Low-temperature-resistant flexible binder prepared from polyoxometalate and lipoic acid
A flexible adhesive composed of polymetallic oxygen clusters and thioctic acid addresses the limitations of traditional adhesives by offering high adhesion and stability in extreme cold, enhancing performance in low-temperature environments.
Patent Information
- Application Number
- CN202411354158.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
AI Technical Summary
Existing adhesives struggle with high crosslinking density, low surface energy, poor interfacial penetration, freezing at low temperatures, and insufficient stability, limiting their effectiveness in extreme cold environments such as the Arctic and outer space.
A low-temperature resistant flexible adhesive is developed using polymetallic oxygen clusters and thioctic acid through in-situ polymerization, with a composition of 25%-75% polymetallic oxygen clusters and the balance of thioctic acid, providing high adhesion, organic solvent stability, and long-term ultra-low temperature resistance.
The adhesive exhibits strong adhesion (up to 3.5MPa), stability in organic solvents, and maintains performance from -196°C to 50°C, withstanding multiple folds and bends without losing adhesive properties, outperforming commercial hot-melt adhesives in flexibility and temperature range.
Smart Images

Figure CN119081636A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation and application of low-temperature resistant flexible adhesive materials, and in particular to a low-temperature resistant flexible adhesive prepared from polyoxometalates and thioctic acid. Background Art
[0002] Adhesives play an important role in many fields such as textiles, electronics, and aerospace. With the sustainable development of society and industry, the actual demand for temperature-resistant flexible adhesives is growing. For example, the research and exploration of the Earth's poles (Antarctic, 20.7 to -94.2°C) and human outer space (Moon, 127 to -183°C; Mars, 20 to -140°C; Saturn, -130 to -191°C; Neptune, -210 to -218°C) require high-strength, low-temperature-resistant flexible adhesives. So far, most traditional adhesives are based on polymers as the main component, such as commercially available hot melt adhesives: ethylene-vinyl acetate copolymer (EVA), polyamide (PA) and polyether sulfone (PES). Although they have been widely used in daily life, they still have the following shortcomings, especially in low temperature environments: (1) high crosslinking density and low surface energy make it difficult for the adhesive to bond to the substrate surface and easy to debond; (2) poor interfacial penetration, which easily generates large residual stress; (3) traditional polymer molecules are easy to freeze at low temperatures, resulting in volume shrinkage and increased brittleness; (4) stability at low temperatures is generally insufficient. Although strategies such as adding plasticizers / crosslinkers or non-polar substituents can improve the temperature resistance range of adhesives to a certain extent, the minimum temperature resistance range of most commercial hot melt adhesives prepared by these methods is above -50°C. Therefore, the current improvement effect is far from satisfactory, and the complex preparation process also seriously limits their promotion and application. Therefore, new strategies are urgently needed to develop new low-temperature resistant flexible adhesives for specific scenarios such as the Arctic / Antarctic or outer space exploration. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a solvent-free adhesive which is simple to prepare, has low raw material cost, is easy to transport and store, is recyclable, easy to operate, repeatable, and resistant to low temperatures, as well as a preparation method thereof and its application in low temperature resistance.
[0004] The technical solution adopted by the present invention is: a low-temperature resistant flexible adhesive prepared from polymetallic oxygen clusters and thioctic acid, a flexible adhesive that can be used at low temperatures is developed through in-situ polymerization, the adhesive has high adhesion performance, organic solvent stability, long-term ultra-low temperature resistance and flexibility, and is counted by weight percentage: composed of 25%-75% of polymetallic oxygen clusters and the remainder of thioctic acid.
[0005] As a further improvement of the present invention, the polymetallic oxygen cluster is silicotungstic acid (SiW 12), phosphotungstic acid (PW 12 ,P2W 18 ), borotungstic acid (BW 11 ) and phosphomolybdic acid (PMo 12 ) or any one or more mixtures thereof.
[0006] As a further improvement of the present invention, the lipoic acid is heated at a certain temperature to undergo in-situ polymerization to form polylipoic acid.
[0007] As a further improvement of the present invention, the lipoic acid is heated at a temperature of 80-130° C. and a heating time of 1-5 hours.
[0008] A method for preparing a low-temperature resistant flexible adhesive prepared from polyoxometalates and thioctic acid comprises the following steps:
[0009] Step 1: Put the weighed polyoxometalate and lipoic acid into a blender according to the proportion and mix them to form a uniform mixture;
[0010] Step 2: Then, the uniformly mixed mixture is placed in an oven for heating;
[0011] Step 3: After the reaction in the oven is completed, the mixture is taken out and restored to room temperature to obtain a binder.
[0012] As a further improvement of the present invention, the rotation speed of the stirrer is 50-150 rpm.
[0013] The invention discloses an application of a low-temperature-resistant flexible adhesive prepared from polyoxometalates and thioctic acid, wherein the adhesive can remain stable in a variety of organic solvents without swelling.
[0014] As a further improvement of the present invention, the adhesive is suitable for a temperature range of -196 to 50°C and can achieve long-term adhesion.
[0015] As a further improvement of the present invention, the adhesive can withstand multiple folding and bending in an ultra-low temperature liquid nitrogen environment without losing adhesive properties.
[0016] Beneficial effects of the present invention: The present invention adopts a simple heat-assisted process to develop a polyoxometalate-based solvent-free low-temperature-resistant flexible adhesive that can be prepared in batches; the prepared solvent-free adhesive exhibits good interfacial adhesion ability on different substrates, has high adhesion strength (up to 3.5MPa) and organic solvent stability, tolerates a wide temperature range (-196 to 50°C), and has a long-lasting adhesion effect (>80 days) at -196°C; in terms of low-temperature resistance and flexibility, the solvent-free adhesive significantly exceeds the commercial hot-melt adhesive EVA; in addition, the strong interaction energy between polyoxometalate and polylipoic acid is the main factor that exhibits high adhesion performance at low temperatures, has enhanced cohesive strength, and inhibits polymer crystallization and volume shrinkage; this work enriches the types of low-temperature-resistant flexible adhesives, and will provide a reliable idea for the development of advanced solvent-free adhesives used in the preparation of Antarctic or planetary exploration. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a CSSP adhesive obtained from a low-temperature-resistant flexible adhesive prepared from polyoxometalates and thioctic acid and a batch preparation diagram of the present invention;
[0018] Figure 2 The FTIR spectrum (a) and PXRD spectrum (b) of the CSSP adhesive prepared from a low-temperature resistant flexible adhesive made of polyoxometalates and thioctic acid according to the present invention are shown in FIG. 1 H NMR spectrum (c), Raman spectrum (d), MALDI-TOF-MS spectrum (e), 32 Si NMR spectrum (f);
[0019] Figure 3 Schematic diagram of the formation of the CPSP binder obtained by preparing a low-temperature resistant flexible binder from polyoxometalates and thioctic acid according to the present invention (a), PW 12 SEM image of (b), SEM image of CPSP adhesive (c) and corresponding element distribution map (d);
[0020] Figure 4 The FTIR spectrum and PXRD spectrum of the CPSP adhesive prepared from polyoxometalate clusters and lipoic acid according to the present invention;
[0021] Figure 5 The CPSP adhesive obtained by the present invention is a low-temperature resistant flexible adhesive prepared from polyoxometalates and thioctic acid, and the hanging weight and solvent immersion diagram (a), shear tensile strength diagram (b); cyclic shear tensile strength diagram (c); spider web diagram woven by the adhesive (d);
[0022] Figure 6The present invention is a reversible curve diagram of the storage modulus (G') and loss modulus (G") of the CPSP adhesive obtained by preparing a low-temperature resistant flexible adhesive from polyoxometalate and thioctic acid over time (a), a macroscopic bonding experiment diagram in liquid nitrogen (b), a freezing and folding diagram of the CPSP adhesive and commercial EVA at ultra-low temperatures (c), a rheological diagram between -60 and 90°C (d), a variable temperature shear stretching (e) and a variable temperature FT-IR spectrum diagram (f). DETAILED DESCRIPTION
[0023] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0024] The invention provides a low-temperature-resistant flexible adhesive prepared from polymetallic oxygen clusters and thioctic acid. The flexible adhesive that can be used at low temperatures is developed through in-situ polymerization. The adhesive has high adhesion performance, organic solvent stability, long-term ultra-low temperature resistance and flexibility. The adhesive is composed of 25%-75% of polymetallic oxygen clusters and the balance of thioctic acid by weight percentage.
[0025] The polymetallic oxygen cluster is silicotungstic acid (SiW 12 ), phosphotungstic acid (PW 12 ,P2W 18 ), borotungstic acid (BW 11 ) and phosphomolybdic acid (PMo 12 ) or any one or more mixtures thereof.
[0026] The lipoic acid is heated at a certain temperature to undergo in-situ polymerization to form polylipoic acid. The lipoic acid heating temperature is 80-130° C. and the heating time is 1-5 hours.
[0027] A method for preparing a low-temperature-resistant flexible adhesive prepared from polyoxometalates and thioctic acid comprises the following steps: weighing polyoxometalates and thioctic acid in a blender according to a proportion and mixing them to form a uniform mixture; then placing the uniformly mixed mixture in an oven for heating; after the reaction in the oven is completed, taking out the mixture and restoring it to room temperature to obtain an adhesive. The speed of the blender is 50-150 rpm.
[0028] The invention discloses an application of a low-temperature-resistant flexible adhesive prepared from polyoxometalates and lipoic acid, wherein the adhesive can remain stable in a variety of organic solvents without swelling. The adhesive is suitable for a temperature range of -196 to 50°C and can achieve long-term adhesion. The adhesive can withstand multiple folding and bending in an ultra-low temperature liquid nitrogen environment without losing adhesive properties.
[0029] Embodiment 1:
[0030] 2g silicotungstic acid (SiW 12 ) and 1g lipoic acid powder are placed in a stirrer and stirred for 5 minutes. The mixture is then collected into a sample bottle and then placed in an oven at 90°C for 2 hours and placed at room temperature for 1 hour to obtain a polymetallic oxygen cluster-based binder (CSSP) which is easy to mass produce ( Figure 1 ).
[0031] The structure of the binder before and after formation was characterized by infrared spectroscopy (FT-IR), X-Ray powder crystal diffraction (PXRD), nuclear magnetic resonance (NMR), Raman spectroscopy and mass spectrometry. These results show that the lipoic acid monomer (TA) undergoes ring-opening polymerization to form a high molecular polymer (PTA), and PTA reacts with SiW 12 There is a strong hydrogen bond between them, and after forming the binder CSSP, SiW 12 The structure remains intact ( Figure 2 ).
[0032] Embodiment 2:
[0033] 2g of phosphotungstic acid (PW 12 or P2W 18 ) and 1g lipoic acid powder were placed in a stirrer and stirred for 5 minutes. The mixture was collected in a sample bottle and then placed in an oven at 90°C for 2 hours and placed at room temperature for 1 hour to obtain a polymetallic oxygen cluster-based binder (CPSP) with a smooth and dense surface ( Figure 3 ).
[0034] The structure of the obtained CPSP binder was analyzed by infrared spectroscopy (FT-IR) and X-Ray powder crystal diffraction (PXRD). The results showed that the PTA formed by the polymerization of lipoic acid monomers and SiW 12 There are obvious hydrogen bonds between them, and after forming the binder CPSP, SiW 12 Can be evenly dispersed in the binder matrix and the structure remains intact ( Figure 4 ).
[0035] Embodiment 3:
[0036] 2g phosphomolybdic acid (PMo 12 ) and 1g of lipoic acid powder are placed in a blender and stirred for 5 minutes. The mixture is collected into a sample bottle and then heated at 90°C in an oven for 2 hours and placed at room temperature for 1 hour to obtain a new polymetallic oxygen cluster-based binder.
[0037] Embodiment 4:
[0038] 2g silicotungstic acid (SiW 12) and 2g of lipoic acid powder are placed in a blender and stirred for 5 minutes. The mixture is collected in a sample bottle and then heated at 100°C in an oven for 2 hours and placed at room temperature for 2 hours to obtain a new polymetallic oxygen cluster-based binder.
[0039] The SSFP adhesive prepared in Example 1 above was used to test the bonding performance and solvent resistance:
[0040] The CSSP adhesive, which can be prepared in batches, can bond different types of artificial or natural materials and show good adhesion ( Figure 5 b), such as stainless steel (SS, 3.5MPa), aluminum (3.2MPa) and glass (Glass, 2.8MPa). On the SS substrate, it can easily withstand a weight of about 60kg ( Figure 5 a), after multiple cycles of bonding, it still remains at around 3.5MPa ( Figure 5 c). Insoluble in some organic solvents, such as trimethylbenzene (TMB), petroleum ether (PE) and n-hexane (N-hexane). No separation or displacement was observed after immersion for 14 days, and the bonding strength remained relatively stable ( Figure 5 a). CSSP adhesive can be processed into high-strength spider webs. The above results show that SSFP adhesive has strong solvent resistance, strong adhesion and flexibility ( Figure 4 ).
[0041] The CSSP adhesive prepared in the above-mentioned Example 1 is applied to low temperature resistance and low temperature flexibility:
[0042] The viscosity, storage modulus and loss modulus of the CSSP adhesive were tested by rheological tests. Below 50°C, the storage modulus of the CSSP adhesive is greater than the loss modulus (G′>G″), and the adhesive is in a gel or solid-like state. In addition, the loss modulus of the CSSP adhesive ( Figure 4 a) The storage modulus (G″>G′) is exceeded at 50 °C, forming a viscoelastic state dominated by viscosity, which will promote the interfacial bonding of the adhesive. In addition, the storage modulus (G′) and loss modulus (G″) can be reversibly cycled in the test under cyclic temperature, which is due to the solvent-free nature and reversible hydrogen bonding, which makes it exhibit reversible behavior.
[0043] CSSP adhesive can withstand a weight of 2kg under liquid nitrogen conditions ( Figure 6 b). In addition, no obvious shrinkage or cracking was observed after the CSSP adhesive was frozen in liquid nitrogen. More satisfactory, the CSSP adhesive was immersed in liquid nitrogen and then folded, and at least 8 freeze-fold-freeze cycles were achieved, indicating that the CSSP adhesive has good low-temperature flexibility ( Figure 6c). In addition, low temperature rheology shows that the CSSP adhesive has stable storage modulus (G′) and loss modulus (G″) in the temperature range of -60 to 0°C, which is consistent with its actual performance. When the temperature drops to -196°C, the bonding strength can still be stabilized to 2.30MPa. In addition, the variable temperature FT-IR spectrum ( Figure 6 f) shows that SiW 12 The characteristic peaks of CSSP and PTA are almost unchanged, indicating that the structure of CSSP adhesive remains intact over a wide temperature range. This work enriches the types of low-temperature resistant adhesives and will provide a reliable idea for the development of advanced solvent-free adhesives for polar or planetary exploration.
[0044] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low-temperature-resistant flexible adhesive prepared from polyoxometalate clusters and lipoic acid, characterized in that: A flexible adhesive that can be used at low temperatures is developed through in-situ polymerization. The adhesive has high adhesion performance, organic solvent stability, long-term ultra-low temperature resistance and flexibility. The adhesive is composed of 25%-75% of polymetallic oxygen clusters and the balance of lipoic acid by weight percentage.
2. The low-temperature resistant flexible adhesive prepared from polyoxometalate and lipoic acid according to claim 1, characterized in that: The polymetallic oxygen cluster is silicotungstic acid (SiW 12 ), phosphotungstic acid (PW 12 ,P2W 18 ), borotungstic acid (BW 11 ) and phosphomolybdic acid (PMo 12 ) or any one or more mixtures thereof.
3. The low-temperature-resistant flexible adhesive prepared from polyoxometalate and lipoic acid according to claim 1, characterized in that: The lipoic acid is heated at a certain temperature to undergo in-situ polymerization to form polylipoic acid.
4. The low-temperature resistant flexible adhesive prepared from polyoxometalate and lipoic acid according to claim 3, characterized in that: The lipoic acid is heated at a temperature of 80-130° C. and for a heating time of 1-5 hours.
5. A method for preparing a low-temperature resistant flexible adhesive prepared from polyoxometalates and thioctic acid, characterized in that: The following steps are involved: Step 1: Put the weighed polyoxometalate and lipoic acid into a blender according to the proportion and mix them to form a uniform mixture; Step 2: Then, the uniformly mixed mixture is placed in an oven for heating; Step 3: After the reaction in the oven is completed, the mixture is taken out and restored to room temperature to obtain a binder.
6. The method for preparing a low-temperature resistant flexible adhesive prepared from polyoxometalates and lipoic acid according to claim 5, characterized in that: The rotation speed of the stirrer is 50-150 rpm.
7. An application of a low-temperature-resistant flexible adhesive prepared from polyoxometalates and lipoic acid, characterized in that: The binder can remain stable in a variety of organic solvents without swelling.
8. The use of a low-temperature resistant flexible adhesive prepared from polyoxometalates and lipoic acid according to claim 7, characterized in that: The adhesive is suitable for a temperature range of -196 to 50°C and can achieve long-term adhesion.
9. The use of a low-temperature resistant flexible adhesive prepared from polyoxometalates and lipoic acid according to claim 7, characterized in that: The adhesive can withstand multiple folding and bending in an ultra-low temperature liquid nitrogen environment without losing adhesive properties.