Method for preparing antimony black through water vapor oxygen-controlled roasting of lead-antimony alloy
By using water vapor controlled oxygen calcining method to separate lead-antimony alloys in low oxygen environments, the problems of incomplete separation and high energy consumption in the existing process were solved, and high purity Sb2O3 was prepared, with excellent oxygen vacancy characteristics, suitable for Electronic materials and other fields.
Patent Information
- Application Number
- CN202411133638.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-06
AI Technical Summary
The existing lead-antimony alloy separation process has a long process, high energy consumption, high cost, and incomplete separation, making it difficult to obtain high-purity Sb2O3.
The lead-antimonial alloy is calcined in a low-oxygen environment by water vapor control. Water vapor is used to promote the reaction of Sb and water vapor to generate Sb2O3, and the separation of Sb and impurities is achieved by controlling the flow rate and temperature of water vapor, thereby obtaining high-purity Sb2O3.
It has achieved high purity and low cost Sb2O3 preparation. The produced Sb2O3 has unique oxygen vacancy characteristics and is suitable for electronic materials and optoelectronic devices, improving the market competitiveness and economic value of the products.
Smart Images

Figure CN119082496A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonferrous metal pyrometallurgy, and specifically relates to a method for preparing antimony black by water vapor oxygen-controlled roasting of a lead-antimony alloy. Background Art
[0002] Lead and antimony are common associated metals. Antimony is often associated with lead ores, while lead is often associated with antimony ores. A large amount of lead-antimony alloy intermediate products will be produced during the smelting process of lead and antimony. At present, the separation of lead-antimony alloys in industry generally adopts the process of two blowing and then reduction smelting in a reverberatory furnace. Since lead and antimony behave similarly in the metallurgical process and have similar physical and chemical properties, it is difficult to separate lead and antimony through pyrometallurgy. Generally, the antimony after separation contains 4% lead and the lead contains about 13% antimony. In the next step, the crude antimony is electrolytically refined by sulfuric acid-hydrofluoric acid-antimony fluoride system to remove lead, and the crude lead is electrolytically refined by lead fluoride silicate system to remove antimony. The above-mentioned lead-antimony separation process is not only long in process, energy-intensive, but also costly. At the same time, due to the high antimony content in lead, although metallurgical workers at home and abroad have successively developed a variety of technologies such as pyrometallurgical separation, Na2S leaching-electrodeposition, slurry electrolysis, sodium sulfide wet separation of lead and antimony and then pyrometallurgical refining of antimony, vacuum distillation, smelting separation, centrifugal segregation, etc., they all have the problems of long processes, high energy consumption, high consumption of raw materials, high processing costs, and incomplete separation.
[0003] Based on the above problems, the present invention aims to improve the traditional lead-antimony alloy separation technology, provide a green, clean, efficient, low-cost and simple process lead-antimony alloy separation technology, and prepare Sb2O3 with higher purity and better performance. This technology uses a small amount of dissolved oxygen carried in water vapor to maintain the reaction system in a low-oxygen environment on the one hand, and promote the reaction of Sb and water vapor on the other hand, so that the reaction proceeds spontaneously (ΔG < 0, see formula 1). In addition, since the saturated vapor pressure of lead (Pb) is much smaller than that of antimony (Sb), Sb first volatilizes into the gas phase and undergoes oxidation reaction with water vapor to generate Sb2O3, while Pb and other small amounts of impurities remain in the melt, thereby achieving effective separation of Sb and impurity elements, and the purity of Sb2O3 in the produced smoke is higher, and the impurity content is less than 0.2%. The Sb2O3 powder obtained after controlled oxidation roasting by water vapor is black, presents a cubic crystal structure and has the characteristics of oxygen vacancy defects.
[0004] ΔG = -145.305 kJ mol -1 (Formula 1)
[0005] Compared with traditional processes, antimony oxide prepared by this new process has higher purity and unique oxygen vacancy characteristics, which brings potential application prospects in the fields of electronic materials, optoelectronic devices, catalytic materials, etc., and provides new possibilities for expanding the application fields of Sb2O3 products. Summary of the invention
[0006] The purpose of the present invention is to provide a new preparation process that is simple, reasonable, energy-saving and environmentally friendly, and can effectively improve the purity and performance of Sb2O3 products in view of the current status of incomplete separation and high energy consumption of the lead-antimony separation process. The process adopts low-cost and industrially easily available water vapor to replace conventional oxygen for roasting and preparing Sb2O3. The roasting atmosphere is controlled by controlling the flow rate of water vapor, and the lead-antimony alloy is roasted in a low oxygen potential atmosphere to obtain another form of Sb2O3 with high purity and better performance. Because the generated antimony black is a Sb2O3 nanocrystal with oxygen-rich vacancies, it has potential application prospects in the fields of electronic materials, optoelectronic devices, catalytic materials, etc., and improves the market competitiveness and economic value of Sb2O3 products in industrial production.
[0007] The invention comprises the following steps: weighing a certain mass of lead-antimony alloy, placing it in a quartz boat, and then putting it into a tube furnace, and heating after introducing nitrogen for a certain period of time to remove the air in the tube to melt the lead-antimony alloy, blowing water vapor into the lead-antimony melt, controlling the gas flow rate of the water vapor to be 0.5-3 g / min, and performing high-temperature controlled oxygen potential roasting at a temperature of 600-900°C to prepare Sb2O3, and keeping the temperature for 1-4 hours. During the roasting process, a large amount of volatile antimony is formed, which meets with water vapor and undergoes an oxidation reaction, producing a large amount of black Sb2O3 products with oxygen-rich vacancies, and then cooling and collecting dust through a bag to obtain antimony black powder. The Sb content in the lead-antimony alloy used is 50%-60%, and the Pb content is 30%-35%. During the roasting process, the flow rate of the water vapor is controlled to be 0.5-3 g / min. During the roasting process, the temperature is controlled at 600-900°C. During the roasting process, the roasting holding time is controlled to be 1-4 hours. Under nitrogen atmosphere, the water vapor flow rate is controlled at 0.5-3 g / min, and the product is calcined at 600-900 ℃ with controlled oxygen potential for 1-4 h. Antimony black with oxygen-rich vacancy shape is prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 This is a flow chart for producing antimony black according to the present invention.
[0009] Figure 2 The XRD comparison diagram of Example 1, Comparative Example 1 and Comparative Example 2 is shown in FIG.
[0010] Figure 3 This is the XRD pattern of antimony black prepared in Example 1.
[0011] Figure 4 The EPR tests of Example 1 and Comparative Examples 1 and 2 are used to verify the existence of oxygen vacancies. DETAILED DESCRIPTION
[0012] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0013] The process flow chart of the present invention is as follows Figure 1 The XRD pattern of antimony black prepared by the present invention is shown in Figure 2 As shown, from Figure 2 It can be seen that the antimony black prepared by the present invention is cubic crystal Sb2O3. The XRD comparison chart and EPR comparison chart of the antimony black prepared by the present invention and the antimony white prepared by passing oxygen and passing oxygen plus water vapor are shown in the figure. Figure 3 , Figure 4 As shown, from Figure 3 It can be seen that the diffraction peak of the antimony black prepared by the present invention is stronger, and the half-peak width of the strongest diffraction peak is smaller, which indicates that the antimony black prepared by the present invention has higher crystallinity and larger grain size. Figure 4 It can be seen that the antimony black prepared by the present invention has the characteristics of oxygen vacancy defects.
[0014] Embodiment 1:
[0015] After the lead-antimony alloy is crushed and sieved, 20 g is weighed and placed in a quartz boat and put into a tube furnace, and nitrogen is introduced for 30 minutes to remove the air in the tube and then heated to melt the lead-antimony alloy. The tube furnace is heated at a heating rate of 10 ℃ / min. When the tube furnace is heated to 400 ℃, the HSG20 steam generator is turned on, and steam is blown in at a rate of 1 g / min. The temperature is kept at 800 ℃ for 2 hours for high-temperature controlled oxygen potential roasting to prepare antimony black. After completing the above operations, the antimony black obtained is tested for composition, and the purity is 99.80%.
[0016] The XRD analysis diagram of antimony black prepared in this example is as follows Figure 2 As shown, from Figure 2 It can be seen that the antimony black prepared by the present invention is Sb2O3.
[0017] Embodiment 2:
[0018] After the lead-antimony alloy is crushed and sieved, 20 g is weighed and placed in a quartz boat and put into a tube furnace, and nitrogen is introduced for 30 minutes to remove the air in the tube and then heated to melt the lead-antimony alloy. The tube furnace is heated at a heating rate of 10 ℃ / min. When the tube furnace is heated to 400 ℃, the HSG20 steam generator is turned on, and steam is blown in at a rate of 1 g / min. The temperature is kept at 850 ℃ for 2 hours for high-temperature controlled oxygen potential roasting to prepare antimony black. After completing the above operations, the antimony black obtained is tested for composition, and the purity is 99.86%.
[0019] Embodiment 3:
[0020] After the lead-antimony alloy is crushed and sieved, 20 g is weighed and placed in a quartz boat and put into a tube furnace, and nitrogen is introduced for 30 minutes to remove the air in the tube and then heated to melt the lead-antimony alloy. The tube furnace is heated at a heating rate of 10 ℃ / min. When the tube furnace is heated to 400 ℃, the HSG20 steam generator is turned on, and steam is blown in at a rate of 0.78 g / min. The temperature is kept at 800 ℃ for 2 hours for high-temperature controlled oxygen potential roasting to prepare antimony black. After completing the above operations, the antimony black obtained is tested for composition, and the purity is 99.88%.
[0021] Comparative Example 1:
[0022] After the lead-antimony alloy is crushed and sieved, 20 g is weighed and placed in a quartz boat and put into a tube furnace. Oxygen is introduced to form an oxygen atmosphere in the tube and then heated to melt the lead-antimony alloy. The tube furnace is heated at a heating rate of 10 °C / min to 800 °C and kept at 800 °C for 2 h for high-temperature roasting to prepare antimony white. After completing the above operations, the antimony white obtained is tested for composition and the purity is 99.21%.
[0023] Comparative Example 2:
[0024] After the lead-antimony alloy is crushed and sieved, 20 g is weighed and placed in a quartz boat and put into a tube furnace. Oxygen is introduced to form an oxygen atmosphere in the tube and then heated to melt the lead-antimony alloy. The tube furnace is heated at a heating rate of 10 °C / min. When the tube furnace is heated to 400 °C, the HSG20 steam generator is turned on, steam is blown in at a rate of 1 g / min, and the temperature is kept at 800 °C for 2 h for high calcination to prepare antimony white. After completing the above operations, the antimony white obtained is tested for composition, and the purity is 99.20%.
[0025] The XRD comparison of Sb2O3 prepared in Comparative Example 1, Comparative Example 2 and Example 1 is shown in Figure 3 As shown, from Figure 3 It can be seen that the antimony black prepared by the present invention has a stronger diffraction peak and a smaller half-peak width of the strongest diffraction peak, which indicates that the antimony black prepared by the present invention has a higher crystallinity and a larger grain size.
[0026] The EPR comparison of Sb2O3 prepared in Comparative Example 1, Comparative Example 2 and Example 1 is shown in the figure Figure 4 As shown, from Figure 4 It can be seen that the antimony black prepared by the present invention has oxygen vacancies.
Claims
1. A method for preparing antimony black by steam-controlled oxygen roasting of lead-antimony alloy, characterized in that: The method comprises the following steps: weighing a certain mass of lead-antimony alloy, placing it in a quartz boat, and then putting it into a tube furnace, introducing nitrogen for a certain period of time to expel the air in the tube, and then heating to melt the lead-antimony alloy, blowing water vapor into the lead-antimony melt, controlling the gas flow rate of the water vapor to be 0.5-3 g / min, and performing high-temperature controlled oxygen potential roasting at a temperature of 600-900°C to prepare Sb2O3, and keeping the temperature for 1-4 hours; a large amount of volatile antimony is formed during the roasting process, which meets the water vapor and undergoes an oxidation reaction, thereby generating a large amount of black Sb2O3 products with oxygen-rich vacancies, and then cooling and collecting the antimony black powder through a bag dust collector.
2. The method for preparing antimony black by steam oxygen-controlled roasting of lead-antimony alloy according to claim 1, wherein: The lead-antimony alloy used has an Sb content of 50%~60% and a Pb content of 30%~35%.
3. The method for preparing antimony black by steam oxygen-controlled roasting of lead-antimony alloy according to claim 1, wherein: The flow rate of water vapor during the roasting process is controlled to be 0.5~3 g / min.
4. The method for preparing antimony black by steam oxygen-controlled roasting of lead-antimony alloy according to claim 1, wherein: The temperature during the calcination process is controlled at 600~900 ℃.
5. The method for preparing antimony black by steam oxygen-controlled roasting of lead-antimony alloy according to claim 1, wherein: During the roasting process, the roasting holding time is controlled to be 1~4 h.
6. The method for preparing antimony black by steam oxygen-controlled roasting of lead-antimony alloy according to claim 1, wherein: Under a nitrogen atmosphere, the flow rate of water vapor is controlled at 0.5-3 g / min, and the product is calcined at 600-900 °C under controlled oxygen potential for 1-4 h. Antimony black with oxygen-rich vacancy shape is prepared.