Preparation method of acid digital printing pretreatment slurry containing modified guar gum

The preparation of acidic digital printing pretreatment slurry by compounding modified guar gum and other additives has solved the problems of low printing depth, poor clarity and poor color fastness in the prior art, and significantly improved the printed fabric Printing effect and comprehensive performance.

CN119083206APending Publication Date: 2024-12-06SHANGHAI QINGMU TEXTILE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411280811.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing acidic digital printing pretreatment agents lead to low printing depth, poor definition and poor color fastness, which affects printing quality.

Method used

Using acidic digital printing pretreatment slurry containing modified guar gum, a highly efficient pretreatment slurry, including modified guar gum and penetration agent, thickener, urea, ammonium sulfate and acidic pH adjusters to improve the printing depth, clarity and color fastness of printed fabrics.

Benefits of technology

It improves the printing depth, clarity, color fastness and uniformity of printed fabrics, and improves the comprehensive performance of acid digital printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of modified guar gum-containing acidic digital printing pretreatment slurry, which comprises the following steps: (a) dissolving modified guar gum in part of water, uniformly stirring, and standing for 20-24 hours; (b) taking the rest water, adding a thickening agent, stirring and dissolving, then adding a penetrating agent while stirring, uniformly mixing, then adding urea, ammonium sulfate and the modified guar gum solution, continuously stirring and uniformly mixing, finally adding an acidic pH regulator, and uniformly mixing to obtain pretreatment slurry; the obtained pretreatment slurry comprises the following components in percentage by weight: 3-6% of modified guar gum, 2-4.3% of a penetrating agent, 1-3.5% of a thickening agent, 3-8% of urea, 1-2% of ammonium sulfate, 1-5% of an acidic pH regulator and the balance of water. When the obtained pretreatment slurry is applied to a printing process, a printed fabric with the characteristics of high color yield, high printing depth, good printing uniformity, high definition and the like can be obtained, and the comprehensive performance of acid digital printing is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of digital printing, and more specifically to a method for preparing an acidic digital printing pretreatment slurry containing modified guar gum. Background Art

[0002] Acid digital printing generally starts with sizing the fabric, and then proceeds with the acid digital printing process, including printing, drying, steaming, soaping, etc., so sizing is the primary process of acid digital printing and is directly related to the effect of acid digital printing. The pre-treatment slurry can promote the acid dye to combine with the fiber under wet and hot conditions to obtain a certain color depth and color fastness, so in a sense, the pre-treatment process is the basis of acid digital printing.

[0003] Currently, most printing manufacturers still use conventional acidic printing pastes such as guar gum, sodium alginate, and carboxymethyl cellulose as pre-treatment agents for acidic digital printing of fabrics. However, such products still have problems such as low printing depth, poor clarity, and low fastness, which directly affect the quality of digital printing. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing an acidic digital printing pretreatment slurry containing modified guar gum. The obtained pretreatment slurry is applied to the printing process to obtain printed fabrics with high color yield, high printing depth, good printing uniformity, high clarity and the like, thereby improving the comprehensive performance of acidic digital printing.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum comprises the following steps:

[0007] (a) dissolving the modified guar gum in a portion of water, stirring evenly and leaving for 20-24 hours;

[0008] (b) taking the remaining water, adding a thickener and stirring to dissolve, then adding a penetrant while stirring, adding urea, ammonium sulfate and the modified guar gum solution prepared in step (a) after mixing, continuing to stir and mix, and finally adding an acidic pH regulator and mixing evenly to obtain a pre-treated slurry;

[0009] The obtained pre-treated slurry comprises the following components in percentage: 3-6% of modified guar gum, 2-4.3% of penetrant, 1-3.5% of thickener, 3-8% of urea, 1-2% of ammonium sulfate, 1-5% of acidic pH regulator and the balance of water.

[0010] Furthermore, the modified guar gum is a composition of carboxymethyl guar gum and methyl carboxymethyl guar gum.

[0011] Furthermore, the modified guar gum is a composition of carboxymethyl guar gum and methyl carboxymethyl guar gum in a mass ratio of 1:1.5-3.

[0012] Furthermore, the penetrant is Snritex CSL penetrant. (Weili Chemical (Shanghai) Co., Ltd.)

[0013] Furthermore, the thickener is EM-616T acid dye printing thickener. (Guangdong Yimei Chemical Technology Co., Ltd.).

[0014] Furthermore, the acidic pH adjuster is one of citric acid, acetic acid and lactic acid.

[0015] Furthermore, the mass ratio of the amount of water used in step (a) to the amount of water used in step (b) is 1:2-4.

[0016] Furthermore, the obtained pre-treated slurry includes the following components in percentage: 4.5% of modified guar gum, 3.1% of penetrant, 2.8% of thickener, 6% of urea, 1.5% of ammonium sulfate, 2.1% of acidic pH regulator and the balance of water.

[0017] The beneficial effects of the present invention are:

[0018] The acid digital printing pretreatment slurry used in the printing process is prepared by rationally compounding modified guar gum, penetrant, thickener and other raw materials. The synergistic effect between modified guar gum, penetrant and thickener is utilized to improve the printing depth, clarity, color fastness, color yield and printing uniformity of printed fabrics, thereby improving the comprehensive performance of acid digital printing. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] The method for preparing the acidic digital printing pretreatment slurry containing modified guar gum of the present invention comprises the following steps:

[0021] (a) taking modified guar gum (modified guar gum is a combination of carboxymethyl guar gum and methyl carboxymethyl guar gum, preferably the mass ratio of carboxymethyl guar gum to methyl carboxymethyl guar gum is 1:1.5-3) and dissolving it in part of water, stirring it evenly and then leaving it for 20-24 hours;

[0022] (b) taking the remaining water, adding a thickener (preferably EM-616T acid dye printing thickener purchased from Guangdong Yimei Chemical Technology Co., Ltd.) and stirring to dissolve, then adding a penetrant (preferably Snritex CSL penetrant purchased from Weili Chemical (Shanghai) Co., Ltd.) while stirring, adding urea, ammonium sulfate and the modified guar gum solution prepared in step (a) after mixing, continuing to stir and mix, and finally adding an acidic pH adjuster (one of citric acid, acetic acid, and lactic acid), mixing evenly, to obtain a pre-treated slurry;

[0023] The obtained pre-treated slurry comprises the following components in percentage: 3-6% of modified guar gum, 2-4.3% of penetrant, 1-3.5% of thickener, 3-8% of urea, 1-2% of ammonium sulfate, 1-5% of acidic pH regulator and the balance of water, wherein the mass ratio of the water used in step (a) to the water used in step (b) is 1:2-4.

[0024] Preferred specific embodiments are:

[0025] Example 1

[0026] (a) dissolving a modified guar gum composition having a mass ratio of carboxymethyl guar gum to methyl carboxymethyl guar gum of 1:2 in a portion of water, stirring the mixture evenly and leaving the mixture for 24 hours;

[0027] (b) Take the remaining water, add EM-616T acid dye printing thickener, stir and dissolve, then add Snritex CSL penetrant while stirring, add urea, ammonium sulfate and the modified guar gum solution prepared in step (a) after mixing, continue to stir and mix, finally add acetic acid, mix evenly, and obtain a pre-treated slurry. The obtained pre-treated slurry includes the following components in percentage: 4.5% modified guar gum, 3.1% penetrant, 2.8% thickener, 6% urea, 1.5% ammonium sulfate, 2.1% acidic pH regulator and the balance water; the mass ratio of the amount of water in step (a) to the amount of water in step (b) is 1:3.

[0028] Comparative Example 1

[0029] The acidic digital printing pretreatment slurry was prepared according to the method of Example 1, except that the modified guar gum was replaced by conventional guar gum of the same mass.

[0030] Comparative Example 2

[0031] The acidic digital printing pretreatment slurry was prepared according to the method of Example 1, except that the EM-616T acid dye printing thickener was replaced by an equal mass of water.

[0032] Comparative Example 3

[0033] The acidic digital printing pretreatment slurry was prepared according to the method of Example 1, except that the Snritex CSL penetrant was replaced with water of equal mass.

[0034] The nylon fabrics were sizing with the agents of Example 1, Comparative Examples 1 to Comparative Examples 3 respectively, and then acid digital printing was performed. The performance test results are shown in Table 1.

[0035] Table 1

[0036]

[0037] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum, It is characterized in that The following steps are involved: (a) dissolving the modified guar gum in a portion of water, stirring evenly and leaving for 20-24 hours; (b) taking the remaining water, adding a thickener and stirring to dissolve, then adding a penetrant while stirring, adding urea, ammonium sulfate and the modified guar gum solution prepared in step (a) after mixing, continuing to stir and mix, and finally adding an acidic pH regulator and mixing evenly to obtain a pre-treated slurry; The obtained pre-treated slurry comprises the following components in percentage: 3-6% of modified guar gum, 2-4.3% of penetrant, 1-3.5% of thickener, 3-8% of urea, 1-2% of ammonium sulfate, 1-5% of acidic pH regulator and the balance of water.

2. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The modified guar gum is a composition of carboxymethyl guar gum and methyl carboxymethyl guar gum.

3. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The modified guar gum is a composition of carboxymethyl guar gum and methyl carboxymethyl guar gum in a mass ratio of 1:1.5-3.

4. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The penetrant is Snritex CSL penetrant (Snritex Chemical (Shanghai) Co., Ltd.).

5. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The thickener is EM-616T acid dye printing thickener (Guangdong Yimei Chemical Technology Co., Ltd.).

6. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The acidic pH adjuster is one of citric acid, acetic acid and lactic acid.

7. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The mass ratio of the amount of water used in step (a) to the amount of water used in step (b) is 1:2-4.

8. A method for preparing an acidic digital printing pretreatment slurry containing modified guar gum according to claim 1, It is characterized in that The obtained pre-treated slurry includes the following components in percentage: 4.5% of modified guar gum, 3.1% of penetrant, 2.8% of thickener, 6% of urea, 1.5% of ammonium sulfate, 2.1% of acidic pH regulator and the balance of water.