Preparation method of NAK80 steel ingot
Through the steps of electric furnace smelting, LF refining, VD vacuum refining and mold casting, combined with oxygen blowing, feeding Al line and Si-Ca line, controlling the packing temperature and argon protection, the slag wrapping and slag preparation in NAK80 steel ingot preparation and The inclusion problem significantly improves the pass rate of flaw detection.
Patent Information
- Application Number
- CN202411361435.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
AI Technical Summary
During the preparation process of NAK80 steel ingot, due to the high aluminum content and high viscosity of the steel, Al oxide is difficult to fully float and remove, resulting in the incorrect selection of overheat and protective slag and easy to cause slag wrapping and subcutaneous inclusion defects, and the pass rate of flaw detection is low.
Using the steps of electric furnace smelting, LF refining, VD vacuum refining and mold casting, through blowing oxygen to fuse, feeding Al and Si-Ca wires, controlling the packing temperature and oxygen content, combining slit-type argon protection device and asbestos The protective sleeve is protected and poured to ensure accurate control of the molten steel composition and pouring conditions.
It effectively avoids alumina inclusion aggregation and casting slag, and improves the flaw detection pass rate of NAK80 steel ingots from 80% to 95%.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy and pressure processing, and in particular to a method for preparing a NAK80 steel ingot. Background Art
[0002] NAK80 (10Ni3MnCuAl) is a low-carbon medium alloy precipitation hardening steel. After solution aging treatment, Ni3Al phase and ε-Cu phase are precipitated to achieve strengthening. After aging treatment, the hardness of NAK80 can reach 37~42HRC, and it still maintains good machinability. In addition, the steel has good hardenability, small segregation tendency and good mirror processing performance. It is mainly used for the production of plastic molds with high mirror surface and high appearance quality, and has a very broad market prospect.
[0003] However, NAK80 has a high aluminum content, which makes the steel liquid more viscous and makes it difficult for Al oxides to float up and be removed completely. Therefore, in the process of preparing NAK80 ingots, improper selection of superheat and protective slag can easily cause defects such as slag inclusion and subcutaneous inclusions, resulting in a low flaw detection pass rate.
[0004] Therefore, it is of great significance to provide a method for preparing NAK80 ingots to improve the qualified flaw detection rate and ultimately ensure the performance of NAK80 ingots. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for preparing NAK80 steel ingots. The preparation method provided by the present application can solve the problem of NAK80 steel ingots failing flaw detection and successfully cast qualified large steel ingots.
[0006] In view of this, the present application provides a method for preparing a NAK80 steel ingot, comprising the following steps:
[0007] S1) mixing ingredients according to the composition ratio of NAK80 steel ingot to obtain mixed raw materials;
[0008] S2) smelting the mixed raw materials in an electric furnace;
[0009] During the electric furnace smelting process, after the mixed raw materials form a molten pool, oxygen blowing is performed to assist melting. When the oxidation is completed, samples are taken to analyze the contents of C and P. If the carbon content is ≤0.05%, the carbon content is increased to more than 0.05% by inserting electrodes or spraying coke particles.
[0010] S3) subjecting the molten steel obtained in step S2) to LF refining;
[0011] During the LF refining process, Al wire is fed; during the LF reduction process, steel slag and carbon powder are added;
[0012] [S] in the bag ≤ 0.005%, the bag temperature is 1650~1700℃, the fixed oxygen ≤ 10ppm; remove 1 / 2~2 / 3 of the slag;
[0013] S4) subjecting the molten steel obtained in step S3) to VD vacuum refining;
[0014] During the VD vacuum refining process, Al ingots are added to the molten steel and then Si-Ca wires are added for Ca treatment; after breaking the vacuum, samples are taken for analysis of element Al, and Al is adjusted according to the limited Al wire in the internal control component;
[0015] S5) casting the molten steel obtained in step S4);
[0016] In the process of the mold casting, a slit type argon protection device and an asbestos protection sleeve are combined for protective pouring; the distance between the water inlet and the gate is within 20 mm; the mold casting protective slag adopts Xibaoda steel ingot protective slag, which is added in a hanging manner.
[0017] Preferably, in step S1), the mixed raw material has [C] 0.3-1.5%, P ≤ upper specification limit ~ 0.010%, and [Cr] 12-13.5%.
[0018] Preferably, in step S2), lime is placed on the bottom of the electric furnace before loading the furnace; when the temperature is ≥1540°C, if the P content exceeds the standard, lime is added or the slag is replaced; if the residual elements and the five harmful elements are abnormal, samples are taken for analysis and treatment when the temperature is ≥1560°C.
[0019] Preferably, in step S2), the mixed raw material is subjected to low-temperature dephosphorization in the late stage of melting and the early stage of oxidation;
[0020] The tapping conditions of the electric furnace smelting are: final carbon ≥ 0.03%, tapping temperature 1600-1700°C, tapping P ≤ 0.006%;
[0021] During the steel-tapping process of the electric furnace, reducing agent and slag are added along with the molten steel flow.
[0022] Preferably, in step S3), the inlet temperature of LF refining is ≥1540°C; and Nb iron is added during the LF refining process.
[0023] Preferably, in step S4), the slag thickness is 60-100 mm; the amount of Si-Ca wire added is 150-200 m / furnace, and the wire feeding speed is ≥4 m / s.
[0024] Preferably, in step S4), the ultimate vacuum degree is ≤67Pa, the holding time under the ultimate vacuum is ≥20min, and the soft argon blowing time is ≥25min; the bag temperature is 1500-1600°C; H is determined during the temperature measurement, requiring the [H] content to be ≤1.5ppm, and the bag temperature is 1550-1560°C.
[0025] Preferably, in step S5), an insulating board and a heating agent are used during the pouring process; the heating agent is a high-aluminum heating agent.
[0026] Preferably, in step S5), the pouring temperature is 1550-1556°C.
[0027] Preferably, in step S5), the ingot shape of the NAK80 steel ingot is Φ660 / 10.0t, the ingot body time is 780~960s, and the riser time is 300~420s; the ingot shape of the NAK80 steel ingot is Φ730 / 13.0t, the ingot body time is 840~1020s, and the riser time is 360~480s.
[0028] The present application provides a method for preparing a NAK80 steel ingot, which includes batching, electric furnace smelting, LF refining, VD vacuum refining and die casting in sequence. In the above preparation process, the present application avoids the aggregation of alumina inclusions and slag wrapping during casting by accurately controlling the process conditions of the four steps of electric furnace smelting, LF refining, VD vacuum refining and die casting, and successfully casts a qualified large steel ingot, thereby improving the flaw detection pass rate of the NAK80 steel ingot from 80% to 95%. DETAILED DESCRIPTION
[0029] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0030] In view of the problem of low flaw detection pass rate of NAK80 steel ingots in the prior art, the present application provides a smelting method of NAK80 steel ingots, which includes batching, electric furnace smelting, LF refining, VD vacuum refining and die casting in sequence. By limiting the relevant process conditions in the above process steps, the accumulation of inclusions and slag wrapping during casting are avoided, and qualified ingots are successfully cast, so that the flaw detection pass rate of NAK80 steel ingots is improved. Specifically, the embodiment of the present invention discloses a preparation method of NAK80 steel ingots, which includes the following steps:
[0031] S1) preparing ingredients according to the composition ratio of NAK80 to obtain a mixed raw material;
[0032] S2) smelting the mixed raw materials in an electric furnace;
[0033] During the electric furnace smelting process, after the mixed raw materials form a molten pool, oxygen blowing is performed to assist melting. When the oxidation is completed, samples are taken to analyze the contents of C and P. If the carbon content is ≤0.05%, the carbon content is increased to more than 0.05% by inserting electrodes or spraying coke particles.
[0034] S3) subjecting the molten steel obtained in step S2) to LF refining;
[0035] During the LF refining process, Al wire is fed; during the LF reduction process, steel slag and carbon powder are added;
[0036] [S] in the bag ≤ 0.003%, the bag temperature is 1650~1700℃, the fixed oxygen ≤ 10ppm; remove 1 / 2~2 / 3 of the slag;
[0037] S4) subjecting the molten steel obtained in step S3) to VD vacuum refining;
[0038] During the VD vacuum refining process, Al ingots are added to the molten steel and then Si-Ca wires are added for Ca treatment; after breaking the vacuum, samples are taken for analysis of element Al, and Al is adjusted according to the limited Al wire in the internal control component;
[0039] S5) casting the molten steel obtained in step S4);
[0040] In the process of the mold casting, a slit type argon protection device and an asbestos protection sleeve are combined for protective pouring; the distance between the water inlet and the gate is within 20 mm; the mold casting protective slag adopts Xibaoda steel ingot protective slag, which is added in a hanging manner.
[0041] The preparation process of NAK80 steel ingot includes raw material preparation → electric furnace → LF refining → VD vacuum refining → mold casting in sequence.
[0042] In the step of raw material preparation, the present application prepares the raw materials according to the composition ratio of NAK80 steel ingot to obtain mixed raw materials; in the process of preparing the raw materials, the furnace charge metal materials used include: scrap steel, agreement billet, DP-1, H-Cr, H-Mn, Si-Fe; the ingredients of the raw materials are: [C] 0.3~1.5%, P≤specification upper limit~0.010%, [Cr] 12~13.5%.
[0043] In the process of electric furnace smelting, the technical method of electric furnace smelting is not particularly limited in this application, and it can be carried out in a manner familiar to those skilled in the art, but the detailed process is limited in this application; among them, 800 kg of lime is placed on the bottom of the furnace before charging, charging, and power melting; after power melting to form a molten pool, oxygen blowing and fluxing should be done immediately, and the melting situation in the furnace should be observed frequently to avoid large boiling or electrode breakage caused by large collapse of the material; low-temperature P removal should be done in the late stage of melting and the early stage of oxidation; when the temperature is ≥1540°C, sampling and full analysis, including various related residual elements and five harmful elements, if P is found to be abnormally high, it can be supplemented Add appropriate amount of lime or replace slag; if the residual elements and five harmful elements are abnormal, take samples for analysis and confirmation after the temperature is ≥1560℃ and make corresponding disposal; after the oxidation is completed, take samples for analysis of C and P. When the carbon content is ≤0.05%, increase the carbon content to above 0.05% by inserting electrodes or spraying coke particles; the conditions for tapping in electric furnace smelting: the final carbon is ≥0.03%; the tapping temperature is 1650~1690℃; the tapping P is ≤0.006%, and the reducing agent and slag are added with the steel flow during the tapping process: add 80~120kg of Al blocks / furnace, 600~800kg of lime / furnace, and 100~200kg of dolomite / furnace. After electric furnace smelting, the amount of tapping = [planned ingot amount + soup channel amount + middle injection tube amount + injection surplus] - the amount of alloy added.
[0044] After the electric furnace smelting, LF refining is carried out. The operation mode of LF refining is carried out in a manner well known to those skilled in the art, and this application has no special restrictions on this. However, this application defines the detailed process of LF refining; wherein, the seat bag is checked to see if Ar is normal, and Al wire is fed at 80-100 m / furnace; temperature measurement is required, and the inlet temperature is required to be ≥1540°C; during the LF reduction process, 50 kg of steel slag is added in batches, and the total amount added is 200 kg / furnace, and 20-60 kg / furnace of C powder can be added in batches for reduction; if it is still If the original is not good, you can add steel slag or Al for deoxidation, but you need to add the corresponding weight of lime: the amount of lime added is 3 times the weight of steel slag or 5 times the amount of Al added; slag white, temperature measurement, sampling and full analysis (including Al), according to the sampling and analysis results, add alloys as required to adjust the chemical composition; add alloys to ensure that the addition of other elements except Al meets the internal control requirements, and add Nb iron at 10kg / furnace; in the above-mentioned alloys, the alloys can be selected according to the composition requirements High carbon ferromanganese, silicon manganese, nickel plate, copper plate, ferromolybdenum, ferroniobium, sponge high. In this process, the bag hanging conditions: bag hanging [S] ≤ 0.003%; bag hanging temperature: 1650~1660℃; the oxygen determination result ≤ 10ppm can be hung into VD; remove about 1 / 2~2 / 3 of the slag, and the bag is put into VD vacuum treatment.
[0045] The present application then performs VD vacuum refining on the molten steel obtained by LF. In the step of VD vacuum refining, the specific operation process is carried out in a manner well known to those skilled in the art, and the present application has no special restrictions on this. However, the present application defines the specific process stages of VD vacuum refining, specifically: measuring the temperature and slag thickness before entering the tank, requiring the slag thickness to be 60-100 mm; adding Al ingots according to the upper limit of the specification to adjust Al, ensuring that all Al ingots enter the molten steel, avoiding the operation of supplementary feeding of Al wire after VD, and feeding Si-Ca wire at 150-200 meters / furnace for Ca treatment after the Al ingots are added, and the wire feeding speed of the wire feeder is ≥4m / s, ensuring that all Si-Ca wires enter the molten steel instead of being coiled on the slag surface; after evacuation, the ultimate vacuum degree is ≤67Pa, the holding time under the ultimate vacuum is ≥20min, the argon flow rate is adjusted to 100-150L / min, the soft argon blowing time is ≥25min, the argon flow rate is controlled during the soft argon blowing time, and the molten steel is prohibited from leaking naked into the air. After breaking the air, take samples for analysis of element Al, and adjust Al according to the limited Al feed line in the internal control composition; measure temperature, determine H, and require [H] content ≤1.5ppm; the bag temperature is 1550~1560℃.
[0046] After VD vacuum refining, the present application will mold the obtained molten steel, and use a combination of a slit-type argon protection device and an asbestos protection sleeve for protective pouring, wherein the pressure of the slit-type argon protection is 0.3~0.5MPa; when pouring steel, it must be ensured that pouring is done with a steel pouring car, and the distance between the water nozzle and the pouring gate is controlled within 20mm; the mold casting protective slag must use Xibaoda steel ingot protective slag, which is added in a hanging manner; pouring requires the use of insulation boards and heating agents, wherein the insulation boards are insulation materials installed at the riser position of the ingot mold, which can play a role in heat preservation and reduce the looseness of the ingot, and the insulation boards are insulation materials well known to technicians in this field; the heating agent is added to the riser of the ingot after the molten steel is poured, which can generate heat to prevent the molten steel at the upper end of the ingot from solidifying too quickly, and can also reduce looseness and shrinkage holes. Specifically, the heating agent is selected from high-aluminum heating agents. The pouring temperature is 1550-1556°C; the ingot shape of the NAK80 steel ingot is Φ660 / 10.0t, the ingot body time is 780-960s, and the riser time is 300-420s; the ingot shape of the NAK80 steel ingot is Φ730 / 13.0t, the ingot body time is 840-1020s, and the riser time is 360-480s. In a specific embodiment, the specification of the steel ingot is Φ730 / 13.0t, the ingot body time is 965-1000s, and the riser time is 412-470s.
[0047] The present application provides a method for preparing a NAK80 steel ingot, which includes batching, electric furnace smelting, LF refining, VD vacuum refining and die casting in sequence. By controlling the above processes, the comprehensive control avoids the aggregation of alumina inclusions and slag wrapping during casting, thereby achieving an improvement in the flaw detection pass rate.
[0048] In order to further understand the present invention, the preparation method of the NAK80 steel ingot provided by the present invention is described in detail below in conjunction with examples, and the protection scope of the present invention is not limited by the following examples.
[0049] Example
[0050] 1) Charge: ① Charge composition: metal materials are composed of scrap steel, agreement billet, DP-1, H-Cr, H-Mn, Si-Fe, etc.; ② Accurate composition, clean and dry; size ≤ 1000×700×500mm; ③ Charge: [C] 0.56%, P: 0.005%, [Cr]: 12.80%;
[0051] 2) Electric furnace smelting: After the furnace is discharged, sand is filled and material is loaded. After 45 minutes, the temperature is measured at 1680℃. Samples are taken. The 0:15 sample return C: 0.022%, P: 0.005%, meeting the conditions for steel tapping. Steel is tapped. During the steel tapping process, 80kg of Al ingots are added to the package.
[0052] 3) LF furnace refining: put into the tank, feed Al wire 100m, measure temperature 1555℃; add 100kg of refined slag, 200kg of steel slag, 500kg of lime, turn on the power, take sample 1 (the content is as shown in Table 1 for sample 1), add 300kg of lime according to the content, add alloy (400kg of high carbon ferromanganese, 300kg of silicon manganese, 1169kg of nickel plate, 298kg of copper plate, 130kg of ferromolybdenum); measure temperature 1651℃, take sample 2 (the content is as shown in Table 1 for sample 2); measure temperature 1687℃, take sample 3 (the content is as shown in Table 1 for sample 2); The composition of sample 3), alloy (30kg high carbon ferromanganese, 35kg ferroniobium, 5kg sponge zirconium) was added according to the content of the components; sample return, add 100kg refined slag, 200kg lime; temperature measurement at 1689℃, sample (sample 4), temperature measurement at 1725℃, open the hanging bag, smelting time 2 hours and 51 minutes, the analysis results of the above process sampling are shown in Table 1; (hanging bag conditions: 1) hanging bag [S] ≤ 0.005%; 2) hanging bag temperature: 1650~1700℃; actual control [S] ≤ 0.004%, temperature 1689℃)
[0053] Table 1 Composition data of samples taken during LF furnace refining
[0054]
[0055] 4) VD furnace vacuum refining: sample 1 (content as shown in Table 2 for sample 1) was put into the tank, the temperature was 1725℃, the slag thickness was 86mm, 200kg of aluminum iron was added, vacuum was started, the pressure reached 67pa, the argon flow rate was adjusted to 135L / min, the ultimate vacuum was 2pa, the ultimate holding time was 23min, the air was broken, the temperature was 1635℃, sample 2 (content as shown in Table 2 for sample 2) was taken, 10kg of rare earth was added, 280kg of aluminum ingot was added to the sample, the lid was closed and stirred, 200m of silicon-calcium wire was fed, the temperature was 1603℃, the [H] content was 0.5, sample 3 (content as shown in Table 2 for sample 3), argon was blown statically, the temperature was 1555℃, the steel was cast by hanging the ladle, and the analysis results of the process samples are shown in Table 2:
[0056] Table 2 Composition data of samples taken during VD furnace vacuum refining
[0057]
[0058] 5) Pouring
[0059] The molten steel after vacuum refining in the VD furnace was poured, and the pouring parameters are shown in Table 3;
[0060] Table 3 Parameter data table during casting process
[0061]
[0062] The quality of the obtained ingot was tested and the results are shown below;
[0063] (1) The steel ingot was forged into a 400mm×800mm large-section module, which passed the flaw detection test.
[0064] (2) The chemical composition of the finished product is shown in Table 4:
[0065] Table 4 Ingot composition data
[0066]
[0067] (3) Non-metallic inclusions are shown in Table 5:
[0068] Table 5 Data table of non-metallic inclusions in steel ingots
[0069]
[0070] (4) Grain size: 1# sample level 7, 2# sample level 7.
[0071] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0072] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a NAK80 steel ingot, The following steps are involved: S1) mixing ingredients according to the composition ratio of NAK80 steel ingot to obtain mixed raw materials; S2) smelting the mixed raw materials in an electric furnace; During the electric furnace smelting process, after the mixed raw materials form a molten pool, oxygen blowing is performed to assist melting. When the oxidation is completed, samples are taken to analyze the contents of C and P. If the carbon content is ≤0.05%, the carbon content is increased to more than 0.05% by inserting electrodes or spraying coke particles. S3) subjecting the molten steel obtained in step S2) to LF refining; During the LF refining process, Al wire is fed; during the LF reduction process, steel slag and carbon powder are added; [S] in the bag ≤ 0.005%, the bag temperature is 1650~1700℃, the fixed oxygen ≤ 10ppm; remove 1 / 2~2 / 3 of the slag; S4) subjecting the molten steel obtained in step S3) to VD vacuum refining; During the VD vacuum refining process, Al ingots are added to the molten steel and then Si-Ca wires are added for Ca treatment; after breaking the vacuum, samples are taken for analysis of element Al, and Al is adjusted according to the limited Al wire in the internal control component; S5) casting the molten steel obtained in step S4); In the process of the mold casting, a slit type argon protection device and an asbestos protection sleeve are combined for protective pouring; the distance between the water inlet and the gate is within 20 mm; the mold casting protective slag adopts Xibaoda steel ingot protective slag, which is added in a hanging manner.
2. The preparation method according to claim 1, It is characterized in that In step S1), the mixed raw materials contain [C] 0.3-1.5%, P ≤ upper limit of specification ~ 0.010%, and [Cr] 12-13.5%.
3. The preparation method according to claim 1, It is characterized in that In step S2), lime is placed on the bottom of the electric furnace before loading the furnace; when the temperature is ≥1540°C, if the P content exceeds the standard, lime is added or the slag is replaced; if the residual elements and the five harmful elements are abnormal, samples are taken for analysis and treatment when the temperature is ≥1560°C.
4. The preparation method according to claim 1, It is characterized in that In step S2), the mixed raw material is subjected to low-temperature dephosphorization in the late stage of melting and the early stage of oxidation; The tapping conditions of the electric furnace smelting are: final carbon ≥ 0.03%, tapping temperature 1600-1700°C, tapping P ≤ 0.006%; During the steel-tapping process of the electric furnace, reducing agent and slag are added along with the molten steel flow.
5. The preparation method according to claim 1, It is characterized in that In step S3), the inlet temperature of LF refining is ≥1540°C; Nb iron is added during the LF refining process.
6. The preparation method according to claim 1, It is characterized in that In step S4), the slag thickness is 60-100 mm; the amount of Si-Ca wire added is 150-200 m / furnace, and the wire feeding speed is ≥4 m / s.
7. The preparation method according to claim 1, It is characterized in that In step S4), the ultimate vacuum degree is ≤67Pa, the holding time under the ultimate vacuum is ≥20min, and the soft argon blowing time is ≥25min; the bag temperature is 1500-1600°C; H is determined during the temperature measurement, requiring the [H] content to be ≤1.5ppm, and the bag temperature is 1550-1560°C.
8. The preparation method according to claim 1, It is characterized in that In step S5), an insulating board and a heating agent are used during the pouring process; the heating agent is a high-aluminum heating agent.
9. The preparation method according to claim 1, It is characterized in that In step S5), the pouring temperature is 1550-1556°C.
10. The preparation method according to claim 1, It is characterized in that In step S5), the ingot shape of the NAK80 steel ingot is Φ660 / 10.0t, the ingot body time is 780~960s, and the riser time is 300~420s; the ingot shape of the NAK80 steel ingot is Φ730 / 13.0t, the ingot body time is 840~1020s, and the riser time is 360~480s.