Nanoscale particle hybrid reinforced titanium-based composite material powder and preparation method thereof

By using ultrasonic atomization technology in the preparation of titanium-based composite powder, the problems of irregular shape and poor fluidity of powder particles in traditional methods were solved, and a high spherical and uniform distribution of titanium-based composite powder was prepared, suitable for additive materials Manufacturing improves the mass and mechanical properties of the components.

CN119082527AActive Publication Date: 2024-12-06SHENYANG UNIVERSITY OF TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411198711.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

In the traditional titanium-based composite powder preparation method, the powder particles are irregular in shape, poor in fluidity, large span of reinforcement size and uneven distribution, which makes it difficult to completely melt during the additive manufacturing process, forming defects, affecting the quality and mechanical properties of the components. .

Method used

The preparation method of nano-grade particle hybrid reinforced titanium-based composite powder includes grinding the matrix alloy block, mixing the mechanical powder and the reinforced powder according to a specific mass ratio, pressing into the block and then in a vacuum non-consumable arc furnace smelting to form ingots, and then powdering by ultrasonic atomization to produce titanium-based composite powder with high spherical shape, poreless or broken particles.

Benefits of technology

It solved the problems of irregular powder shape, poor fluidity and uneven distribution of reinforcement bodies, and prepared titanium-based composite powder with smooth surface, high spherical shape and uniform particle size distribution. It is suitable for additive manufacturing, and improves the quality of components and Mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082527A_ABST
    Figure CN119082527A_ABST
Patent Text Reader

Abstract

The invention discloses nanoscale particle hybrid reinforced titanium-based composite material powder and a preparation method thereof. The preparation method comprises the following steps: pressing a matrix alloy block and various reinforcement powder into an alloy block; the alloy block is subjected to vacuum non-consumable smelting, and an embedded reinforcement alloy ingot is prepared; and the alloy ingot is subjected to ultrasonic atomization powder making, and the embedded evenly-distributed nanoscale particle hybrid reinforced titanium-based composite material spherical powder is prepared. By means of the method, the embedded reinforcement particle hybrid reinforced titanium-based composite material powder can be prepared, and the obtained powder is high in sphericity degree, good in surface quality, free of pores or breakage and free of satellite balls or adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal powder preparation, and in particular to a nano-level particle hybrid reinforced titanium-based composite material powder and a preparation method thereof. Background Art

[0002] Titanium-based composites, as a high-performance metal-based composite material, use titanium or titanium alloy as the matrix, and embed reinforcements such as fibers or particles into the matrix to significantly improve its mechanical properties. This material has the advantages of wear resistance, heat resistance, high strength and high hardness, and is widely used in aerospace, automotive and high-performance engineering applications, and shows great development potential. The preparation methods of traditional titanium-based composites mainly include powder metallurgy and casting, both of which use the in-situ reaction between the matrix and the additive to synthesize the reinforcement. However, due to the poor thermal conductivity of titanium-based composites, the introduction of hard reinforcements and the difficulty of processing, it is difficult to achieve near-net-shape processing of its integrated components, which limits its application in fields with high processing precision requirements such as biomedicine and high-end equipment manufacturing.

[0003] Additive manufacturing, as a near-net-shape forming process, has been widely used and recognized in recent decades. Additive manufacturing is based on a three-dimensional digital model to build parts with complex shapes by accumulating materials layer by layer. Its advantage is that it greatly expands the degree of freedom of design and can manufacture complex and multi-component metal structures. Therefore, additive manufacturing technology provides a feasible way to achieve near-net-shape forming of complex components of particle-reinforced titanium-based composite materials. The raw materials in the additive manufacturing process exist in the form of metal powder, wire or strip. Metal powder has high fluidity and adjustability, compatibility with a variety of printing technologies and flexibility in building parts with various geometric shapes, which effectively promotes high-precision and high-performance printing results and meets the high standards of industrial applications. In the additive manufacturing process, the morphology, particle size distribution, performance and quality of metal powder are crucial to the integrity and mechanical properties of the component.

[0004] The preparation of titanium-based composite powder raw materials for additive manufacturing usually uses a mechanical mixing method, that is, the matrix alloy powder and the reinforcement powder are mixed and then high-energy ball milled to make the reinforcement powder adhere to the matrix alloy powder to form an external composite powder, and then the composite powder is used for additive manufacturing. This powder making method has problems such as irregular powder particle shape, poor powder fluidity, and large reinforcement size span and uneven distribution. In addition, due to the short laser processing time and fast cooling, and the melting point of the reinforcement raw material is usually much higher than that of the matrix, it is difficult to completely melt it during the additive manufacturing process, and it is eventually deposited in the matrix to form defects, causing stress concentration or cracks, etc., which seriously affects the quality and mechanical properties of additive manufacturing components. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a nano-scale particle mixed reinforced titanium-based composite material powder and a preparation method thereof, aiming to solve the problem that the composite powder prepared by the traditional method has irregular shape, poor fluidity, and a large size span and uneven distribution of the reinforcement, which makes it difficult to completely melt and form deposition during use.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: In a first aspect, a method for preparing a nano-particle hybrid reinforced titanium-based composite material powder comprises: Step 1: grinding the base alloy block, mixing a plurality of reinforcement powders by mechanical powder mixing, adding the powders to the ground base alloy block, and pressing the mixed powders into a block; Step 2, melting the block into a titanium-based composite ingot using a vacuum non-consumable arc furnace; Step 3: Powdering the titanium-based composite material ingot by ultrasonic atomization to obtain titanium-based composite material powder.

[0007] Furthermore, in step 1, the base alloy block is a Ti6Al4V alloy block, and the surface of the Ti6Al4V alloy block is polished with sandpaper to remove the surface oxide layer and impurities.

[0008] Furthermore, in step 1, adding the reinforcement powder to the polished matrix alloy block and pressing it into a block comprises: The mass fractions of Ti6Al4V alloy block, reinforcement Si powder and TiB2 powder are 95.85%, 2.19% and 1.96% respectively. Then, the reinforcement Si powder and the reinforcement TiB2 powder are mechanically mixed at 200rpm for 2h using a powder mixer, and then pressed into a block with the matrix Ti6Al4V alloy.

[0009] Furthermore, in step 1, adding the reinforcement powder to the polished matrix alloy block and pressing it into a block comprises: The mass fractions of Ti6Al4V alloy block, reinforcement C powder and reinforcement TiB2 powder are 97.43%, 0.69% and 1.88% respectively. Then, the reinforcement C powder and the reinforcement TiB2 powder are mechanically mixed at 200rpm for 2h using a powder mixer, and then pressed into a block with the matrix Ti6Al4V alloy.

[0010] Furthermore, in step 1, adding the reinforcement powder to the polished matrix alloy block and pressing it into a block comprises: The mass fractions of Ti6Al4V alloy block, reinforcement C powder and Si powder are 98.54%, 0.71% and 0.75% respectively. Then, the reinforcement C powder and the reinforcement Si powder are mechanically mixed at 200 rpm for 2 hours using a powder mixer, and then pressed into a block with the matrix Ti6Al4V alloy.

[0011] Furthermore, in step 2, the block is melted into a titanium-based composite material ingot using a vacuum non-consumable arc furnace, which includes: First, clean the furnace of the electric arc furnace: use argon gas to wash the furnace of the electric arc furnace three times to minimize gas impurities such as oxygen, nitrogen, and hydrogen during the smelting process and reduce pollution sources. Then, vacuum the electric arc furnace to a vacuum degree of 1×10 -4 ~1×10 -5 Pa; The block is placed on a water-cooled copper crucible in a vacuum non-consumable electric arc furnace, the door of the electric arc furnace is closed, and smelting is performed to obtain an ingot.

[0012] Further, the smelting block parameters include: The melting current is set to 1-3.5 kA, and the melting times are ≥5 times, among which, the melting is performed once after turning over, and finally a titanium-based composite material ingot is obtained.

[0013] Furthermore, the step 3 comprises: First, the titanium-based composite ingot is placed on an ultrasonic atomization table. The input heat source is the plasma generated by an arc melter, the current is 215A, and the melting temperature is above 1400°C. The ultrasonic frequency is set to 40kHz, the amplitude displacement is 100%, and the argon flow rate is set to 10NL / min, and finally the titanium-based composite powder is obtained.

[0014] The technical solution adopted by the present invention has the following beneficial effects: In the present application, the reinforcement powder is mixed with the matrix Ti6Al4V alloy according to the corresponding mass ratio and then pressed into a block, and then placed in a water-cooled copper crucible in the furnace of a vacuum non-consumable arc furnace for arc melting, and the reinforcement phase is directly generated by the in-situ autogenous reaction between the matrix alloy and the reinforcement to prepare a particle-reinforced Ti6Al4V-based composite material ingot, and then the ingot is placed on an ultrasonic atomization table, and the titanium-based composite material ingot is melted by an arc melter, and then atomized into fine droplets under the action of ultrasound, and solidified into metal powder during the outward spraying process. The titanium-based composite material powder prepared by the embedded reinforcement preparation method has the advantages of high sphericity, no pores or broken particles, and a smooth surface without satellite balls, etc., which solves the problems of irregular powder shape, rough surface, poor fluidity, wide particle size distribution, uneven distribution of reinforcements and inconsistent powder properties existing in the titanium-based composite material powder prepared by the traditional mechanical mixing method or gas atomization method. Therefore, ultrasonic atomization powder making technology can not only effectively prepare titanium-based composite material powders, but also the powders can be used as high-quality raw materials in additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A powder preparation flow chart of a nano-particle hybrid reinforced titanium-based composite material powder provided by the present invention; Figure 2 The technical route of the method for manufacturing a nano-particle hybrid reinforced titanium-based composite material powder provided by the present invention and the scanning electron microscope image of the spherical powder; Figure 3 A powder cross-section scanning electron microscope image of a nano-particle hybrid reinforced titanium-based composite material powder provided by the present invention. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0017] In the first aspect, in this embodiment, the present invention provides a nano-scale particle hybrid reinforced titanium-based composite material powder, which has the advantages of high sphericity, no pores or broken particles, and a smooth surface without satellite balls, and can be used as a high-quality titanium-based composite material powder raw material in additive manufacturing; wherein, please refer to Figure 1 The preparation method of nano-particle hybrid reinforced titanium-based composite material powder is as follows: Example 1 Preparation of ingot raw materials In order to improve the quality of the ingot after smelting, the surface of the Ti6Al4V alloy block is first polished with sandpaper to remove the surface oxide layer and impurities, thereby reducing inclusions during the smelting process and ensuring the purity and uniformity of the ingot.

[0018] The mass fractions of Ti6Al4V, reinforcement Si powder and TiB2 powder added to prepare titanium-based composite ingots are 95.85%, 2.19% and 1.96%, respectively. Subsequently, the reinforcement Si powder and the reinforcement TiB2 powder are mechanically mixed at 200rpm for 2h in a powder mixer and then pressed into blocks with the matrix Ti6Al4V alloy. The purpose of powder mixing is to make the reinforcement powders mix evenly and distribute them evenly on the matrix Ti6Al4V alloy after being pressed into blocks, so as to ensure that the reinforcements are evenly distributed in the organization during the subsequent smelting process, avoid segregation during the smelting process, and improve the uniformity and consistency of the titanium-based composite ingots.

[0019] The pressed block is then placed on a water-cooled copper crucible in a vacuum non-consumable electric arc furnace, and the door of the electric arc furnace is closed. In order to prepare titanium-based composite materials with high purity and few impurities, it is necessary to use argon gas to wash the furnace of the electric arc furnace three times to minimize gas impurities such as oxygen, nitrogen, and hydrogen during the smelting process, reduce pollution sources, and ensure the high purity of the ingot. The electric arc furnace is then evacuated to a vacuum degree of 1×10 -4 ~1×10 -5 Pa, a vacuum degree lower than this value range may result in gas contamination of the ingot, increased porosity and reduced surface quality, etc.

[0020] In order to ensure the full melting of the matrix alloy and the reinforcement powder and the complete in-situ autogenous reaction, the melting current is 1~3.5kA. At the same time, in order to ensure the uniformity and melting quality of the melting ingot, the melting times are ≥5 times (including one melting after the ingot is turned over), and finally a titanium-based composite ingot is obtained.

[0021] Ultrasonic atomization powder making; The entire powder making process is completed in a stainless steel vacuum chamber. First, the titanium-based composite ingot is placed on an ultrasonic atomization table, and the input heat source is the plasma generated by the arc melter, the current is 215A, and the melting temperature is 1400℃. Below this temperature, the ingot cannot be completely melted, affecting the fluidity and surface tension of the melt, and further affecting the size, distribution, powder making efficiency and yield of the powder particles.

[0022] Since different ultrasonic frequencies and amplitude displacements can have a significant impact on the yields of different powder particle size ranges, in order to prepare the powder with the highest yield in the target particle size range (50-100 μm) and promote melt breakage and atomization to improve atomization efficiency, the ultrasonic frequency was set to 40 kHz and the amplitude displacement was set to 100%.

[0023] In order to promote the condensation of tiny droplets produced by melt atomization into powder, and to ensure the effective collection of powder and prevent its oxidation, the argon flow rate was set to 10NL / min. The particle size distribution, yield and sphericity of the final prepared powder are shown in the following table.

[0024] Example 2 Preparation of ingot raw materials In order to improve the quality of the ingot after smelting, the surface of the Ti6Al4V alloy block is first polished with sandpaper to remove the surface oxide layer and impurities, thereby reducing inclusions during the smelting process and ensuring the purity and uniformity of the ingot.

[0025] The mass fractions of Ti6Al4V, reinforcement C powder and reinforcement TiB2 powder added to prepare titanium-based composite ingots are 97.43%, 0.69% and 1.88%, respectively. Subsequently, the reinforcement C powder and the reinforcement TiB2 powder are mechanically mixed at 200rpm for 2h in a powder mixer and then pressed into blocks with the matrix Ti6Al4V alloy. The purpose of powder mixing is to mix the reinforcement powders evenly and distribute them evenly on the matrix Ti6Al4V alloy after being pressed into blocks, so as to ensure that the reinforcements are evenly distributed in the organization during the subsequent smelting process, avoid segregation during the smelting process, and improve the uniformity and consistency of the titanium-based composite ingots.

[0026] The pressed block is then placed on a water-cooled copper crucible in a vacuum non-consumable electric arc furnace, and the door of the electric arc furnace is closed. In order to prepare titanium-based composite materials with high purity and few impurities, it is necessary to use argon gas to wash the furnace of the electric arc furnace three times to minimize gas impurities such as oxygen, nitrogen, and hydrogen during the smelting process, reduce pollution sources, and ensure the high purity of the ingot. The electric arc furnace is then evacuated to a vacuum degree of 1×10 -4 ~1×10 -5 Pa, a vacuum degree lower than this value range may result in gas contamination of the ingot, increased porosity and reduced surface quality, etc.

[0027] In order to ensure the full melting of the matrix alloy and the reinforcement powder and the complete in-situ autogenous reaction, the melting current is 1~3.5kA. At the same time, in order to ensure the uniformity and melting quality of the melting ingot, the melting times are ≥5 times (including one melting after the ingot is turned over), and finally a titanium-based composite ingot is obtained.

[0028] Ultrasonic atomization powder making The entire powder making process is completed in a stainless steel vacuum chamber. First, the titanium-based composite ingot is placed on an ultrasonic atomization table, and the input heat source is the plasma generated by the arc melter, the current is 215A, and the melting temperature is 1400℃. Below this temperature, the ingot cannot be completely melted, affecting the fluidity and surface tension of the melt, and further affecting the size, distribution, powder making efficiency and yield of the powder particles.

[0029] Since different ultrasonic frequencies and amplitude displacements can have a significant impact on the yields of different powder particle size ranges, in order to prepare the powder with the highest yield in the target particle size range (50~100μm) and promote melt crushing and atomization to improve atomization efficiency, the ultrasonic frequency is set to 40kHz and the amplitude displacement is set to 100%. In order to promote the condensation of tiny droplets produced by melt atomization into powder, while ensuring effective collection of the powder and preventing its oxidation, the argon flow rate is set to 10NL / min. The particle size distribution, yield and sphericity of the final prepared powder are shown in the following table.

[0030] Example 3 Preparation of ingot raw materials In order to improve the quality of the ingot after smelting, the surface of the Ti6Al4V alloy block was first polished with sandpaper to remove the surface oxide layer and impurities, thereby reducing inclusions during the smelting process and ensuring the purity and uniformity of the ingot. The mass fractions of Ti6Al4V, reinforcement C powder and Si powder added to prepare the titanium-based composite ingot were 98.54%, 0.71% and 0.75%, respectively. Then, the reinforcement C powder and reinforcement Si powder were mechanically mixed at 200rpm for 2h by a powder mixer and then pressed into a block with the matrix Ti6Al4V alloy. The purpose of powder mixing is to make the reinforcement powder mix evenly and evenly distribute it on the matrix Ti6Al4V alloy after being pressed into a block, so as to ensure that the reinforcement is evenly distributed in the organization during the subsequent smelting process, avoid segregation during the smelting process, and improve the uniformity and consistency of the titanium-based composite ingot.

[0031] The pressed block is then placed on a water-cooled copper crucible in a vacuum non-consumable electric arc furnace, and the door of the electric arc furnace is closed. In order to prepare titanium-based composite materials with high purity and few impurities, it is necessary to use argon gas to wash the furnace of the electric arc furnace three times to minimize gas impurities such as oxygen, nitrogen, and hydrogen during the smelting process, reduce pollution sources, and ensure the high purity of the ingot.

[0032] The arc furnace is then vacuumed to a vacuum degree of 1×10 -4 ~1×10 -5Pa, vacuum degree lower than this value range may cause gas contamination of the ingot, increased porosity and decreased surface quality, etc. In order to ensure the full melting of the matrix alloy and the reinforcement powder, and complete in-situ autogenous reaction, the smelting current is 1~3.5kA. At the same time, in order to ensure the uniformity and smelting quality of the smelting ingot, the smelting times are ≥5 times (including one smelting after the ingot is turned over), and finally a titanium-based composite ingot is obtained.

[0033] Ultrasonic atomization powder making The entire powder making process is completed in a stainless steel vacuum chamber. First, the titanium-based composite ingot is placed on an ultrasonic atomization table, and the input heat source is the plasma generated by the arc melter, the current is 215A, and the melting temperature is 1400℃. Below this temperature, the ingot cannot be completely melted, affecting the fluidity and surface tension of the melt, and further affecting the size, distribution, powder making efficiency and yield of the powder particles.

[0034] Since different ultrasonic frequencies and amplitude displacements can have a significant impact on the yields of different powder particle size ranges, in order to prepare the powder with the highest yield in the target particle size range (50~100μm) and promote melt crushing and atomization to improve atomization efficiency, the ultrasonic frequency is set to 40kHz and the amplitude displacement is set to 100%. In order to promote the condensation of tiny droplets produced by melt atomization into powder, while ensuring effective collection of the powder and preventing its oxidation, the argon flow rate is set to 10NL / min. The particle size distribution, yield and sphericity of the final prepared powder are shown in the following table.

[0035] In this example, see Figure 2 The object of the present invention is to provide a high-quality embedded uniformly distributed nano-particle hybrid reinforced titanium-based composite material powder for additive manufacturing and a preparation method thereof, wherein the reinforcement powder is mixed with the matrix Ti6Al4V alloy according to the corresponding mass ratio and then pressed into a block, which is then placed in a water-cooled copper crucible in the furnace of a vacuum non-consumable arc furnace for arc melting, and a reinforcement phase is directly generated by an in-situ autogenous reaction between the matrix alloy and the reinforcement to prepare a particle-reinforced Ti6Al4V-based composite material ingot, and then the ingot is placed on an ultrasonic atomization table, and the titanium-based composite material ingot is melted by an arc melter, and then atomized into fine droplets under the action of ultrasonic waves, and solidified into metal powder during the outward spraying process.

[0036] See also Figure 3 , Figure 3 The scanning electron microscope image of the powder cross section is shown in the figure. It can be seen that the reinforcements are evenly distributed in the powder structure of the titanium-based composite material prepared by the embedded reinforcement preparation method, and there are no cracks or shrinkage holes inside the particles.

[0037] In the present invention, the titanium-based composite material powder prepared by the embedded reinforcement preparation method has the advantages of high sphericity, no pores or broken particles, and a smooth surface without satellite balls, etc., which solves the problems of irregular powder shape, rough surface, poor fluidity, wide particle size distribution, uneven reinforcement distribution and inconsistent powder properties existing in the titanium-based composite material powder prepared by the traditional mechanical mixing method or gas atomization method. Therefore, the ultrasonic atomization powder making technology can not only effectively prepare titanium-based composite material powder, but also the powder can be used as a high-quality raw material in additive manufacturing.

[0038] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the schemes disclosed herein. The present invention is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed in this disclosure. The description and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the claims.

Claims

1. A method for preparing nano-particle hybrid reinforced titanium-based composite material powder, characterized in that: include: Step 1: grinding the base alloy block, mixing a plurality of reinforcement powders by mechanical powder mixing, adding the powders to the ground base alloy block, and pressing the mixed powders into a block; Step 2, melting the block into a titanium-based composite ingot using a vacuum non-consumable arc furnace; Step 3: Powdering the titanium-based composite material ingot by ultrasonic atomization to obtain titanium-based composite material powder.

2. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 1, characterized in that: In the step 1, the base alloy block is a Ti6Al4V alloy block, and the surface of the Ti6Al4V alloy block is polished with sandpaper to remove the surface oxide layer and impurities.

3. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 1, characterized in that: In step 1, adding a plurality of reinforcement powders to the ground base alloy block and pressing the block into a block comprises: The mass fractions of Ti6Al4V alloy block, reinforcement Si powder and TiB2 powder are 95.85%, 2.19% and 1.96% respectively. Then, the reinforcement Si powder and the reinforcement TiB2 powder are mechanically mixed at 200rpm for 2h using a powder mixer, and then pressed into a block with the matrix Ti6Al4V alloy.

4. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 1, characterized in that: In step 1, adding a plurality of reinforcement powders to the ground base alloy block and pressing the block into a block comprises: The mass fractions of Ti6Al4V alloy block, reinforcement C powder and reinforcement TiB2 powder are 97.43%, 0.69% and 1.88% respectively. Then, the reinforcement C powder and the reinforcement TiB2 powder are mechanically mixed at 200rpm for 2h using a powder mixer, and then pressed into a block with the matrix Ti6Al4V alloy.

5. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 1, characterized in that: In step 1, adding a plurality of reinforcement powders to the ground base alloy block and pressing the block into a block comprises: The mass fractions of Ti6Al4V alloy block, reinforcement C powder and Si powder are 98.54%, 0.71% and 0.75% respectively. Then, the reinforcement C powder and the reinforcement Si powder are mechanically mixed at 200 rpm for 2 hours using a powder mixer, and then pressed into a block with the matrix Ti6Al4V alloy.

6. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 1, characterized in that: In step 2, the block is melted into a titanium-based composite material ingot by using a vacuum non-consumable arc furnace, which comprises: First, clean the furnace of the electric arc furnace: use argon gas to wash the furnace of the electric arc furnace three times to minimize gas impurities such as oxygen, nitrogen, and hydrogen during the smelting process and reduce pollution sources. Then, vacuum the electric arc furnace to a vacuum degree of 1×10 -4 ~1×10 -5 Pa; The block is placed on a water-cooled copper crucible in a vacuum non-consumable electric arc furnace, the door of the electric arc furnace is closed, and smelting is performed to obtain an ingot.

7. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 6, characterized in that: Melting block parameters include: The melting current is set to 1-3.5 kA, and the melting times are ≥5 times, among which, the melting is performed once after turning over, and finally a titanium-based composite material ingot is obtained.

8. The method for preparing nano-particle hybrid reinforced titanium-based composite material powder according to claim 1, characterized in that: The step 3 comprises: First, the titanium-based composite ingot is placed on an ultrasonic atomization table. The input heat source is the plasma generated by an arc melter, the current is 215A, and the melting temperature is above 1400°C. The ultrasonic frequency is set to 40kHz, the amplitude displacement is 100%, and the argon flow rate is set to 10NL / min, and finally the titanium-based composite powder is obtained.

Citation Information

Patent Citations

  • Boron-containing ti-based composite powder for 3D printing and preparation method thereof

    CN110218907A

  • Preparation method for powder for additive manufacturing for particle-reinforced titanium-based composite material

    CN110340371A

  • Boron-containing titanium-based composite powder for 3D printing and method of preparing same

    US20200399135A1

  • AU2020101927A4