Sodium germanate solution desiliconization reagent MC306 and preparation method and application thereof
The sodium germanate solution desilicate reagent MC306 prepared by pressurized reaction of sodium sulfate, gelatin, flocculant, and ethylenediaminetetraacetic acid under an oxygen atmosphere was solved by complexation reaction and flocculation. The sodium germanate solution in copper smelting smoke dust was solved by using complexation reaction and flocculation. The efficient removal of silicon in the medium achieves efficient desiliconization effect and reduces operational complexity and cost.
Patent Information
- Application Number
- CN202411086694.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-06
AI Technical Summary
There is an impurity silicon in the sodium germanate solution in the existing copper smelting smoke dust. If it is not processed and directly enters the germanium dioxide preparation process, it will affect the product quality. The existing desilencing method is inefficient, costly and complex in operation.
The sodium germanate solution desilicate reagent MC306 prepared by pressurized reaction under an oxygen atmosphere using sodium sulfate, gelatin, flocculant, and ethylenediaminetetraacetic acid (EDTA) as raw materials, and the desilicate reagent MC306 is formed through the modification of gelatin. The separation of silicon and germanium is achieved by combining the action of flocculant.
Under high acid and high temperature conditions, the silicon delamination effect in sodium germanate solution is significantly improved, and the desilencing rate reaches 92-99%, reducing operational complexity and cost.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and chemical industry, and specifically relates to a sodium germanate solution desiliconization reagent MC306 and a preparation method and application thereof. Background Art
[0002] A large amount of smoke containing valuable elements is produced during the smelting and blowing process of copper smelting. Due to the diversity of copper concentrate, the associated metals such as molybdenum, indium, germanium, bismuth, zinc, and lead enter the smoke during the smelting and blowing process. For the copper smelting smoke leaching solution of a copper enterprise, a separation study on the efficient extraction of germanium was carried out. Sodium germanate is the main source of germanium dioxide, and its solution is often accompanied by a certain amount of impurity element silicon. If it is directly entered into the next step of the process of preparing germanium dioxide without treatment, it will seriously affect the product quality. Although the existing desiliconization methods and desiliconization reagents are diverse, they often face problems such as low efficiency, high cost and complex operation in practical applications. Therefore, it is very necessary to develop a sodium germanate solution desiliconization reagent and application that can solve the above technical problems. Summary of the invention
[0003] The first purpose of the present invention is to provide a sodium germanate solution desiliconization reagent MC306; the second purpose is to provide a preparation method of the sodium germanate solution desiliconization reagent MC306; the third purpose is to provide an application of the sodium germanate solution desiliconization reagent MC306.
[0004] The first object of the present invention is achieved in that the sodium germanate solution desiliconization reagent MC306 is prepared using sodium sulfate, gelatin, flocculant, and ethylenediaminetetraacetic acid (EDTA) as raw materials; the flocculant is CMC, aluminum chloride, aluminum sulfate or polyacrylamide.
[0005] The second object of the present invention is achieved by subjecting sodium sulfate, gelatin, flocculant and ethylenediaminetetraacetic acid (EDTA) in a prescribed ratio to a pressure reaction under an oxygen atmosphere to prepare the product.
[0006] The specific operation is as follows: sodium sulfate, gelatin, flocculant, ethylenediaminetetraacetic acid (EDTA) are pressurized and reacted for 1-4 hours at an oxygen pressure of 1.2-1.5 kPa and a temperature of 180-300°C, and then separated by suction filtration to obtain a composite reagent MC306 for desiliconization in sodium germanate solution; wherein the molar ratio of sodium sulfate, gelatin, flocculant, and EDTA is 1:2-40:1-10:1-15. The desiliconization agent has a significant effect on the removal of silicon from the sodium germanate solution under high acid and high temperature conditions.
[0007] The third object of the present invention is achieved by using the sodium germanate solution desiliconization reagent MC306 in the sodium germanate solution desiliconization process.
[0008] The technical principle of the sodium germanate solution desiliconization reagent MC306 described in the present invention is: under the modification of gelatin, the sodium ions in sodium sulfate exchange hydroxyl groups with the carboxyl groups in ethylenediaminetetraacetic acid (EDTA) to form a cationic complex, which then reacts with the anionic silicate to form a silicate complex. Under the action of a flocculant (CMC, aluminum chloride, aluminum sulfate, polyacrylamide), the silicate complex agglomerates and precipitates, thereby achieving the separation of silicon and germanium. DETAILED DESCRIPTION
[0009] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0010] The sodium germanate solution desiliconization reagent MC306 of the present invention is prepared by using sodium sulfate, gelatin, flocculant and ethylenediaminetetraacetic acid (EDTA) as raw materials; the flocculant is CMC, aluminum chloride, aluminum sulfate or polyacrylamide.
[0011] The molar ratio of the sodium sulfate, gelatin, flocculant and ethylenediaminetetraacetic acid (EDTA) is 1: (2-40): (1-10): (1-15).
[0012] The method for preparing the sodium germanate solution desiliconization reagent MC306 of the present invention is to prepare the sodium germanate solution desiliconization reagent MC306 by subjecting sodium sulfate, gelatin, flocculant and ethylenediaminetetraacetic acid (EDTA) in a prescribed ratio to a pressure reaction under an oxygen atmosphere.
[0013] The oxygen pressure of the pressurized reaction is 1.2~1.5KPa.
[0014] The temperature of the pressurized reaction is 180-300°C.
[0015] The time of the pressurized reaction is 1 to 4 hours.
[0016] The application of the sodium germanate solution desiliconization reagent MC306 described in the present invention is the application of the sodium germanate solution desiliconization reagent MC306 in the sodium germanate solution desiliconization process.
[0017] The application of the sodium germanate solution desiliconization reagent MC306 in the sodium germanate solution desiliconization process is to add the sodium germanate solution desiliconization reagent MC306 into the sodium germanate solution for oscillation separation.
[0018] The frequency of the oscillation separation is 150-200 r / min.
[0019] The oscillation separation time is 40 to 60 minutes.
[0020] The present invention is further described below with specific implementation cases: Example 1 Sodium sulfate, gelatin, flocculant CMC and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 1:2:1:1 were pressurized and reacted for 4 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 180-200°C. The sodium germanate solution desiliconization reagent MC306 was prepared by suction filtration and separation.
[0021] Example 2 Sodium sulfate, gelatin, flocculant aluminum chloride and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 1:40:10:15 were pressurized and reacted for 1 hour at an oxygen pressure of 1.2-1.5 KPa and a temperature of 280-300°C. The sodium germanate solution desiliconization reagent MC306 was prepared by suction filtration and separation.
[0022] Example 3 Sodium sulfate, gelatin, flocculant aluminum sulfate, and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 1:5:6:10 were pressurized and reacted for 3 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 200-230°C. The sodium germanate solution desiliconization reagent MC306 was prepared by suction filtration and separation.
[0023] Example 4 Sodium sulfate, gelatin, flocculant polyacrylamide and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 1:30:5:8 were pressurized and reacted for 2 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 260-280°C. The sodium germanate solution desiliconization reagent MC306 was prepared by suction filtration and separation.
[0024] Example 5 Sodium sulfate, gelatin, flocculant CMC and ethylenediaminetetraacetic acid (EDTA) in a molar ratio of 1:15:3:6 were pressurized and reacted for 2.5 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 230-260°C. The sodium germanate solution desiliconization reagent MC306 was prepared by suction filtration and separation.
[0025] Example 6 The copper fume leaching solution prepared in Example 3 was used to extract the molybdenum reagent for testing, as follows: Accurately measure 15-40% volume fraction of copper fume leaching solution to extract molybdenum reagent, and carry out desiliconization test on sodium germanate solution containing Si0.1-5g / L, compared with O / A=1:1-8, the oscillation frequency is 150-200r / min, and the oscillation is carried out at room temperature for 40-60min. After the reaction stops, the desiliconization rate of the sodium germanate solution reaches 92-99% after filtration and separation.
[0026] Example 7 The sodium germanate solution desiliconization reagent MC306 prepared in Example 1, Example 2, Example 4, and Example 5 were tested respectively, using the same method as Example 6. The results all showed that the sodium germanate solution desiliconization reagent MC306 described in the present invention had a desiliconization rate of 92-99% for the sodium germanate solution.
Claims
1. A sodium germanate solution desiliconization reagent MC306, characterized in that: The sodium germanate solution desiliconization reagent MC306 is prepared using sodium sulfate, gelatin, flocculant, and ethylenediaminetetraacetic acid (EDTA) as raw materials; the flocculant is CMC, aluminum chloride, aluminum sulfate or polyacrylamide.
2. The sodium germanate solution desiliconization reagent MC306 according to claim 1, characterized in that: The molar ratio of the sodium sulfate, gelatin, flocculant and ethylenediaminetetraacetic acid (EDTA) is 1: (2-40): (1-10): (1-15).
3. A method for preparing the sodium germanate solution desiliconization reagent MC306 described in 1 or 2, characterized in that: The preparation method is prepared by subjecting sodium sulfate, gelatin, flocculant and ethylenediaminetetraacetic acid (EDTA) in a formulated ratio to a pressure reaction under an oxygen atmosphere.
4. The preparation method according to claim 3, characterized in that: The oxygen pressure of the pressurized reaction is 1.2~1.5KPa.
5. The preparation method according to claim 3, characterized in that: The temperature of the pressurized reaction is 180-300°C.
6. The preparation method according to claim 3, characterized in that: The time of the pressurized reaction is 1 to 4 hours.
7. An application of the sodium germanate solution desiliconization reagent MC306 according to claim 1 or 2, characterized in that: The application of the sodium germanate solution desiliconization reagent MC306 in the sodium germanate solution desiliconization process.
8. The use according to claim 7, characterized in that: The application of the sodium germanate solution desiliconization reagent MC306 in the sodium germanate solution desiliconization process is to add the sodium germanate solution desiliconization reagent MC306 into the sodium germanate solution for oscillation separation.
9. The use according to claim 8, characterized in that: The frequency of the oscillation separation is 150-200 r / min.
10. The use according to claim 8, characterized in that: The oscillation separation time is 40 to 60 minutes.