Luminescence regulation and control method and application of mechanochromic EuWO4 fluorescent powder

EuWO4 phosphor is prepared by high-temperature solid phase method and color change is achieved under pressure, which solves the problem of insufficient thermal stability and use cycle times inorganic force-causing materials, and realizes efficient optical regulation and high-precision pressure sensing. Its application in many fields.

CN119081675APending Publication Date: 2024-12-06KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193621.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the field of inorganic force-discolored materials, the existing technology lacks effective research and application, especially in terms of thermal stability and the number of use cycles, which limits its potential applications in the fields of encryption, signal sensing, etc.

Method used

The EuWO4 phosphor was prepared by sintering the high-temperature solid phase method in a reducing atmosphere, and the color changed from orange to black by pressure of 1-50Mpa. The emission spectrum before and after the color change was measured by ultraviolet spectrometer and fluorescence spectrometer, achieving 100 % luminescence regulation.

Benefits of technology

It realizes the high thermal stability and reversibility of the inorganic force-changing material EuWO4, and has excellent optical regulation performance and high-precision pressure sensing capabilities. It is suitable for mechanical sensors and safe and anti-counterfeiting papers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081675A_ABST
    Figure CN119081675A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of mechanochromic inorganic fluorescent powder, in particular to a luminescence regulation and control method and application of mechanochromic EuWO4 fluorescent powder, EuWO4 fluorescent powder is colored after acting for 10-50 minutes under the pressure of 1-50 Mpa, and the fluorescent powder turns black from orange; and diffuse reflection and emission spectrums before and after color change are measured by using an ultraviolet spectrophotometer and a fluorescence spectrophotometer. The color of the EuWO4 fluorescent powder is changed after the EuWO4 fluorescent powder is subjected to pressure action, at the moment, the luminous intensity of the EuWO4 fluorescent powder can be found to be reduced compared with that before color change through 395nm ultraviolet excitation, which indicates that the regulation and control of the luminescence of the EuWO4 fluorescent powder are realized through photochromism. The EuWO4 fluorescent powder is obtained by sintering in a reducing atmosphere by adopting a high-temperature solid-phase method, and color transformation is realized under the action of pressure; compared with an organic mechanochromic material, the material has high chemical stability and thermal stability, the stability and durability of the fluorescent powder in practical application can be improved, and meanwhile, the application of the material in various fields is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mechanochromic inorganic phosphors, and in particular to a luminescence control method and application of mechanochromic EuWO4 phosphors. Background Art

[0002] Mechanochromic materials are stimuli-responsive materials, which can change color significantly under the action of external mechanical forces (grinding, stretching and impact, etc.). Mechanochromic materials can be simply divided into inorganic mechanochromic materials and organic mechanochromic materials. Mechanochromic materials have the characteristic of adjustable color of pressure-responsive samples, which is of great significance in many fields such as mechanical sensors, security paper and storage devices.

[0003] However, there is still a lack of research on mechanochromism in the field of inorganic materials. Current research is mainly focused on organic matter, and the mechanochromic system based on spiropyran has attracted widespread attention in the research field of mechanochromic materials. In addition, there are also many studies in polymers. Mechanochromic polymers can be manufactured by physically doping or covalently bonding force groups to a selected polymer matrix to achieve mechanical response heterochromic behavior. The above-mentioned organic mechanochromic materials achieve mechanochromism mostly by forming isomers under pressure. Among them, inorganic materials have the advantages of better thermal stability and longer service cycles compared to organic materials, and have attracted much attention.

[0004] Therefore, it is crucial to study inorganic mechanochromic materials, which can expand their potential application prospects in encryption, signal sensing and other fields. Summary of the invention

[0005] The purpose of the present invention is to provide a luminescence control method and application of mechanochromic EuWO4 phosphor. In view of the problems existing in the prior art, the present invention adopts a high-temperature solid-phase method to sinter in a reducing atmosphere to obtain EuWO4 phosphor, and realizes color change under the action of pressure.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] A method for regulating the luminescence of a mechanochromic EuWO4 phosphor comprises the following steps: preparing an inorganic EuWO4 phosphor by a high-temperature solid phase method, subjecting the EuWO4 phosphor to a pressure of 1-50 MPa for 10-50 minutes for coloring, and changing the phosphor from orange to black; and measuring the diffuse reflection and emission spectra before and after the color change by using an ultraviolet spectrometer (U4100) and a fluorescence spectrometer (F7000). After the EuWO4 phosphor is subjected to pressure, the color changes. At this time, through 395 nm ultraviolet excitation, it can be found that the luminescence intensity of the EuWO4 phosphor is lower than that before the color change, and the luminescence is completely quenched. This indicates that the present invention prepares a new inorganic mechanochromic material and the mechanochromism achieves 100% regulation of the luminescence of the EuWO4 phosphor.

[0008] Furthermore, the preparation method of the EuWO4 phosphor comprises the following steps:

[0009] S1: According to the chemical formula EuWO4, weigh WO3 and Eu2O3 in molar ratio, add anhydrous ethanol, mix and grind evenly until dry to obtain a mixed material;

[0010] S2: The uniformly ground mixture of S1 was sintered at 1150° C. for 4 hours in a reducing atmosphere, and then cooled to room temperature to obtain EuWO4 phosphor.

[0011] Furthermore, the reducing atmosphere is nitrogen-hydrogen reducing gas, with hydrogen accounting for 5%-10% and nitrogen accounting for 90%-95%.

[0012] On the other hand, the present invention proposes the application of the above method in realizing rare earth ion luminescence regulation of inorganic mechanochromic materials.

[0013] Beneficial effects of the present invention:

[0014] Advantages of high-temperature solid-phase method: The present invention obtains EuWO4 phosphor by sintering in a reducing atmosphere through high-temperature solid-phase method. The high-temperature solid-phase method can be carried out at a higher temperature, which is conducive to the full reaction of the raw materials and the rearrangement of the lattice, thereby obtaining a ceramic powder with good crystallinity and uniformity. In addition, the high-temperature solid-phase method also has the characteristics of good controllability and simple preparation process, making the preparation of photochromic ceramic powder more reliable and controllable.

[0015] Color change mechanism: The prepared EuWO4 phosphor changes its color from orange to black under the action of an external pressure of 1-50Mpa. In this process, Eu ions have two valence states. Due to their instability, they are prone to valence state changes under pressure. In order to maintain charge balance, W undergoes valence state changes, resulting in color change. Compared with the current organic mechanochromic materials, which are mainly organic bond breaking, it is difficult to restore the original color after color change. The valence state change has excellent thermal stability and repeated reversibility.

[0016] Structural stability: Compared with traditional organic mechanochromic materials, EuWO4, as an inorganic material, exhibits higher thermal stability and long service life. This is mainly due to the inherent properties of inorganic materials, such as high melting point and chemical inertness, which can maintain the stability of their chemical and physical properties under high temperature or harsh environment. EuWO4 phosphor is prepared by high-temperature sintering at 1150°C for 4 hours in a reducing atmosphere, which gives it excellent crystal structure and thermal stability. In this way, it can withstand high temperature and mechanical shock in applications, ensuring its reliability and long-term effectiveness in fields such as mechanical sensors, security anti-counterfeiting paper, and persistent optical storage. In addition, there is currently no research and development of inorganic mechanochromic materials, which is a new breakthrough.

[0017] Excellent optical regulation performance: the color of the sample changes after pressure is applied. The luminescence spectrum before and after the color change is tested. The luminescence is completely quenched after the color change. The luminescence regulation rate of the color change can reach 100%. (The regulation rate calculation formula is △R r =(R i -R0) / R0*100%,R i R0 represents the luminous intensity before and after the color change. It is difficult to achieve a 100% control rate for the current color-changing luminescence control, because the material turns black after pressure, and its absorption of light is enhanced, and the luminescence is quenched. For color-changing materials, the higher the control, the more obvious the contrast is when the data is displayed separately, and the higher the contrast.

[0018] The experimental results show that as the applied pressure increases, the diffuse reflection intensity of EuWO4 phosphor gradually decreases. The diffuse reflection spectra measured by UV spectrometer and fluorescence spectrometer show that the increase in pressure causes the light scattering characteristics to change, which provides a technical basis for its application in the field of pressure sensing. Specifically, the lattice distortion caused by pressure affects the propagation path and scattering intensity of light inside the material. By measuring the change in diffuse reflection intensity, the applied pressure can be accurately identified, making this material an ideal choice for high-precision pressure sensors, especially in environments that require rapid response and high accuracy.

[0019] Under 395nm excitation, the emission spectrum of EuWO4 phosphor changes significantly before and after pressure, and the luminescence intensity decreases significantly or even completely quenches after color change. This phenomenon shows that color change has an effect on the rare earth ion Eu 3+ The effect of regulating the luminescence performance is very significant. Specifically, the lattice structure changes caused by pressure make Eu 3+ The energy level of the light changes, which in turn affects its luminous intensity. In this way, not only can complex optical signal regulation be achieved, but this characteristic can also be used to develop a pressure sensor based on changes in luminous intensity. This sensor can reflect external pressure changes by detecting changes in optical signals, providing a new solution for high-sensitivity and high-precision pressure sensing applications.

[0020] In summary, the present invention not only achieves precise regulation of rare earth ion luminescence through the inorganic mechanochromic material EuWO4, but also achieves 100% luminescence regulation. In addition, compared with organic mechanochromic materials, this material has high chemical stability and thermal stability, which can improve the stability and durability of phosphors in practical applications, and expand the application of this material in various fields. The most important preparation method proposed in this technical solution is relatively simple. The preparation method has good adaptability to the large-scale production of this kind of phosphor, which helps to promote the practical application of this technology.

[0021] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0023] Figure 1 is a photo of the EuWO4 phosphor obtained by the present invention;

[0024] Figure 2 It is the X-ray diffraction pattern of EuWO4 obtained by the present invention;

[0025] Figure 3 This is a photograph of the color change of EuWO4 obtained by the present invention under pressure;

[0026] Figure 4 It is the diffuse reflection spectrum corresponding to the color change of EuWO4 obtained by the present invention under pressure;

[0027] Figure 5This is the emission spectrum corresponding to the two groups of EuWO4 phosphors obtained by the present invention before and after the color change, and the excitation wavelength is 395nm. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] The luminescence control method of a mechanochromic EuWO4 phosphor described in this embodiment comprises the following steps: subjecting the EuWO4 phosphor to a pressure of 1-50 MPa for 10-50 minutes for coloring, and the phosphor changes from orange to black; and using an ultraviolet spectrometer (U4100) and a fluorescence spectrometer (F7000) to measure diffuse reflection and emission spectra before and after the color change. After the EuWO4 phosphor is subjected to pressure, the color changes. At this time, through 395 nm ultraviolet excitation, it can be found that the luminescence intensity of the EuWO4 phosphor is lower than that before the color change, indicating that the luminescence of the EuWO4 phosphor is controlled by photochromism.

[0031] In this embodiment, the preparation method of the EuWO4 phosphor comprises the following steps:

[0032] S1: According to the chemical formula EuWO4, weigh WO3 and Eu2O3 in molar ratio, add anhydrous ethanol, mix and grind evenly until dry to obtain a mixed material;

[0033] S2: The uniformly ground mixture of S1 was sintered at 1150° C. for 4 hours in a reducing atmosphere, and then cooled to room temperature to obtain EuWO4 phosphor.

[0034] In this embodiment, the reducing atmosphere in S2 is nitrogen-hydrogen reducing gas, with hydrogen accounting for 5%-10% and nitrogen accounting for 90%-95%.

[0035] Example 2

[0036] like Figure 1 and 2 As shown, by the method provided by the present invention, the obtained EuWO4 is subjected to X-ray diffraction to obtain an X-ray diffraction pattern, from which it can be seen that the target crystal phase is synthesized.

[0037] Example 3

[0038] like Figure 3As shown, the color of the obtained orange-yellow phosphor changes significantly when it is subjected to a pressure of 30 MPa for 10 minutes, indicating that it has excellent mechanochromic properties.

[0039] Example 4

[0040] like Figure 4 The following is a graph of diffuse reflection spectra obtained under different pressures. As the pressure increases, the diffuse reflection intensity gradually decreases. Based on the relationship between diffuse reflection intensity and pressure, it is expected to be applied in pressure sensing.

[0041] Example 5

[0042] like Figure 5 The emission spectrum under 395nm excitation before and after pressure is shown. The luminescence intensity of EuWO4 phosphor decreases before and after color change, and the luminescence is completely quenched after color change, indicating that color change has excellent performance in regulating the luminescence of rare earth ions. Based on this, in addition to using diffuse reflected light to correspond to changes in pressure, the change in luminescence intensity with pressure can also be used in pressure sensing.

[0043] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A mechanochromic EuWO 4 Method for controlling the luminescence of phosphors, It is characterized in that The following steps are involved: EuWO 4 The phosphor was colored under a pressure of 1-50Mpa for 10-50 minutes, and the phosphor changed from orange to black. The diffuse reflection and emission spectra before and after the color change were measured by UV spectrometer and fluorescence spectrometer. The photochromic effect of EuWO on the color change was proved by 395nm UV excitation. 4 The luminescence of phosphors can be regulated.

2. The mechanochromic EuWO according to claim 1 4 Method for controlling the luminescence of phosphors, Features: The EuWO 4 The preparation method of the phosphor comprises the following steps: S1: According to the chemical formula EuWO 4 Weigh WO in molar ratio 3 、Eu 2 O 3 , adding anhydrous ethanol and mixing and grinding evenly until dry to obtain a mixed material; S2: The mixed material of S1 was ground evenly and sintered at 1150℃ for 4 hours in a reducing atmosphere, and then cooled to room temperature to obtain EuWO 4 Phosphor.

3. The mechanochromic EuWO as claimed in claim 2 4 Method for controlling the luminescence of phosphors, Features: The reducing atmosphere is nitrogen-hydrogen reducing gas, with hydrogen accounting for 5%-10% and nitrogen accounting for 90%-95%.

4. Application of the method according to any one of claims 1 to 3 in regulating the luminescence of rare earth ions in inorganic mechanochromic materials.