.

[0049] Since the resin composition layer has high followability to the concave and convex surface, it is preferably used to follow the multiple micro-LEDs arranged on the substrate and fill the gaps between the micro-LEDs. By filling the resin composition layer between the micro-LEDs, a sealing layer including the resin composition layer is formed. The sealing layer has the function of fixing adjacent micro-LEDs to prevent them from falling off. In particular, it is further preferred to use the resin composition layer as a sealing layer of a micro-LED display panel.

[0050] Micro LED refers to a tiny LED element (chip) of 50μm or 100μm or less. A display using multiple optical semiconductor elements as light sources is formed by mounting multiple micro LEDs on a substrate with wiring or circuits. Micro LEDs are formed by LED elements such as GaAs, GaP, AlGaInP, InGaN, sealing resins for sealing them, packaging substrates, electrodes, etc., and the operating temperature is 25℃ to 60℃.

[0051] Below, use Figure 2 (a)~ Figure 2 (c-2) An example of the step of forming the sealing layer is described.

[0052] Step (a): Sealing sheet placement step

[0053] like Figure 2As shown in (a), after the first film 3 is peeled off from the sealing sheet 1 to expose the resin composition layer 2, the resin composition layer 2 side of the sealing sheet is placed on a substrate 6 having a micro LED 5 as a light-emitting element so as to directly cover the micro LED.

[0054] In this specification, the number of micro-LEDs is not particularly limited. In display applications, the number of micro-LEDs used is determined by the display size or the number of pixels. In addition, the light-emitting color of the micro-LED is not particularly limited, and examples of the light-emitting color include red, green, and blue. The size of the micro-LED is preferably less than 100 μm thick and 40,000 μm in area when viewed from above. 2 The thickness is preferably 50 μm or less and the area is preferably 10,000 μm or less when viewed from above. 2 The thickness is preferably 20 μm or less and the area is preferably 2,500 μm when viewed from above. 2 The following size.

[0055] The spacing between the micro LEDs mounted on the substrate is, for example, 10 μm to 5,000 μm. When a group of red, green, and blue micro LEDs is mounted on the substrate as a pixel, the spacing between the pixels is, for example, 10 μm to 2,000 μm, preferably 20 μm to 1,800 μm, and more preferably 500 μm to 1,500 μm. The spacing between the micro LEDs in one pixel is, for example, 10 μm to 200 μm, preferably 10 μm to 100 μm, and more preferably 20 μm to 60 μm.

[0056] Process (b): Pressing process

[0057] like Figure 2 As shown in (b), the resin composition layer 2 is made to flow by pressing and filled around the micro-LED or between the micro-LEDs. The resin composition layer 2 filled around the micro-LED or between the micro-LEDs becomes a sealing layer 2'. The pressing method is not particularly limited, and hot pressing and vacuum pressing are preferred. From the perspective of the filling property of the resin composition layer, the temperature during pressing is preferably 20°C to 200°C, more preferably 30°C to 150°C, further preferably 40°C to 130°C, and most preferably 60°C to 110°C.

[0058] In order to improve the adhesion with the micro-LED or adherend, heat aging may also be further performed after pressing. The heating temperature is preferably 40°C to 250°C, more preferably 80°C to 220°C, and more preferably 100°C to 190°C. The heating time is preferably 30 minutes to 300 minutes, more preferably 60 minutes to 240 minutes, and more preferably 90 minutes to 180 minutes. By setting the heating temperature and heating time, the residual stress of the resin composition layer can be removed and the close contact surface can be smoothed. Heat aging can also be implemented after step (c) described later. The second film can be peeled off before heat aging or after heat aging.

[0059] Step (c): Etching step

[0060] In step (c), etching can be performed as needed to remove the sealing layer on the optical semiconductor element or to thin it. When performing step (c), it is preferably performed after peeling off the second film. By removing the excess sealing layer, the brightness of the micro-LED is increased to ensure visibility when emitting light. The thickness of the sealing layer after etching is preferably as follows: Figure 2 As shown in (c-1) of FIG. 1 , the thickness of the micro LED is the same as that of the micro LED, or as shown in FIG. Figure 2 As shown in (c-2), the thickness of the micro-LED is less than that of the micro-LED. In addition, even if the sealing layer is not completely removed from the micro-LED, it is sufficient to substantially remove it, and a small amount of thin film may remain. In addition, step (c) may be omitted if the brightness can be fully ensured.

[0061] The etching method is not particularly limited, and wet etching methods such as chemical polishing using a reagent, physical polishing using an abrasive, laser etching, plasma etching using argon plasma or oxygen plasma, and dry etching methods such as ion beam etching can be cited as preferred examples. From the perspective of reducing surface unevenness, it is preferred to use plasma etching, or wet etching and dry etching in combination.

[0062] In addition, as the plasma etching conditions, for example, as long as CF 4 / O 2 / N 2 The mixed gas can be dry-etched at a power of 1500W to 3000W for 180 seconds to 600 seconds. 4 The gas supply amount can be, for example, 50 sccm to 100 sccm. 2 The gas supply rate can be set to 500 sccm to 1000 sccm, for example. 2 The gas supply amount can be, for example, set to 50 sccm to 100 sccm.

[0063] The sealing sheet of the present disclosure can form a sealing layer from the resin composition layer through the above-mentioned steps (a) to (c). Next, the constituent components of the sealing sheet of the present disclosure will be described in detail with reference to preferred examples.

[0064] [First film]

[0065] The first film is not particularly limited, and examples thereof include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyolefin films such as polypropylene and polyethylene, polyvinyl chloride films, polyurethane films, nylon films, polyolefin films, triacetyl cellulose films, and cycloolefin films. From the viewpoint of handling, polyester films or polyolefin films are preferred.

[0066] The first film has a release layer on the surface facing the resin composition layer. The release layer is preferably formed by applying a release agent such as silicone resin, alkyd resin, fluororesin, melamine resin, etc. to the film, and from the perspective of handling (preventing unintentional separation), a release layer using silicone resin is more preferred.

[0067] The peel force Pl of the first film is preferably 0.1 gf / 20 mm to 3 gf / 20 mm, more preferably 0.3 gf / 20 mm to 2 gf / 20 mm, and further preferably 0.5 gf / 20 mm to 1 gf / 20 mm.

[0068] The peeling force Pl of the first film can be adjusted by the release treatment of the release layer. For example, it can be adjusted by the type of release agent, the coating amount of the release agent, and the surface roughness of the release layer. In the case of reducing the value of the peeling force, it is effective to increase the surface roughness, increase the coating amount of the release agent, etc. In the case of increasing the value of the peeling force, it is only necessary to adjust the opposite.

[0069] The peel force Pl of the first film can be measured, for example, by attaching the second film of the sealing sheet to a stainless steel (SUS) plate and peeling the first film from the resin composition layer at a peeling angle of 180° and a peeling speed of 300 mm / min under an environment of 23°C and a relative humidity of 50%.

[0070] The first film may have a functional layer in addition to the release layer. Specific examples of the functional layer include an antistatic layer and an anti-blocking layer.

[0071] The thickness Tl of the first film is preferably 2 μm to 250 μm, more preferably 10 μm to 100 μm, and further preferably 20 μm to 60 μm. When the first film is provided with a peeling layer or a functional layer, the thickness Tl is a value including the peeling layer and the functional layer. By setting Tl to 2 μm to 250 μm, the ripple of the first film can be transferred to the resin composition layer to form a uniform resin composition layer.

[0072] The first film is preferably directly laminated with the resin composition layer. In the case where the first film is directly laminated with the resin composition layer, on the surface of the first film in contact with the resin composition layer, the ratio of the root mean square height Sq of the surface roughness according to the International Organization for Standardization (ISO) 25178 to the thickness Ta of the resin composition layer is preferably 30% or less, more preferably 15% or less, and further preferably 7.5% or less. By setting it to less than 30%, the surface roughness transferred to the resin composition layer is controlled, and the resin composition layer is fully smoothed in the pressing process described later, thereby the die shiftability and adhesion become good. The root mean square height Sq can be measured, for example, by the method described in the embodiments described later.

[0073] The root mean square height Sq value is preferably 0.01 μm to 2 μm, more preferably 0.04 μm to 1.5 μm, and even more preferably 0.1 μm to 1.5 μm.

[0074] In addition, the root mean square height Sq can be adjusted by the demoulding treatment of the peeling layer of the first film. For example, it can be adjusted by the type of peeling agent, the coating amount of the peeling agent, and the coating method of the peeling agent. In the case of increasing the value of the root mean square height Sq, it is effective to reduce the coating amount of the peeling agent, speed up the drying after coating the peeling agent, and make the peeling agent contain fillers. In the case of reducing the value of the root mean square height Sq, it is sufficient to adjust it in the opposite way. In addition, a method of transferring the concave and convex using a film or carrier material with a specified root mean square height Sq can also be applied.

[0075] [Second film]

[0076] The second film is not particularly limited, and examples thereof include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyolefin films such as polypropylene and polyethylene, polyvinyl chloride films, polyurethane films, nylon films, polyolefin films, triacetyl cellulose films, and cycloolefin films. From the viewpoint of handling, polyester films or polyolefin films are preferred.

[0077] The second film is preferably directly laminated on the resin composition layer.

[0078] The Young's modulus of the second film is preferably 1 to 6 GPa, more preferably 2 to 5 GPa, and still more preferably 3 to 5 GPa. By setting it to 1 to 6 GPa, the flow of the resin composition layer can be controlled while applying uniform pressure to the resin composition layer in the pressing step described later, thereby improving embedding properties.

[0079] The Young's modulus of the second film can be adjusted by the crystal state and the orientation direction, and a high Young's modulus can be exhibited by increasing the degree of crystallization or converting the random amorphous chains to oriented amorphous chains. In the case of reducing the Young's modulus, it is sufficient to adjust it in the opposite direction. When the Young's modulus is set to 1 GPa to 6 GPa, it is preferred to use a polyester film or a polyolefin film, and more preferably a polyethylene terephthalate film.

[0080] The Young's modulus of the second film can be measured by, for example, the method described in Examples below.

[0081] The second film preferably has a peeling layer on the surface facing the resin composition layer. The peeling layer is preferably formed by applying a peeling agent such as silicone resin, alkyd resin, fluororesin, melamine resin, etc. to the film, and from the perspective of handling (preventing unintentional separation), a peeling layer using silicone resin is more preferred.

[0082] The peel force Ph of the second film is preferably 0.5 gf / 20 mm to 5 gf / 20 mm, more preferably 0.8 gf / 20 mm to 4 gf / 20 mm, and still more preferably 1.0 gf / 20 mm to 3 gf / 20 mm.

[0083] The peeling force Ph of the second film can be adjusted by the release treatment of the release layer. For example, it can be adjusted by the type of release agent, the coating amount of the release agent, and the surface roughness of the release layer. In the case of reducing the value of the peeling force, it is effective to increase the surface roughness, increase the coating amount of the release agent, etc. In the case of increasing the value of the peeling force, it is only necessary to adjust it in the opposite way.

[0084] The peeling force Ph of the second film is preferably greater than the peeling force Pl of the first film. Specifically, the value of Ph / Pl is more preferably 1.1 to 11, and further preferably 1.1 to 6.

[0085] The peel force Ph of the second film can be measured, for example, by attaching the exposed resin composition layer to a SUS plate after peeling the first film from the sealing sheet, and further peeling the second film from the resin composition layer at a peeling angle of 180° and a peeling speed of 300 mm / min under an environment of 23° C. and a relative humidity of 50%.

[0086] The second film may have a functional layer in addition to the release layer. Specific examples of the functional layer include an antistatic layer and an anti-blocking layer.

[0087] The thickness Th of the second film is 12 μm to 188 μm, more preferably 12 μm to 100 μm, and even more preferably 20 μm to 60 μm. In the case where the second film is provided with a peeling layer or a functional layer, the thickness Th is a value including the peeling layer and the functional layer. By setting Th to 12 μm to 188 μm, the pressure transfer applied to the resin composition layer is controlled in the pressing step described later, so that the resin composition layer flows uniformly, thereby improving embedding property, die shifting property, and adhesion.

[0088] [Resin composition layer]

[0089] The resin composition layer preferably contains the resin (A), more preferably contains the colorant (B) and / or the polymerization initiator (C), and may contain other components.

[0090] In the present disclosure, the resin (A) is a substance having a function of bonding and fixing objects together as an adhesive. As a specific example, the resin (A) has a function of bonding and fixing to a substrate having micro-LEDs or micro-LEDs.

[0091] The maximum value of the loss tangent (tan δ maximum value) of the resin composition layer of the present disclosure obtained by dynamic viscoelasticity measurement in the range of -50°C to 80°C is 0.6 to 2.2, more preferably 0.9 to 1.7, and even more preferably 1.1 to 1.5.

[0092] The maximum value of tan δ is, for example, the value of loss tangent (tan δ) when the tan δ curve reaches a maximum value. When there are two or more local values, the maximum value of loss tangent (tan δ) is indicated.

[0093] When the maximum value of tan δ is greater than 0.6, the pressure applied to the resin composition layer in the pressing process is better in transferability, and the stress applied to the micro-LED is reduced, so the die displacement is improved. When the maximum value of tan δ is less than 2.2, the pressure applied to the resin composition layer in the pressing process is better in absorptiveness, and the embedding property is improved by following the unevenness of the micro-LED.

[0094] The maximum value of tan δ of the present disclosure can be adjusted by the type or composition of the resin (A), the type, dispersion state or content of the colorant (B), the type or content of the polymerization initiator (C), and the type or content of the crosslinking agent or monomer as other components.

[0095] When the resin (A) contains a (meth)acrylic resin (a1), the maximum value of tan δ can be increased compared to the case of containing a urethane resin (a2), but it is not limited to this depending on the resin composition. When the resin (A) contains a (meth)acrylic resin (a1), the maximum value of tan δ can be reduced by increasing the content of alkyl methacrylate such as methyl methacrylate. When it is desired to increase the maximum value of tan δ, it is sufficient to adjust it in the opposite way.

[0096] When carbon black is contained as the colorant (B), the maximum value of tan δ can be lowered compared to the case where a metal oxide pigment is contained, but this is not limited to this depending on the dispersion state of the particles. When the colorant (B) contains carbon black, the maximum value of tan δ can be lowered by increasing the content of carbon black. When it is desired to increase the maximum value of tan δ, it is sufficient to adjust the opposite.

[0097] When a thermal polymerization initiator is contained as the polymerization initiator (C), the maximum value of tan δ can be increased by increasing the content. When it is desired to reduce the maximum value of tan δ, it is only necessary to adjust the content inversely.

[0098] When the resin composition layer contains a crosslinking agent as another component, the maximum value of tan δ can be increased by increasing the content. When it is desired to reduce the maximum value of tan δ, it is only necessary to adjust it in the opposite way.

[0099] By increasing the content of the low-viscosity monomer, the maximum value of tan δ can be lowered. If the maximum value of tan δ is to be increased, it is only necessary to adjust it in the opposite direction. Specific examples of the low-viscosity monomer include 1,6-hexanediol diacrylate.

[0100] In addition, the loss tangent (tan δ40) of the resin composition layer of the present disclosure at 40°C obtained by dynamic viscoelasticity measurement is preferably 0.6 to 2.0, more preferably 0.8 to 1.9, and further preferably 1.1 to 1.5. By setting tan δ40 to 0.6 to 2.0, the pressure applied to the resin composition layer in the pressing process is appropriately transmitted, and the embedding property and die shifting property are improved.

[0101] In order to control the diffusibility of the pressure applied to the resin composition layer in the range of 20°C to 200°C, which is a preferred temperature band for the pressing process, the loss tangent at 40°C (tanδ40) is adjusted to 0.6 to 2.0, thereby achieving a balance between the loss tangent at 20°C to 40°C and the loss tangent at 40°C to 200°C without deviation.

[0102] Tan δ40 can be adjusted by the type or composition of the resin (A) and the type or dispersion state of the colorant (B). Specifically, the same adjustment method as that for the tan δ peak intensity can be cited.

[0103] In addition, the peak temperature of the loss tangent obtained by the dynamic viscoelasticity measurement of the resin composition layer of the present disclosure (tanδ peak temperature) refers to the temperature when the tanδ curve reaches a maximum, and when there are two or more peaks, it indicates the peak temperature on the lowest temperature side. The tanδ peak temperature is preferably -30°C to 70°C, more preferably -20°C to 50°C, further preferably -10°C to 30°C, and most preferably -10°C to 10°C.

[0104] When the tan δ peak temperature is within a range of -30°C to 70°C, the residual stress of the resin can be sufficiently removed in the heat aging step, thereby improving the adhesion to the adherend.

[0105] In addition, the tanδ peak temperature of the present disclosure can be adjusted by the type or composition of the resin (A). When the resin (A) contains a (meth) acrylic resin (a1), the tanδ peak temperature can be increased by increasing the content of a monomer having a high glass transition temperature (Tg) of the homopolymer. When the tanδ peak temperature is to be lowered, it is sufficient to adjust it in the opposite direction. The glass transition temperature (Tg) of the homopolymer in the present disclosure can be the value described in "POLYMER HANDBOOK, 1999, FOURTH EDITION".

[0106] The loss tangent (tan δ) is a ratio of loss elastic modulus / storage elastic modulus obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 10 Hz and at -50°C to 150°C.

[0107] The dynamic viscoelasticity and loss tangent (tan δ) in the present disclosure are measured by the method described in the embodiments described later. In addition, when the resin composition layer includes any one of a polymerization initiator (C) and a cross-linking agent, the polymerization / cross-linking reaction during measurement is an unfinished state. In addition, the measurement is preferably measured on a sheet with a thickness of more than 50 μm, and in the case of measuring a sheet less than the thickness, two groups of sealing sheets without the first film can also be prepared, and the resin composition layer is bonded to each other using a laminator, and a laminate of a second film / resin composition layer / second film is made, and the second film of one of the faces of the laminate is further peeled off, and the resin composition layer of the sealing sheet is repeatedly bonded, and thus after being laminated in a manner of more than 50 μm, the dynamic viscoelasticity is measured.

[0108] From the viewpoint of embedding property and die shifting property, the thickness Ta of the resin composition layer is 2 μm to 100 μm, preferably 5 μm to 60 μm, more preferably 10 μm to 40 μm, further preferably 10 μm to 30 μm, and particularly preferably 13 μm to 30 μm from the viewpoint of light shielding property.

[0109] By setting the thickness Ta of the resin composition layer to 2 μm to 100 μm, the pressure applied to the resin composition layer in the pressing process is appropriately dispersed and made sufficiently uniform, thereby improving embedding properties and die shifting properties. The resin composition layer may be a single layer or a stack of two or more layers, and the case of two or more layers refers to the total thickness.

[0110] The thickness Ta of the resin composition layer can be adjusted by the method for forming the resin composition layer described later. The thickness Ta in the present disclosure is measured by the method described in the examples described later.

[0111] The thickness Ta of the resin composition layer satisfies the formula (1) 0.1≦Ta / Th≦2 representing the ratio to the thickness Th of the second film, more preferably 0.2≦Ta / Th≦1.5, and even more preferably 0.2≦Ta / Th≦1.2.

[0112] By setting 0.1≦Ta / Th≦2, the pressure transmission to the resin composition layer in the pressing step described later is controlled, and the resin composition layer flows uniformly, thereby improving embedding properties and die shifting properties.

[0113] From the viewpoint of embedding property and die shifting property, the pencil hardness of the resin composition layer is preferably 5B to 2H, more preferably 4B to H, and still more preferably 3B to F. By setting the pencil hardness of the resin composition layer to 5B to 2H, the pressure applied to the resin composition layer in the pressing step is appropriately dispersed and sufficiently uniform, thereby improving embedding property and die shifting property.

[0114] The pencil hardness of the resin composition layer can be adjusted by the type of resin (A), the content of the polymerization initiator (C), and the content of the monomer. Increasing the content of the polymerization initiator (C) can make it harder, while increasing the content of the monomer can make it softer.

[0115] The pencil hardness of the resin composition layer in the present disclosure is measured by the method described in Examples below. When the resin composition layer contains any of a polymerization initiator (C) and a crosslinking agent, the polymerization / crosslinking reaction is in an incomplete state during measurement.

[0116] [Method for forming resin composition layer]

[0117] The method for forming the resin composition layer is not particularly limited, and as a suitable example, a method of applying a resin composition obtained by adding an arbitrary solvent to the components constituting the resin composition layer to form the resin composition layer can be cited. The purpose of adding the solvent is to adjust the viscosity level suitable for coating and to adjust the film thickness.

[0118] For coating, known coating machines or methods such as notch wheel coater, die coater, roll coater, die lip coater, reverse coater, gravure coater, rod coater, curtain coater, dip coating, spin coating, screen coating, and casting can be used. The solvent contained in the resin composition can be removed by a drying process after coating.

[0119] As a preferred embodiment, the resin composition can be applied to supports such as the first film and the second film, and then the coated film is heated and dried using a hot air oven, an infrared heater, etc., thereby forming a resin composition layer on one side of the support. And then, in order to improve the crosslinking density of the resin composition layer, it is preferably, for example, to stand under specific temperature conditions such as aging treatment or irradiation of ultraviolet light (ultraviolet, UV) etc. In addition, it is also possible to use a laminator to transfer to other supports such as the first film, the second film, and a substrate after coating.

[0120] [Resin composition]

[0121] The resin composition can be obtained by mixing the solvent and the components constituting the resin composition layer while stirring. As the components constituting the resin composition layer, it is preferably containing resin (A), more preferably containing colorant (B) and / or polymerization initiator (C), and other components may also be contained. Any solvent is used for the purpose of adjusting the processing adaptability such as viscosity when the components constituting the resin composition layer are mixed. For example, ester system, ether ester system, ether system, alcohol system, aromatic system, etc. can be suitably used. Solvents that are compatible with resin (A) include, for example, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, cyclohexanone, toluene, xylene, isopropanol, N-methyl-2-pyrrolidone, etc. can be cited as suitable examples.

[0122] A known stirring device can be used for stirring, and preferably a disperser, a mixer, an oscillator, a homogenizer or the like is used.

[0123] In order to obtain the resin composition, the following production process can be adopted: first, a mixture is prepared by mixing the resin (A) or an arbitrary solvent with the colorant (B), and second, a two-stage or more production process is performed by adding the resin (A), the polymerization initiator (C), and other components as needed.

[0124] [Resin (A)]

[0125] The weight average molecular weight (Mw) of the resin (A) is preferably 1,000,000 or less. It is more preferably 300,000 or less, and further preferably 150,000 or less. By setting the weight average molecular weight (Mw) of the resin (A) to 1,000,000 or less, the entanglement of the molecular chains in the heat aging process becomes easy to untangle, and the adhesion is improved.

[0126] The lower limit of the weight average molecular weight (Mw) of the resin (A) is not particularly limited, but is preferably 400 or more, more preferably 900 or more, further preferably 3000 or more, further preferably 5000 or more, and particularly preferably 10,000 or more. By setting the weight average molecular weight (Mw) of the resin (A) to 400 or more, the coating film strength of the resin composition layer is improved.

[0127] The weight average molecular weight (Mw) is a value in terms of polystyrene measured by gel permeation chromatography (GPC). The weight average molecular weight (Mw) in the present disclosure is measured by the method described in Examples described below.

[0128] The glass transition temperature (Tg) of the resin (A) is preferably -30°C to 80°C, more preferably -20°C to 60°C, further preferably -15°C to 40°C, further preferably -10°C to 20°C, and particularly preferably -10°C to 10°C. By setting the temperature to -30°C to 80°C, the residual stress of the resin (A) after the pressing step is reduced, so that the adhesion becomes suitable.

[0129] Regarding the glass transition temperature (Tg) of the resin (A) in the present disclosure, when the resin (A) undergoes a polymerization / crosslinking reaction caused by heat or light, the polymerization / crosslinking reaction is in an incomplete state during measurement. The glass transition temperature (Tg) of the resin (A) in the present disclosure is measured by the method described in the Examples described below.

[0130] Resin (A) can be used alone or in combination of two or more. Based on the total amount (100% by mass) of the resin composition layer, the content of resin (A) is preferably 10% by mass to 98% by mass, more preferably 25% by mass to 95% by mass, and further preferably 60% by mass to 90% by mass. In the case of comprising two or more resins (A), the content of any resin (A) is preferably 5% by mass or more, and the total content is preferably in the range. By setting the content of resin (A) to 10% by mass to 98% by mass, the compatibility with colorant (B) becomes good, and light-shielding property is improved.

[0131] Preferred examples of the resin (A) include (meth)acrylic resins (a1), urethane resins such as polyurethane resins or polyurethane urea resins (a2), epoxy resins (a3), maleic acid resins, styrene-maleic acid copolymers, polystyrene resins, polybutadiene resins, polyester resins, condensation-type polyester resins, addition-type polyester resins, melamine resins, polycarbonate resins, oxetane resins, phenoxy resins, polyimide resins, polyamideimide resins, alkyd resins, amino resins, polyamide resins, polylactic acid resins, oxazoline resins, benzoxazine resins, silicone resins, fluororesins, butyral resins, chlorinated polyethylene, chlorinated polypropylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, polyvinyl acetate, vinyl resins, rubber resins, cyclized rubber resins, celluloses, polyethylene (high-density polyethylene (HDPE), low-density polyethylene (LDPE)), and the like. From the viewpoint of embedding properties, it is preferred to contain at least one of a (meth)acrylic resin (a1), a urethane resin (a2), and an epoxy resin (a3). Furthermore, from the viewpoint of adhesion, it is more preferred to contain a (meth)acrylic resin (a1).

[0132] The resin (A) preferably has one or more functional groups that can be used for polymerization / crosslinking reaction induced by heat or light. The functional group can be appropriately selected according to the reactivity with the resin (A) or the polymerization initiator (C) or the crosslinking agent described later, and may be a functional group capable of self-crosslinking.

[0133] Examples of the functional group include a hydroxyl group, a carboxyl group, an amino group, an epoxy group, an oxetanyl group, an oxazoline group, an oxazine group, an aziridine group, a thiol group, an isocyanate group, a blocked isocyanate group, a silanol group, a (meth)acryloyl group, an N-vinyl group, a vinyl ether group, an allyl group, an unsaturated carboxylic acid group, etc. Preferred free radical polymerizable functional groups are a (meth)acryloyl group, an N-vinyl group, a vinyl ether group, an allyl group, and an unsaturated carboxylic acid group.

[0134] [(Meth)acrylic resin (a1)]

[0135] In the present disclosure, the (meth)acrylic resin (a1) is an acrylic copolymer obtained by copolymerizing a monomer containing a (meth)acrylic ester monomer, and is a polymer having a structural unit based on 2 to 20,000 monomers. As a suitable example of the (meth)acrylic ester monomer, an alkyl (meth)acrylic acid ester monomer can be exemplified. In the case of introducing a functional group that can be used for polymerization / crosslinking reaction, it is preferably a (meth)acrylic copolymer obtained by copolymerizing a monomer containing a functional group with a (meth)acrylic ester monomer.

[0136] In addition, the (meth)acrylic resin (a1) of the present disclosure excludes compounds having two or more urethane bonds in one molecule and compounds having two or more epoxy groups in one molecule.

[0137] The (meth)acrylic acid alkyl ester monomer is a compound obtained by esterifying (meth)acrylic acid and introducing an alkyl group or a cycloalkyl group, and the alkyl group or the cycloalkyl group may be any of a linear, branched, or cyclic saturated aliphatic hydrocarbon group. The saturated aliphatic hydrocarbon group is preferably a saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, and more preferably a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms. Specific examples thereof include: methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, and (meth)acrylate. The colorant (B) may be selected from the group consisting of isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. Among these, methyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate are particularly preferably used, and methyl (meth)acrylate and n-butyl (meth)acrylate are particularly preferably used, from the viewpoint of the dispersibility of the colorant (B).

[0138] The structural unit derived from the (meth)acrylic acid alkyl ester monomer preferably accounts for 1 to 100% by mass, more preferably 20 to 99.5% by mass, and even more preferably 80 to 99% by mass, relative to 100% by mass of the (meth)acrylic resin (a1), from the viewpoint of adhesion.

[0139] The (meth)acrylic resin (a1) preferably has a structural unit derived from a functional group-containing monomer and / or an unsaturated bond.

[0140] As the monomer containing a functional group, there can be exemplified carboxyl-containing monomers, hydroxyl-containing monomers, epoxy-containing monomers, and amino-containing monomers. By containing a monomer containing a functional group, the cohesive force of the resin (A) is improved, and a tough resin composition layer can be obtained. Particularly preferably, it contains carboxyl-containing monomers, hydroxyl-containing monomers, and epoxy-containing monomers.

[0141] Examples of carboxyl group-containing monomers include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, p-carboxybenzyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, citraconic acid, and isocrotonic acid. Among these, (meth)acrylic acid is preferred from the viewpoint of adhesion.

[0142] Examples of hydroxyl-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Among these, 4-hydroxybutyl (meth)acrylate and 2-hydroxyethyl (meth)acrylate are more preferred from the viewpoint of adhesion.

[0143] Examples of the amino group-containing monomer include monoalkylamino (meth)acrylates such as monomethylaminoethyl (meth)acrylate, monoethylaminoethyl (meth)acrylate, monomethylaminopropyl (meth)acrylate, and monoethylaminopropyl (meth)acrylate.

[0144] For the purpose of introducing unsaturated bonds into (meth) acrylic resin (a1), epoxy-containing monomers may also be used. As epoxy-containing monomers, for example, examples include: (meth) glycidyl acrylate, (meth) methyl glycidyl acrylate, (meth) 3,4-epoxycyclohexyl methyl ester, (meth) 6-methyl-3,4-epoxycyclohexyl methyl ester. Among these, from the viewpoint of reactivity, it is preferred to include (meth) glycidyl acrylate. Furthermore, it is preferred to react the epoxy group of the epoxy-containing monomer with the carboxyl group of the carboxyl-containing monomer such as (meth) acrylic acid to introduce unsaturated bonds such as (meth) acryloyl into (meth) acrylic resin (a1). At this time, the epoxy group is one or less in one molecule, and preferably no epoxy group remains.

[0145] The total amount of the structural units derived from the functional group-containing monomer is preferably 0.1% by mass to 20% by mass relative to 100% by mass of the (meth)acrylic resin (a1). By setting it within the above range, the cohesive force can be adjusted.

[0146] The content of the structural unit derived from the carboxyl group-containing monomer is preferably 0.1% to 10% by mass based on 100% by mass of the (meth)acrylic resin (a1). By being within the above range, the adhesion can be improved.

[0147] The content of the structural unit derived from the hydroxyl group-containing monomer is preferably 0.1% to 10% by mass based on 100% by mass of the (meth)acrylic resin (a1). By being within the above range, the adhesion can be improved.

[0148] The (meth)acrylic resin (a1) may also contain structural units derived from other monomers that can be copolymerized with the (meth)acrylic acid alkyl ester and the functional group-containing monomer. For example, monomers having an alkylene oxide group and other vinyl monomers can be cited. For example, methoxyethyl acrylate, methoxydiethylene glycol acrylate, vinyl acetate, crotonic acid vinyl ester, styrene, acrylonitrile, and acrylamide can be illustrated. The structural units derived from the other monomers are preferably 0.1% to 20% by mass in 100% by mass of the (meth)acrylic acid copolymer.

[0149] (Meth) acrylic resin (a1) can be obtained by polymerizing an acrylic monomer mixture. During polymerization, a polymerization initiator can be used as needed. The content of the polymerization initiator is set to, for example, 0.01% to 10% by mass relative to 100% by mass of the monomer mixture. The polymerization method is not limited. For example, polymerization can be carried out by solution polymerization, block polymerization, emulsion polymerization, and suspension polymerization. In terms of the ease of polymerization control, solution polymerization is particularly preferred. The solvent used in the solution polymerization can be exemplified by: acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl acetate, ethyl acetate, butyl acetate, toluene, xylene, anisole, cyclohexanone, isopropanol. The polymerization temperature can be set to, for example, about 60°C to 120°C, and the polymerization time can be set to about 2 hours to 12 hours.

[0150] The polymerization initiator is preferably a free radical polymerization initiator. As the free radical polymerization initiator, peroxides and azo compounds are suitable. Any of the thermal free radical polymerization initiators described below can be used, and specifically, 2,2'-azobisisobutyronitrile (abbreviation: AIBN (2,2'-azobisisobutyronitrile)) is preferred.

[0151] [Urethane resin (a2)]

[0152] In the present disclosure, the urethane resin (a2) refers to a compound containing two or more urethane bonds in one molecule. An example of the urethane resin (a2) is a urethane resin obtained by reacting polyisocyanate with polyol.

[0153] As long as the polyisocyanate has two or more isocyanate groups in one molecule, it is preferably a diisocyanate or a triisocyanate, and more preferably a diisocyanate in terms of the dispersibility of the colorant (B). As the diisocyanate, it can be appropriately selected from known aliphatic diisocyanates such as hexamethylene diisocyanate or known aromatic diisocyanates such as benzene-1,3-diisocyanate for use. In addition, an isocyanate-terminated prepolymer obtained by reacting a polyol with an excess of polyisocyanate can also be used as an intermediate of a urethane resin.

[0154] The polyol may be a substance having two or more hydroxyl groups in one molecule, and is preferably a diol or a triol, more preferably a diol, from the perspective of the dispersibility of the colorant (B). As the diol, it can be appropriately selected from known aliphatic diols such as ethylene glycol or known aromatic diols such as benzene glycol. In addition, prepolymers such as polyether polyols, polyester polyols, and polycarbonate polyols may also be used.

[0155] The urethane resin (a2) may be a polyurethane urea resin having a urea bond. The polyurethane urea resin can be synthesized by reacting, for example, a polyamine with a urethane resin having an isocyanate group at the terminal.

[0156] The polyamine may be a substance having two or more amino groups in one molecule, and is preferably a diamine or a triamine, and more preferably a diamine, from the perspective of the dispersibility of the colorant (B). The diamine may be appropriately selected from known aliphatic diamines such as ethylenediamine or known aromatic diamines such as phenylenediamine.

[0157] From the viewpoint of the dispersibility of the colorant (B), the urethane resin (a2) preferably further has a (meth)acryloyl group, N-vinyl group, vinyl ether group, allyl group, unsaturated carboxylic acid group, etc. as a free radical polymerizable functional group as a functional group, and more preferably has a (meth)acryloyl group. Specifically, the (meth)acryloyl group can be introduced by an addition reaction of the polyol, diisocyanate or triisocyanate with an acrylate having a hydroxyl group.

[0158] [Epoxy resin (a3)]

[0159] In the present disclosure, epoxy resin (a3) ​​refers to a compound having two or more epoxy groups in one molecule. Epoxy resin (a3) ​​also includes compounds formed by adding functional groups. As the functional group, it is preferred to have a (meth)acryloyl group, N-vinyl group, vinyl ether group, allyl group, unsaturated carboxylic acid group, etc. as a free radical polymerizable functional group, and it is further preferred to have a (meth)acryloyl group.

[0160] As for the properties of the epoxy resin (a3), the adhesiveness can be optimized by using the epoxy resin (a3) ​​in a liquid form, and the film-forming property of the resin composition layer can be optimized by using the epoxy resin (a3) ​​in a solid form.

[0161] As epoxy resin (a3), for example, glycidyl ether epoxy resin, glycidyl amine epoxy resin, glycidyl ester epoxy resin, cycloaliphatic (alicyclic) epoxy resin, bisphenol epoxy resin, hydrogenated bisphenol epoxy resin, etc. are preferred. In addition, from the viewpoint of adhesion, epoxy resin (a3) ​​is more preferably bisphenol epoxy resin, high-purity hydrogenated epoxy resin. As a compound having a free radical polymerizable functional group added to one or more epoxy groups as a functional group, bisphenol A diglycidyl ether diacrylate is preferred.

[0162] Examples of the glycidyl ether epoxy resin include cresol novolac epoxy resin, tris(glycidyloxyphenyl)methane, and tetrakis(glycidyloxyphenyl)ethane.

[0163] As a glycidylamine type epoxy resin, tetraglycidyldiaminodiphenylmethane and tetraglycidyl-meta-xylylenediamine are mentioned, for example.

[0164] As a glycidyl ester type epoxy resin, diglycidyl phthalate, diglycidyl hexahydrophthalate, diglycidyl tetrahydrophthalate etc. are mentioned, for example.

[0165] As a cyclic aliphatic (alicyclic) epoxy resin, epoxycyclohexylmethyl-epoxycyclohexanecarboxylate, bis(epoxycyclohexyl) adipate, etc. are mentioned, for example.

[0166] Examples of the bisphenol epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, and bisphenol AD ​​epoxy resin. From the viewpoint of adhesion, bisphenol A epoxy resin is particularly preferred.

[0167] As a hydrogenated bisphenol type epoxy resin, a hydrogenated bisphenol A type epoxy resin, a hydrogenated bisphenol F type epoxy resin, etc. are mentioned, for example. From the viewpoint of adhesiveness, a hydrogenated bisphenol A type epoxy resin is particularly preferable.

[0168] [Colorant (B)]

[0169] The colorant (B) may be any of an inorganic pigment, an organic pigment, and a dye, and may be toned by a mixed system. The hue is not particularly limited, but is preferably black from the viewpoint of light-shielding properties. Black may be obtained by subtractively mixing a plurality of pigments by a mixed system colorant. From the viewpoint of dispersibility, a black pigment is more preferred.

[0170] Examples of black pigments include carbon black, Ketjen black, carbon nanotube (CNT), perylene black, titanium black, iron black, aniline black, acetylene black, chromium iron oxide, etc. From the viewpoint of adhesion, carbon black is preferred.

[0171] As the carbon black used in the present disclosure, known carbon black such as channel black, furnace black, thermal black, and lamp black can be used.

[0172] Specific examples of carbon black include "Raven 3500, 1180, 1080 Ultra, 1060 Ultra, 1040" manufactured by Birla Carbon, "TOKABLACK #8300, #7360SB" manufactured by Tokai Carbon, "Special Black" manufactured by Orion Engineered Carbons, and "Special Black" manufactured by Orion Engineered Carbons. Black) 350, 250, 100, 550, 5, 4, 4A, 6", "Nipex 160IQ, 170IQ", "Printex U, V, 140U, 140V, 95, 90, 85, 80, 75, 55, 45, P, 60, L6, L, 300, 30, 3, 35, 25, A, G", "Color Black FW200, FW2, S170", "REGAL 400R, 330R, 250R" manufactured by Cabot, "Mogu ( "MOGUL)E, L", "MONARCH 1300, 280", "MA7, 8, 11, 14, 77, 100, 100R, 100S, 220, 230", "#2650, #2600, #2350, #2300, #1000, #980, #970, #960, #950, #900, #850, #750B, #650B, #52, #47, #45, #45L, #44, #40, #33, #32, #30, #25, #20, #10, #5, #95" manufactured by Mitsubishi Chemical Corporation, etc.

[0173] From the viewpoint of dispersibility, the carbon black preferably has a specific surface area of ​​50 m2 based on the Buehr method (BET). 2 / g~400m 2 / g, a volatile matter of 0.1 wt% to 10 wt%, and a pH value of 2 to 10, more preferably a carbon black having a pH value of 3 to pH 8, and further preferably a carbon black having a pH value of 3 to pH 6.

[0174] The colorant (B) preferably has an average primary particle diameter (hereinafter referred to as particle diameter) of 10 nm to 100 nm. By making the particle diameter more than 10 nm, it is easy to maintain the viscosity of the resin composition at a level suitable for coating. In addition, by making the particle diameter less than 100 nm, the blackness is improved, showing high light-shielding performance. In addition, when the particle shape of the colorant (B) has an average aspect ratio (major axis length / minor axis length) of more than 1.5, the particle diameter is obtained by averaging the major axis length.

[0175] The particle size of the colorant (B) can be determined from the average value of about 20 primary particles observed in an image magnified about 50,000 to 1,000,000 times by a transmission electron microscope (TEM).

[0176] The content of the colorant (B) is preferably 5% to 45% by mass, more preferably 15% to 35% by mass, and further preferably 20% to 30% by mass, based on the total amount (100% by mass) of the light-shielding layer. The reason for this is that by setting the content of the colorant (B) to 5% to 45% by mass, the light-shielding property is at an excellent level.

[0177] From the viewpoint that the film-forming property and light-shielding property of the resin composition layer are adjusted, it is preferred that the colorant (B) is dispersed in the resin (A) and used as a dispersion. As a dispersion, the disperser used in the mechanical crushing can be any disperser as long as it is a generally used disperser, and examples thereof include: a ball mill, a roller mill, a sand mill, a bead mill, and a nano machine. Among them, a bead mill is preferably used. As such a disperser, for example, a super mill, a sand mill, an agitator mill, a grain mill, a dyno mill, a pearl mill, and a cobol mill (all trade names) can be listed.

[0178] In the present disclosure, from the viewpoint of storage stability of the dispersion, it is preferred to use a dispersant in the dispersion treatment of the colorant (B). In the present disclosure, the dispersant has a function of imparting repulsion between particles to prevent the particles divided by the dispersion treatment from aggregating again.

[0179] As the dispersant, conventionally known compounds can be used, for example, cationic, anionic or nonionic surfactants, cationic, anionic or nonionic polymer dispersants, pigment derivative dispersants. From the viewpoint of storage stability of the dispersion, pigment derivative dispersants are preferred.

[0180] Pigment derivative dispersants are compounds having acidic groups, basic groups, neutral groups, etc. in the organic pigment residue. Examples include compounds having acidic substituents such as sulfonic groups, carboxyl groups, or phosphoric acid groups, and their amine salts, compounds having basic substituents such as sulfonamide groups, amide groups, or tertiary amino groups at the end, and compounds having neutral substituents such as phenyl or phthalimide alkyl groups. Examples of organic pigments include phthalocyanine pigments, diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perylene pigments, thiazine indigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzisoindole, isoindoline pigments, isoindoline ketone pigments, quinophthalone pigments, naphthol pigments, styrene pigments, metal complex pigments, azo pigments such as azo, disazo, and polyazo. By using these pigment dispersants, the colorant (B) contained in the resin composition can be prevented from aggregating over time, thereby maintaining good light-shielding properties.

[0181] Based on the total amount (100% by mass) of the resin composition layer, the content of the pigment dispersant (the total content when two or more are included) is preferably 0.01% by mass to 10% by mass, and more preferably 0.1% by mass to 5% by mass. By containing 0.01% by mass or more of the pigment dispersant, the light shielding property becomes good, and by being 10% by mass or less, the viscosity of the black dispersion becomes within an appropriate range, and the coating adaptability becomes good.

[0182] [Polymerization initiator (C)]

[0183] In the present embodiment, any one of a photopolymerization initiator and a thermal polymerization initiator can be used. From the viewpoint of film-forming property and adhesion of the resin composition layer, it is preferred to use a thermal polymerization initiator. When any one of a photopolymerization initiator and a thermal polymerization initiator is used, the resin (A) preferably has one or more free radical polymerizable functional groups as functional groups in one molecule. Examples of free radical polymerizable functional groups include: (meth)acryloyl, N-vinyl, vinyl ether, allyl, unsaturated carboxylic acid groups, and the like.

[0184] Examples of the photopolymerization initiator include triazine-based photopolymerization initiators, borate-based photopolymerization initiators, carbazole-based photopolymerization initiators, acetophenone-based photopolymerization initiators, and oxime-ester-based photopolymerization initiators. Acetophenone-based photopolymerization initiators and oxime-ester-based photopolymerization initiators are preferred because they are less yellowed during the heat aging process.

[0185] From the viewpoint of yellowing, the content of the photopolymerization initiator is preferably 0.5 to 10% by mass, more preferably 0.5 to 5% by mass, based on the total amount (100% by mass) of the resin composition layer.

[0186] In the present embodiment, a thermal cationic polymerization initiator or a thermal radical polymerization initiator can be used as the thermal polymerization initiator. From the viewpoint of the storage stability of the resin composition layer, a thermal radical polymerization initiator is preferred.

[0187] Thermal cationic polymerization initiators have the function of generating ions by heat. Regarding thermal cationic polymerization initiators, as cationic components, sulfonium cations, quaternary ammonium cations, iodonium cations, etc. can be listed. As anionic components, antimony hexafluoride anions, phosphorus hexafluoride anions, tetrakis(pentafluorophenyl)borate anions, trifluoromethanesulfonic acid, etc. can be listed.

[0188] The thermal radical polymerization initiator has a function of generating radicals by heat. Examples of the thermal radical polymerization initiator include organic peroxide polymerization initiators and azo thermal polymerization initiators.

[0189] Examples of the organic peroxide polymerization initiator include dialkyl peroxides such as diacetyl peroxide, di-tert-butyl peroxide, di-tert-hexyl peroxide, diisopropylbenzene peroxide, tert-butylisopropylbenzene peroxide, α,α′-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3,2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,3-bis(tert-butylperoxyisopropyl)hexane, and (2-ethylhexanoyl)(tert-butyl)peroxide;

[0190] Dipropionyl peroxide, tert-butyl peroxyacetate, tert-butyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, bis(3,5,5-trimethylhexanoyl)peroxide, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, α-isopropylphenyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneoheptanoate, tert-hexyl peroxyvalerate, tert-butyl peroxyvalerate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoic acid Peroxyesters such as tert-butyl peroxyisobutyrate, di-tert-butyl peroxyhexahydroterephthalate, 1,1,3,3-tetramethylbutyl peroxy-3,5,5-trimethylhexanoate, tert-amyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, dibutyl peroxytrimethyladipate, 2,5-dimethyl-2,5-di-ethylhexanoyl peroxyhexane, tert-hexyl peroxy-2-ethylhexanoate, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxylaurate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate;

[0191] Ketone peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, acetylacetone peroxide, cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, methylcyclohexanone peroxide, tert-butyl benzoate, and pivaloyl tert-butyl peroxide;

[0192] Peroxy ketals such as 2,2-bis(tert-butylperoxy)butane, 2,2-bis(4,4-di-tert-butylperoxycyclohexyl)propane, 1,1-bis(tert-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, and 4,4-bis(tert-butylperoxy)butyl valerate;

[0193] Hydroperoxides such as tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, 2,5-dimethylcyclohexane-2,5-dihydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and p-methane hydroperoxide;

[0194] Diacyl peroxides such as dibenzoyl peroxide, didecanoyl peroxide, dilauroyl peroxide, diisobutyryl peroxide, bis-3,5,5-trimethylhexanol peroxide, m-toluoylbenzoyl peroxide, succinic acid peroxide, 2,4-dichlorobenzoyl peroxide;

[0195] Peroxydicarbonates such as bis(tert-butylcyclohexyl)peroxydicarbonate, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, tert-butylperoxyisopropyl carbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, tert-amylperoxyisopropyl carbonate, tert-butylperoxy-2-ethylhexyl carbonate, and 6-bis(tert-butylperoxycarboxyoxy)hexane are not limited thereto.

[0196] From the viewpoint of storage stability, dialkyl peroxides are preferred, and di-tert-butyl peroxide is more preferred.

[0197] Examples of the azo thermal polymerization initiator include 2,2'-azobisisobutyronitrile and 2,2'-azobis(2-methylbutyronitrile);

[0198] 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile) and other 2,2'-azobisvaleronitriles;

[0199] 1,1'-azobis(cyclohexane-1-carbonitrile) and other 1,1'-azobis-1-alkanenitrile; 2,2'-azobis(2-hydroxymethylpropionitrile) and other 2,2'-azobispropionitrile;

[0200] 2,2'-azobispropionamides such as 2,2'-azobis(N-butyl-2-methylpropionamide) and 2,2'-azobis(N-cyclohexyl-2-methylpropionamide);

[0201] As well as dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 1-[(1-cyano-1-methylethyl)azo]formamide, etc.

[0202] Examples of the azo compound having a carboxyl group or a hydroxyl group include, but are not limited to, 4,4'-azobis(4-cyanovaleric acid), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide), and 2,2'-azobis(N-(carboxyethyl)-2-methylpropionamidine) tetrahydrate.

[0203] From the viewpoint of storage stability, 2,2'-azobispropionamides are preferred, and 2,2'-azobis(N-butyl-2-methylpropionamide) is more preferred.

[0204] The 10-hour half-life temperature of the thermal radical polymerization initiator is preferably 60° C. to 200° C., more preferably 80° C. to 180° C., further preferably 100° C. to 150° C., and particularly preferably 105° C. to 130° C. By setting the temperature to 60° C. or higher, the storage stability of the resin composition layer can be improved, and by setting the temperature to 200° C. or lower, the heat aging step of the sealant layer can be shortened.

[0205] The 10-hour half-life temperature is the temperature at which the thermal polymerization initiator is reduced to half of the initial value by thermal decomposition after 10 hours. Specifically, for the free radicals of the thermal polymerization initiator, a thermal polymerization initiator solution is prepared using an inert solvent and sealed in a glass tube after nitrogen substitution. It is immersed in a constant temperature layer set to a specified temperature for 10 hours and thermally decomposed, and the amount of the remaining thermal polymerization initiator is measured. By performing these series of operations at several temperatures, the half-life can be calculated based on the straight line obtained by drawing.

[0206] The content of the thermal radical polymerization initiator is preferably 0.01 to 20% by mass, more preferably 0.05 to 10% by mass, and still more preferably 0.1 to 5% by mass, based on the total amount (100% by mass) of the resin composition layer. By setting the content to such a level, the adhesion can be appropriately adjusted.

[0207] [Other ingredients]

[0208] The resin composition layer of the present disclosure may contain other components within the scope that does not impair the purpose of the present disclosure, such as a crosslinking agent, a monomer, an inorganic filler, a surface conditioning additive, a hardening accelerator, a hardening retarder, a softener, an antistatic agent, a lubricant, an anti-caking agent, an adhesion improver, etc.

[0209] From the viewpoint of controlling the film-forming property of the resin composition layer, it is preferred to contain a crosslinking agent and a monomer.

[0210] Examples of the inorganic filler include inorganic compounds such as silicon dioxide, aluminum oxide, magnesium hydroxide, barium sulfate, calcium carbonate, titanium oxide, zinc oxide, antimony trioxide, magnesium oxide, zirconium oxide, talc, kaolinite, mica, basic magnesium carbonate, sericite, montmorillonite, bentonite, boron nitride, aluminum nitride, and titanium nitride. Among these, titanium oxide, titanium nitride, silicon dioxide, and zirconium oxide are preferred from the viewpoint of the coating film resistance to scratches.

[0211] In order to adjust the crosslinking speed of the resin composition layer of the present disclosure, a hardening accelerator may be contained. The hardening accelerator is not particularly limited and can be selected appropriately. Specific examples of the hardening accelerator include, for example, amine-based hardening accelerators, guanidine-based hardening accelerators, and metal-based hardening accelerators.

[0212] [Crosslinking agent]

[0213] The resin composition layer of the present disclosure may also contain a crosslinking agent. The crosslinking agent undergoes a crosslinking reaction with the reactive functional groups of the resin (A) during hot pressing or heat aging in the pressing process, thereby increasing the cohesive force of the resin composition layer and improving the adhesion. The crosslinking agent has a plurality of functional groups that can react with the functional groups of the resin (A). Examples of the crosslinking agent include known compounds such as silane coupling agents, anhydride group-containing compounds, imidazole compounds, isocyanate compounds, aziridine compounds, and amine compounds. From the perspective of adjusting the loss tangent (tanδ) of the resin composition layer, silane coupling agents, aziridine compounds, and imidazole compounds are preferred.

[0214] Examples of the aziridine compound include trimethylolpropane tris[3-(aziridin-1-yl)propionate], tetramethylolmethane-tris-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane.

[0215] Examples of the imidazole compound include 2-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-dimethylimidazole, 2-phenylimidazole, imidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitic acid, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. Further examples include compounds having improved storage stability such as those obtained by encapsulating the imidazole compound in microcapsules.

[0216] The isocyanate compound is an isocyanate having two or more isocyanate groups and is preferably an isocyanate monomer such as aromatic polyisocyanate, aliphatic polyisocyanate, aromatic aliphatic polyisocyanate, alicyclic polyisocyanate, and a biuret form, urate form, and adduct thereof.

[0217] From the viewpoint of forming a sufficient cross-linked structure, the isocyanate compound is preferably a trifunctional isocyanate compound. The isocyanate compound is more preferably an adduct of a reaction product of an isocyanate monomer and a trifunctional compound containing low molecular active hydrogen, and a urate body. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a urate body of hexamethylene diisocyanate, a trimethylolpropane adduct of toluene diisocyanate, a urate body of toluene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, and a urate body of isophorone diisocyanate, more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of toluene diisocyanate, and a trimethylolpropane adduct of isophorone diisocyanate.

[0218] The silane coupling agent is a compound in which a hydrolyzable group such as a methoxy group or an ethoxy group and a functional group such as an epoxy group are bonded to a Si atom via an alkylene group.

[0219] Examples of the silane coupling agent include alkoxysilane compounds having a (meth)acryloxy group such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropyltripropoxysilane, 3-(meth)acryloxypropyltributoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane;

[0220] Alkoxysilane compounds having a vinyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltributoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane;

[0221] Alkoxysilane compounds having an amino group such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltripropoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane;

[0222] Alkoxysilane compounds having a mercapto group such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropylmethyldiethoxysilane;

[0223] Alkoxysilane compounds having one epoxy group, such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltripropoxysilane, 3-glycidoxypropyltributoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane;

[0224] Tetraalkoxysilane compounds such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane;

[0225] 3-Chloropropyltrimethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-decyltrimethoxysilane, n-decyltriethoxysilane, styryltrimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylene)propylamine, 1,3,5-tris(3-trimethoxysilylpropyl)isocyanurate, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, hexamethyldisilazane, silicone resin having an alkoxysilyl group in the molecule, and the like.

[0226] From the viewpoint of adhesion, an alkoxysilane compound is preferred, and 3-glycidyloxypropyltrimethoxysilane is more preferred.

[0227] The content of the crosslinking agent is preferably 0.01 to 30% by mass, more preferably 0.05 to 20% by mass, and still more preferably 0.1 to 10% by mass, based on the total amount (100% by mass) of the resin composition layer. By setting the content to such a level, the adhesion can be appropriately adjusted.

[0228] [monomer]

[0229] The monomer used in the resin composition of the present disclosure refers to a compound having a free radical polymerizable functional group added to the resin composition. As free radical polymerizable functional groups, for example, (meth) acryloyl, N-vinyl, vinyl ether, allyl, unsaturated carboxylic acid group, etc. can be cited. In addition, the monomer can be a monofunctional monomer or a polyfunctional monomer. In addition, "monofunctional" in this specification refers to a compound having only one free radical polymerizable functional group in one molecule, and "difunctional" and "trifunctional" refer to compounds having two and three free radical polymerizable functional groups in one molecule, respectively. In addition, in this specification, difunctional and above are collectively referred to as "polyfunctional". By containing monomers, the film-forming property of the resin composition layer is adjusted, and the adhesion becomes good.

[0230] Specific examples of the monomer include: a monofunctional (meth)acrylate monomer having one (meth)acryloyl group in the molecule, a monofunctional vinyl monomer having one N-vinyl group in the molecule, a difunctional (meth)acrylate monomer having two (meth)acryloyl groups in the molecule, a difunctional (meth)acrylate monomer having one (meth)acryloyl group and one allyl group in the molecule, a trifunctional (meth)acrylate monomer having three (meth)acryloyl groups in the molecule, a tetrafunctional (meth)acrylate monomer having four acryloyl groups in the molecule, a pentafunctional (meth)acrylate monomer having five (meth)acryloyl groups in the molecule, a hexafunctional (meth)acrylate monomer having six (meth)acryloyl groups in the molecule, etc., but the monomers are not limited thereto.

[0231] Among these, from the viewpoint of adhesion, it is preferred to contain 3-((meth)acryloxy)propyltrimethoxysilane and 3-((meth)acryloxy)propyltriethoxysilane.

[0232] The content of the monomer is preferably 0.01 to 30% by mass, more preferably 0.05 to 20% by mass, and still more preferably 0.1 to 15% by mass, based on the total amount (100% by mass) of the resin composition layer. Adhesion can be appropriately adjusted by setting the content to this level.

[0233] [Example]

[0234] Hereinafter, the present disclosure will be specifically described by way of Examples and Comparative Examples, but the present disclosure is not particularly limited to the Examples. In the following description, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified.

[0235] (a) Determination method

[0236] The numerical values ​​obtained in the present examples are values ​​obtained by the following method.

[0237] [Weight average molecular weight (Mw)]

[0238] The weight average molecular weight (Mw) was determined by using GPC "LC-GPC System" manufactured by Shimadzu Corporation and converting polystyrene having a known molecular weight as a standard substance.

[0239] Device name: LC-GPC system "Prominence" manufactured by Shimadzu Corporation

[0240] Pipe string: Four GMHXL pipes manufactured by Tosoh and one HXL-H pipe manufactured by Tosoh were connected.

[0241] Mobile phase solvent: tetrahydrofuran

[0242] Flow rate: 1.0mL / min

[0243] Column temperature: 40℃

[0244] [Solid content]

[0245] The mass of the aluminum cup is measured using a precision balance (W0). Then, about 1 g of the sample is placed in the aluminum cup, and the mass of the sample with the aluminum cup is measured using a precision balance (W1). The sample with the aluminum cup is heated in an oven at 150°C for 120 minutes, then taken out of the oven and returned to room temperature. The residual mass (W2) of the heated sample with the aluminum cup is measured using a precision balance. Thereafter, the solid content is calculated using the formula (W2-W0) / (W1-W0)×100(%).

[0246] [Thickness Tt of Sealing Sheet, Thickness Ta of Resin Composition Layer, Thickness Tl of First Film, Thickness Th of Second Film]

[0247] Determine 10 equally spaced locations within the range from the end in the width direction to the other end of a sealing sheet cut into a size of 10 cm × 10 cm, measure the thickness of the 10 locations, and set the average value thereof as the thickness Tt of the sealing sheet. Next, peel off the first film from the sealing sheet, and measure the thickness of the first film after peeling at 10 locations corresponding to the same position as the location. Set its average value as Tl. Thereafter, further peel off the second film from the resin composition layer, and measure the thickness of the second film after peeling at 10 locations corresponding to the same position as the location. Set its average value as Th. The thickness Ta of the resin composition layer is obtained by the formula Ta=Tt-Tl-Th. In addition, the thickness is measured using MH-15M (manufactured by Nikon).

[0248] [Loss tangent (tanδ) of resin composition layer]

[0249] The sealing sheet prepared in such a way that the thickness Ta of the resin composition layer becomes 50 μm is cut into a size of 0.5 cm×2 cm, and the first film and the second film are peeled off. For the obtained resin composition layer, the dynamic viscoelasticity measuring device DVA-200 / L2 (manufactured by IT Measurement and Control Co., Ltd.) is used to measure the dynamic viscoelasticity and plot the loss tangent (tanδ) at a frequency of 10 Hz, a measurement temperature range of -50°C to 150°C, a heating rate of 5°C / min, and a tensile mode. The maximum value (tanδ maximum value) of the loss tangent (tanδ), the loss tangent at 40°C (tanδ40°C), and the peak temperature of the loss tangent (tanδ peak temperature) are read from the obtained curve graph.

[0250] [Young's modulus of the second film]

[0251] For the second film, the stress-strain curve was measured by a tensile testing machine "EZ Tester" (manufactured by Shimadzu Corporation) under the conditions of 23°C, 50% relative humidity, a tensile speed of 50 mm / min and 25 mm between markings, and the linear regression (slope) in the region where the strain (elongation) was 0.1% to 0.3% was taken as the Young's modulus.

[0252] [Pencil hardness]

[0253] The first film of the sealing sheet was peeled off, and the exposed surface of the resin composition layer was measured according to the test method of Japanese Industrial Standards (JIS) K 5600-5-4. The pencil used was a pencil for pencil hardness test (manufactured by Mitsubishi Pencil Co., Ltd.).

[0254] (b) Preparation of a solution of resin (A)

[0255] [Example of Preparation of (Meth)Acrylic Resin (a1) (A-1) Solution]

[0256] In a reaction container (hereinafter simply referred to as "reaction container") including a stirrer, a thermometer, a reflux cooling tube, a dropping device, and a nitrogen introduction tube, 80 parts of ethyl acetate, 13 parts of n-butyl acrylate, 85 parts of n-butyl methacrylate, 2 parts of methacrylic acid, and 0.1 parts of 2,2'-azobisisobutyronitrile as an initiator were placed, and the atmosphere in the reaction container was replaced with nitrogen. Thereafter, the reaction was started by heating to 65°C while stirring under a nitrogen atmosphere. Thereafter, the reaction solution was reacted at 65°C for 4 hours. After the reaction was completed, the solution was cooled and diluted with ethyl acetate to obtain a solution of (meth)acrylic resin (a1) (A-1) having a weight average molecular weight (Mw): 100,000 and a solid content: 25%.

[0257] [Example of Preparation of Solution of (Meth)Acrylic Resin (a1) (A-2)]

[0258] (Meth)acrylic resin (a1) (A-2) was prepared by the same method as (meth)acrylic resin (a1) (A-1) except that the monomer blending amount was changed to 20 parts of n-butyl acrylate, 70 parts of n-butyl methacrylate, 5 parts of methacrylic acid, and glycidyl methacrylate. In addition, the weight average molecular weight (Mw) was 130,000, and the solid content was 25%.

[0259] [Example of Preparation of Solution of (Meth)Acrylic Resin (a1) (A-3)]

[0260] KRM8912 (manufactured by Daicel-Allnex) was diluted with ethyl acetate to prepare a (meth)acrylic resin (a1) (A-3). The weight average molecular weight (Mw) was 1,000 and the solid content was 25%.

[0261] [Production Example of Solution of Urethane Resin (a2) (A-4)]

[0262] Art Resin UN-9000PEP (manufactured by Negami Industries) was diluted with ethyl acetate to prepare a urethane resin (a2) (A-4). The weight average molecular weight (Mw) was 5,000 and the solid content was 25%.

[0263] [Example of Preparation of Solution of Epoxy Resin (a3) ​​(A-5)]

[0264] Epoxy resin (a3) ​​(A-5) was prepared by diluting jER256B40 (manufactured by Mitsubishi Chemical Corporation) with ethyl acetate. The weight average molecular weight (Mw) was 45,000, and the solid content was 25%.

[0265] (c) Preparation of dispersion of colorant (B)

[0266] [Production Example of Dispersion (D-1) of Colorant (B)]

[0267] 800 parts of a solution of a resin (A-1), 800 parts of carbon black MA100 (manufactured by Mitsubishi Chemical Corporation) as a colorant (B-1), and 400 parts of methyl ethyl ketone as a solvent were mixed and pre-dispersed using a disperser. Then, a formal dispersion was carried out for 2 hours using a 0.6 L Dyno mill filled with 1800 g of zirconia beads with a diameter of 1.0 mm to prepare a dispersion (D-1).

[0268] [Production Example of Dispersion (D-2) of Colorant (B)]

[0269] 800 parts of a solution of resin (A-2), 800 parts of carbon black MA100 (manufactured by Mitsubishi Chemical Corporation) as a colorant (B-1), 400 parts of methyl ethyl ketone as a solvent, and 2 parts of Solsperse 5000 (manufactured by Lubrizol) as a pigment derivative dispersant were mixed and pre-dispersed using a disperser. Then, a formal dispersion was carried out for 2 hours using a 0.6 L Dyno mill filled with 1800 g of zirconia beads with a diameter of 1.0 mm to prepare a dispersion (D-2).

[0270] [Production Example of Dispersion (D-3) of Colorant (B)]

[0271] 800 parts of a solution of resin (A-1), 800 parts of Black 6340 (manufactured by Asahi Chemicals Co., Ltd.) as a metal oxide pigment as a colorant (B-2), and 400 parts of methyl ethyl ketone as a solvent were mixed and pre-dispersed using a disperser. Then, a formal dispersion was carried out for 2 hours using a 0.6 L Dyno mill filled with 1800 g of zirconia beads with a diameter of 1.0 mm to prepare a dispersion (D-3).

[0272] (d) Production of resin composition

[0273] [Production Example of Resin Composition of Example 1]

[0274] Dispersion (D-1): 60 parts (24 parts of colorant (B-1), 6 parts of resin (A-1), 30 parts of solvent), solution of resin (A-1): 276 parts (69 parts of resin (A-1), 207 parts of solvent), 1 part of Chemitite PZ-33 (manufactured by Nippon Catalyst Co., Ltd.) as an aziridine compound, and 63 parts of toluene as a solvent were added in sequence while stirring with a disperser, and stirred until fully uniform. Then, the mixture was filtered with a membrane filter having a pore size of 10 μm to remove coarse foreign matter that causes uneven coating, thereby obtaining a resin composition having a non-volatile component of 33%. In addition, other components are set as solid content conversion amounts.

[0275] (e) Manufacturing of sealing sheet

[0276] [Manufacturing Example of Sealing Sheet of Example 1]

[0277] The resin composition was applied to the release layer of SP-PET-O3-BU (Mitsui Chemicals Tohcello) as the second film (H-2) with a thickness of 50 μm in a manner to have a thickness of 20 μm after drying, and dried in a hot air oven at 100°C for 3 minutes to form a resin composition layer. Next, the release layer side of (L-2) SP-PET-O1-T (Mitsui Chemicals Tohcello) as the first film with a thickness of 25 μm was bonded to the exposed resin composition layer, and aged at 0°C for 7 days to obtain a sealing sheet of Example 1 stacked in the order of first film / resin composition layer / second film. In addition, the tanδ peak temperature was 29°C.

[0278] (f) Evaluation method of sealing sheet

[0279] [Embeddability]

[0280] Prepare a test substrate that simulates the concave and convex patterns of a micro-LED substrate (a plate with a concave portion with a width of 200 μm, a convex portion with a height of 5 μm, and a convex portion with a width of 200 μm formed on one surface of a 25 mm × 25 mm glass plate). Figure 3 middle.

[0281] The sealing sheet is cut into a size of 30 mm × 30 mm, the first film is peeled off to expose the resin composition layer, and the resin composition layer is placed on the surface of the test substrate with a concave-convex portion. Thereafter, TPX (Opulent X-44B, manufactured by Mitsui Chemicals Tohcello) with a thickness of 50 μm and a vinyl chloride film (Celeb T, manufactured by Okamoto) with a thickness of 2.0 mm are sequentially stacked on the second film as a buffer material, and then cardboard is stacked to prevent sticking. The laminate comprising a glass substrate / resin composition layer / second film / buffer material (TPX / vinyl chloride film) / cardboard is pressed from above to the substrate surface under the conditions of 5 MPa and 100 ° C for 20 minutes, so that the resin composition layer is filled into the concave portion of the test substrate, thereby forming a sealing layer. After pressing, the buffer material and the cardboard are peeled off.

[0282] The sealing layer extending from the side of the obtained test substrate with a sealing layer is roughly removed using a cutter, and then filed to remove the sealing layer remaining on the side of the test substrate with a sealing layer, exposing the side of the test substrate, thereby making it possible to observe the concave and convex parts. The embedding property is evaluated by observing the concave parts of the test substrate at any 15 locations using a microscope. The groove is considered to be embedded when the maximum gap between the sealing layer and the test substrate in the concave part of the test substrate is less than 1 μm. The evaluation criteria are as follows.

[0283] A: There are more than 14 buried grooves

[0284] B: The number of buried grooves is less than 13 and more than 11

[0285] C: The number of buried grooves is less than 10 and more than 8

[0286] D: The number of buried grooves is less than 7

[0287] [Die displacement]

[0288] LEDs with wiring (SMD, 0402, 1.0 mm x 0.5 mm in size) were placed on a general-purpose glass epoxy substrate (32 mm wide x 53 mm deep x 1.2 mm thick, 2.54 mm pitch), and the conduction of electricity to the LEDs was confirmed to prepare a test substrate.

[0289] The sealing sheet is cut into a size of 60 mm × 60 mm, and the first film is peeled off to expose the resin composition layer, and the resin composition layer is placed in a manner that the LED arranged on the test substrate is in contact with it. Subsequently, TPX (Opulent X-44B, manufactured by Mitsui Chemicals Tohcello) with a thickness of 50 μm and a vinyl chloride film (Celeb T, manufactured by Okamoto) with a thickness of 2.0 mm are sequentially stacked on the second film as a buffer material, and then cardboard is stacked to prevent sticking. The laminate has a structure of glass substrate / resin composition layer / second film / buffer material (TPX / vinyl chloride film) / cardboard. Next, the substrate surface is pressed from the top of the test piece under the conditions of 5 MPa and 100 ° C for 20 minutes to fill the resin composition layer around the LED, thereby forming a sealing layer. After pressing, the buffer material and the cardboard are peeled off. Use a power-on tester to confirm the power-on of the LED on the obtained pressed test piece. The LEDs that were not powered were considered to have wiring displacement due to the displacement of the bare chip during embedding, and were evaluated as having wiring displacement. This evaluation was conducted 10 times, and the evaluation criteria were as follows.

[0290] A: There is wiring deviation 0 to 1 time

[0291] B: There are 2 wiring deviations

[0292] C: There are 3 wiring deviations

[0293] D: There are 4 to 10 wiring deviations

[0294] [Light blocking properties]

[0295] The first film and the second film of the sealing sheet were peeled off to expose the resin composition layer. The optical density (visual) of the resin composition layer was measured using an optical densitometer (361T tabletop transmission densitometer, manufactured by X-Rite). The evaluation criteria are as follows.

[0296] A: Optical density is 6 or more

[0297] B: Optical density is 4 or more and less than 6

[0298] C: Optical density less than 4

[0299] [Tightness]

[0300] Prepare a sealing sheet obtained by cutting the sealing sheet into 25mm×100mm, peel off the first film to expose the resin composition layer, and place it on a glass plate (25mm×100mm×1.1mm, blue plate glass, manufactured by Kawamura Jiuzhang Store). Thereafter, TPX (Opulent X-44B, manufactured by Mitsui Chemicals Tohcello) with a thickness of 50μm and a vinyl chloride film (Celeb T, manufactured by Okamoto) with a thickness of 2.0mm as a buffer material are sequentially stacked on the second film, and then cardboard is stacked to prevent sticking. The laminate comprising a glass plate / resin composition layer / second film / buffer material (TPX / vinyl chloride film) / cardboard is pressed from above to the substrate surface under the conditions of 5MPa and 100°C for 20 minutes, and the glass plate and the resin composition layer are pressed together to form a sealing layer on the glass plate. After pressing, the buffer material, cardboard, and second film are peeled off. A test piece including a glass plate and a sealing layer was left to stand at 180° C. for 120 minutes to prepare a test piece in which the glass plate and the sealing layer were in close contact with each other.

[0301] According to JIS K 5600-5-6 (cross-cut method), a 1 mm square right-angle grid pattern (25 grids) was made on the sealing layer of the test piece using a cross-cut guide and a cutting knife, and an adhesive tape (CT1835, manufactured by Nichiban) was attached to the grid-cut portion to be in close contact with the sealing layer. Within 5 minutes of attachment, the seal was peeled off at an angle of nearly 60° for 0.5 to 1.0 seconds. The condition of the peeled sealing layer was observed and the adhesion was evaluated. The evaluation criteria are as follows. In addition, the situation where the sealing layer peeled off from the glass plate when peeling off the second film was set as C evaluation.

[0302] A: The number of cells peeled off is 0

[0303] B: 1 to 2 cells peeled off

[0304] C: 3 to 25 peeling grids

[0305] In any of the above evaluations, the best evaluation is A, the second best evaluation is B, the next best evaluation is C, and the evaluation that does not reach the target performance is D. In addition, it is consistent with the present disclosure that all performance evaluations are A to C.

[0306] [Example 2 to Example 25], [Comparative Example 1 to Comparative Example 8]

[0307] A sealing sheet was prepared and evaluated in the same manner as in Example 1 except that the content and thickness Ta were changed to those shown in Tables 1 to 3. In addition, any other components were also added at the same time.

[0308] In Tables 1 to 3, the resin (A), colorant (B), polymerization initiator (C) and other components are in terms of solid content, and blank columns indicate that they were not blended. In addition, the tan δ peak temperature of Example 2 was 22°C.

[0309] The abbreviations in the table are as follows.

[0310] C-1: di-tert-butyl peroxide (Perbutyl D, manufactured by NOF Corporation)

[0311] C-2: 2,2'-azobis(N-butyl-2-methylpropionamide) (VAm-110, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0312] O-1: Aziridine compound as a crosslinking agent (Chemitite PZ-33, manufactured by Nippon Catalyst Co., Ltd.)

[0313] O-2: Silane coupling agent as a crosslinking agent (KBE-403, manufactured by Shin-Etsu Silicone Co., Ltd.)

[0314] O-3: 2-phenylimidazole as a crosslinking agent (Curezol 2PZ, manufactured by Shikoku Chemical Industry Co., Ltd.)

[0315] O-4: Ethylene oxide (EO)-modified (3) trimethylolpropane triacrylate (Miramer M3130, manufactured by MIWON, trifunctional) as a monomer

[0316] O-5: 3-methacryloxypropyltrimethoxysilane (KBE-503, manufactured by Shin-Etsu Silicone Co., Ltd., monofunctional) as a monomer

[0317] L-1: First film with a thickness of 10 μm (matte film (type M3), manufactured by IM, Sq: 1.5 μm)

[0318] L-2: First film with a thickness of 25 μm (SP-PET-O1-T, manufactured by Mitsui Chemicals Tohcello, Sq: 0.2 μm)

[0319] L-3: First film with a thickness of 50 μm (matte film (type M3), manufactured by IM, Sq: 1.5 μm)

[0320] L-4: First film with a thickness of 100 μm (SP-PET-O1-T, manufactured by Mitsui Chemicals Tohcello, Sq: 0.2 μm)

[0321] H-1: Second film with a thickness of 12 μm (Torayfan High-End OPP film, manufactured by Toray Industries, Ltd., Young's modulus: 3.5 GPa)

[0322] H-2: Second film with a thickness of 50 μm (SP-PET-O3-BU, manufactured by Mitsui Chemicals Tohcello, Young's modulus: 4.7 GPa)

[0323] H-3: Second film with a thickness of 100 μm (release film PE, manufactured by IM Co., Ltd., Young's modulus: 1.1 GPa)

[0324] H-4: Second film with a thickness of 188 μm (Cosmo Peel E7004, manufactured by Toyobo Co., Ltd., Young's modulus: 5.9 GPa)

[0325] H-5: Second film with a thickness of 6 μm (Lumirror F53, manufactured by Toray Industries, Ltd., Young's modulus: 4.4 GPa)

[0326] H-6: 250 μm thick second film (Lumirror T60, manufactured by Toray Industries, Ltd., Young's modulus: 4.8 GPa)

[0327]

[0328]

[0329]

[0330] In the present disclosure, in the case of a sealing sheet where the thickness Ta of the resin composition layer is outside the range of 2 μm to 100 μm and Ta and the thickness Th of the second film do not satisfy the relationship of 0.1≦Ta / Th≦2, as shown in Comparative Examples 1 and 2, it is found that there are problems with embedding properties and die shifting properties.

[0331] In the case of a sealing sheet having a second film thickness Th outside the range of 12 μm to 188 μm and not satisfying the relationship of 0.1≦Ta / Th≦2, as shown in Comparative Examples 3 and 4, there are problems with embedding properties and die shifting properties.

[0332] In addition, in the case of a sealing sheet that does not satisfy the relationship of 0.1≦Ta / Th≦2, as shown in Comparative Examples 5 and 6, it is found that there are problems in one or more of embedding property and die shifting property.

[0333] In addition, when the maximum value of the loss tangent (tanδ maximum value) of the resin composition layer obtained by dynamic viscoelasticity measurement in the range of -50°C to 80°C is outside the range of 0.6 to 2.2, as shown in Comparative Examples 7 and 8, there are problems with either embedding property or die shifting property.

[0334] As shown in Table 3, the sealing sheets of Comparative Examples 1 to 8 cannot satisfy both embedding property and die shifting property at a well-balanced and high level.

[0335] In contrast, according to Examples 1 to 25, as described in Tables 1 to 3, the sealing sheet of the present disclosure exhibits excellent embedding properties and excellent bare die shifting properties. Furthermore, it was found that the sealing sheet of the present disclosure is excellent in light controllability because it is also excellent in light shielding properties or adhesion, thereby preventing light leakage due to insufficient light shielding power or light leakage from gaps in the sealing layer due to poor adhesion, thereby ensuring visibility of the display.

Claims

1. A sealing sheet for sealing a micro-light emitting diode used in a display using the micro-light emitting diode as a light source, The sealing sheet is sequentially provided with a first film, a resin composition layer and a second film, The first film has a release layer on a surface facing the resin composition layer. The thickness Ta of the resin composition layer is 2 μm to 100 μm, The thickness Th of the second film is 12 μm to 188 μm, Ta and Th satisfy formula (1), The maximum value of the loss tangent of the resin composition layer obtained by dynamic viscoelasticity measurement in the range of -50°C to 80°C is 0.6 to 2.2, Formula (1): 0.1≦Ta / Th≦2.

2. The sealing sheet according to claim 1, wherein: The Young's modulus of the second film is 1 GPa to 6 GPa.

3. The sealing sheet according to claim 1, wherein: The ratio of the root mean square height Sq of the surface of the first film in contact with the resin composition layer as specified in ISO 25178 to the thickness Ta of the resin composition layer is 30% or less.

4. The sealing sheet according to claim 1, wherein: The pencil hardness of the resin composition layer is 5B-2H.

5. The sealing sheet according to any one of claims 1 to 4, wherein: The resin composition layer comprises a resin (A), The resin (A) includes at least one selected from the group consisting of acrylic resin (a1), urethane resin (a2), and epoxy resin (a3).

6. The sealing sheet according to claim 5, wherein: The resin composition layer contains a colorant (B).

7. The sealing sheet according to claim 6, wherein: The resin composition layer contains a polymerization initiator (C).

8. A display using a micro light emitting diode having a resin composition layer of the sealing sheet according to claim 5 as a light source.

9. A method for manufacturing a display using a micro-light emitting diode as a light source, comprising the following steps (1) to (6): (1) a step of preparing a sealing sheet according to claim 1 to 4 in which a first film, a resin composition layer for forming a sealing layer, and a second film are sequentially arranged; (2) a step of preparing a sealing object in which a plurality of micro light-emitting diodes are arranged at intervals from each other on one surface of a substrate; (3) a step of peeling the first film from the sealing sheet to expose the resin composition layer for forming a sealing layer; (4) a step of placing the exposed resin composition layer for forming a sealing layer so as to cover the plurality of micro light-emitting diodes; (5) a step of flowing a resin composition layer for forming a sealing layer and filling the space between the plurality of micro light-emitting diodes; (6) A step of peeling off the second film.

Citation Information

Patent Citations

  • Thermosetting resin composition

    JP2023012051A

  • Optical semiconductor device sealing sheet

    WO2021200035A1

  • Semiconductor package, core layer material, buildup layer material, and sealing resin composition

    CN102790018A

  • Micro LED light emitting device and manufacturing method thereof

    CN113130459A

  • Sheet for sealing optical semiconductor element

    CN115397870A