Non-woven fabric, preparation method and membrane material

By introducing main fibers and molten fibers into nonwoven fabrics and hot pressing, a significant opposite-element on both sides is formed, which solves the problem that the uniform distribution of fibers in the prior art is difficult to meet different surface needs, and realizes nonwoven fabrics in photovoltaics and other fields Improved adaptability and mechanical performance.

CN119083230APending Publication Date: 2024-12-06杭州福斯特功能膜材料有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411168977.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The fibers of existing nonwoven fabrics are single and evenly distributed, making it difficult to meet the application needs of significant differences in the surfaces on both sides in the fields of photovoltaics, water treatment, battery separators, etc., especially in the field of photovoltaics, it is difficult to ensure that the printing and transmission of the battery cells are not simultaneously unavailable. Slip occurs.

Method used

By introducing main fibers and molten fibers into the fiber layer of the nonwoven fabric, the melting point difference is greater than 50°C, and the area of ​​the melting area on both sides is different by hot pressing, forming a significant opposite-element on both sides to meet the needs of different contact interfaces.

Benefits of technology

It realizes that nonwoven fabrics can adapt to the application scenarios where the two sides of the surfaces contact different interfaces without reducing breathability and strength, and improve the adaptability and mechanical properties to different interfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083230A_ABST
    Figure CN119083230A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of non-woven fabrics. The non-woven fabric comprises at least one fiber layer, the fiber layer comprises main body fibers and molten fibers, and the difference value between the melting point of the main body fibers and the melting point of the molten fibers is larger than or equal to 50 DEG C; the two surfaces of the non-woven fabric are the first surface and the second surface respectively, and the difference value between the area of a melting area in the first surface and the area of a melting area in the second surface is 20%-50%. The fusion degree of the non-woven fabric is different, and the non-woven fabric can be applied to the field with different performance requirements on the two faces of the non-woven fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of nonwoven fabrics, and in particular relates to a nonwoven fabric, a preparation method and a membrane material. Background Art

[0002] Nonwoven fabrics are made by diluting fibers and then putting them on a forming net, and then fixing them physically or chemically. Nonwoven fabrics are widely used because of their simple manufacturing and high production efficiency. The fibers in nonwoven fabrics are arranged in a staggered manner vertically and horizontally, with good overall uniformity, and the types of fibers are not restricted or limited during the preparation process.

[0003] Nonwoven fabrics are made of fibers using nonwoven production technology. However, in the process of implementing the technical solution in the embodiments of this application, the applicant found that the above technology has at least the following technical problems:

[0004] As the application of nonwoven fabrics becomes more and more extensive, some new demands have also emerged. In the fields of photovoltaics, water treatment, battery separators, chemistry, etc., the interfaces on both sides of the nonwoven fabric are different, and the two surfaces of the nonwoven fabric need to have significant differences to meet the corresponding use requirements. However, the fibers in the existing nonwoven fabrics are single and evenly distributed, and the surface properties on both sides are basically uniform, which makes it difficult to apply them to related fields.

[0005] For example, in the photovoltaic field, one side of the photovoltaic countertop paper is in contact with the battery cell, and the other side is in contact with the roller, realizing functions such as support and transmission of the battery cell during the printing stage. Since it is necessary to ensure that the battery cell does not slip during the printing stage and to achieve smooth transmission of the battery cell on the production line, and at the same time, it is also required that the transmission between the photovoltaic countertop paper and the roller does not slip, conventional non-woven fabrics with uniform surfaces on both sides are difficult to meet the transmission requirements of the roller and the battery cell at the same time. Summary of the invention

[0006] The embodiment of the present application provides a nonwoven fabric, which can adapt to application scenarios where both sides of the nonwoven fabric contact different interfaces without reducing the air permeability and strength of the nonwoven fabric.

[0007] An embodiment of the present application provides a non-woven fabric, which includes at least one fiber layer, the fiber layer includes main fibers and molten fibers, the difference between the melting point of the main fibers and the melting point of the molten fibers is greater than or equal to 50°C; the two surfaces of the non-woven fabric are respectively a first surface and a second surface, there are molten areas on the first surface and the second surface, and the ratio of the area of ​​the molten area in the first surface to the total area of ​​the first surface and the ratio of the area of ​​the molten area in the second surface to the total area of ​​the second surface is 20%-50%.

[0008] Furthermore, the ratio of the area of ​​the molten region in the first surface to the total area of ​​the first surface is 85%-95%; the ratio of the area of ​​the molten region in the second surface to the total area of ​​the second surface is 45%-70%.

[0009] Furthermore, the two surfaces of the fiber layer are respectively a first fiber surface and a second fiber surface, and the area of ​​the melting region in the first fiber surface is greater than the area of ​​the melting region in the second fiber surface.

[0010] Furthermore, the nonwoven fabric comprises at least two fiber layers; adjacent fiber layers are stacked in one of the following stacking modes: the first fiber surface of one fiber layer is close to the first fiber surface of another fiber layer, the second fiber surface of one fiber layer is close to the second fiber surface of another fiber layer, or the first fiber surface of one fiber layer is close to the second fiber surface of another fiber layer.

[0011] Furthermore, the fineness of the main fiber is 0.5-3D, and the length is 2-15mm; the fineness of the molten fiber is 0.5-3D, and the length is 2-15mm.

[0012] Furthermore, the mass ratio of the main fiber to the molten fiber is (50-70):(30-50).

[0013] Further, the main fiber includes at least one of polyester fiber, polyolefin fiber, polyamide fiber, aramid fiber or polyimide fiber, and the melting fiber includes at least one of polyester fiber, polyolefin fiber, polyamide fiber, aramid fiber or polyimide fiber.

[0014] The embodiment of the present application also provides a preparation method, which is used to prepare any of the above-mentioned nonwoven fabrics; the preparation method includes pulping, dilution, cloth making, drying and hot pressing. Pulping: mixing the main fiber with the molten fiber to prepare a fiber pulp; dilution: diluting the fiber pulp at least three times to obtain a diluted pulp; cloth making: putting the diluted pulp on the net to make a paper sheet after paper making; drying: drying the paper sheet to obtain a fiber layer; the temperature of the drying treatment is greater than or equal to the melting softening temperature of the molten fiber; hot pressing: using at least one of hard pressing or soft pressing to treat the fiber layer or the laminated body after the fiber layer is stacked at 150 to 240°C to obtain a nonwoven fabric; during the hot pressing treatment, the difference in hot pressing temperature between the two sides of the fiber layer or the laminated body is 30 to 70°C.

[0015] Furthermore, during drying, the difference in hard pressing temperature between the two sides of the sheet is 30-60°C.

[0016] Furthermore, in hot pressing, hard pressing includes hard pressing treatment of the fiber layer or the laminate, and the difference in hard pressing temperature between the two sides of the fiber layer or the laminate is 30 to 70°C; soft pressing includes soft pressing treatment of the fiber layer to obtain a non-woven fabric; before the soft pressing treatment, the temperature of the fiber layer is 70 to 180°C.

[0017] An embodiment of the present application further provides a membrane material, which includes any of the above-mentioned non-woven fabrics or a non-woven fabric prepared by any of the above-mentioned preparation methods.

[0018] The present application arranges two kinds of fibers with different melting points in the fiber layer of the non-woven fabric and makes the areas of the melting regions on both sides of the fiber layer different. There is a specific difference between the melting degrees of the two side surfaces of the non-woven fabric, so that the two side surfaces of the non-woven fabric can respectively cope with different contact interfaces, thereby solving the problem of slippage caused by different surfaces of the non-woven fabric contacting different media in device transmission work in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of the cross-sectional structure of a nonwoven fabric in one embodiment of the present application;

[0020] Figure 2 An electron microscope image of the first surface in one embodiment of the present application;

[0021] Figure 3 An electron microscope image of the second surface in one embodiment of the present application;

[0022] Figure 4 This is a schematic diagram of the cross-sectional structure of a fiber layer in one embodiment of the present application;

[0023] Figure 5 This is an electron microscope image of the first fiber surface in one embodiment of the present application;

[0024] Figure 6 This is an electron microscope image of the second fiber surface in one embodiment of the present application;

[0025] Figure 7 This is a schematic diagram of the cross-sectional structure of the fiber layers after stacking in the first embodiment of the present application;

[0026] Figure 8 This is a schematic diagram of the cross-sectional structure of the fiber layers after stacking in the second embodiment of the present application;

[0027] Fig. 9 This is a schematic diagram of the cross-sectional structure of the fiber layers after stacking in the third embodiment of the present application;

[0028] Fig.10 This is a schematic diagram of the cross-sectional structure of the fiber layers after stacking in the fourth embodiment of the present application.

[0029] In the figure: nonwoven fabric 100 , fiber layer 11 , first surface 101 , second surface 102 , first fiber surface 103 , second fiber surface 104 . DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the specific implementation manner of the present application will be clearly and completely described below in conjunction with the drawings in the implementation manner of the present application.

[0031] The present application embodiment provides a Figure 1 The nonwoven fabric 100 shown in FIG. 1 includes at least one fiber layer 11. The two surfaces of the nonwoven fabric 100 are a first surface 101 and a second surface 102. The first surface 101 (eg, Figure 2 The area of ​​the molten region in the second surface 102 (as shown) is larger than that of the second surface 102 (as shown Figure 3The first surface 101 and the second surface 102 have different melting degrees, so that the two sides of the nonwoven fabric 100 have different properties. At the same time, by regulating the melting degrees of the two sides of the nonwoven fabric 100, the surface roughness of the two sides of the nonwoven fabric 100 can be made different, and the roughness of the first surface 101 in the nonwoven fabric 100 can be made less than the roughness of the second surface 102. The first surface and the second surface of the nonwoven fabric 100 have significant differences, especially in roughness and wetting performance, etc., and the nonwoven fabric 100 in the embodiment of the present application can be adjusted according to the actual application scenario. For example, when the nonwoven fabric 100 is applied to the supporting material of the reverse osmosis membrane, the second surface 102 with higher roughness can be used as the coating surface, effectively increasing the contact area between the membrane layer and the supporting material, and improving the peeling strength, while the first surface 101 can be used as a non-coating surface due to its lower roughness, lower porosity and greater surface density, so that it has higher strength and better supports. For another example, when the nonwoven fabric 100 is applied to photovoltaic table paper, the first surface 101 of the nonwoven fabric 100 is relatively smooth and can better carry the battery sheet, and the second surface 102 of the nonwoven fabric 100 is relatively rough, and the friction between the nonwoven fabric 100 and the table surface is relatively large, and it is not easy to slide and shift. Further, the difference between the ratio of the area of ​​the molten area in the first surface 101 to the total area of ​​the first surface 101 and the ratio of the area of ​​the molten area in the second surface 102 to the total area of ​​the second surface 102 is 20%-50%. The difference between the ratio of the area of ​​the molten area in the first surface 101 to the total area of ​​the first surface 101 and the ratio of the area of ​​the molten area in the second surface 102 to the total area of ​​the second surface 102 can make the first surface 101 and the second surface 102 have different properties, and improve the adaptability of the two sides of the nonwoven fabric 100 to different interfaces. The roughness Ra of the first surface can be 1-3.5μm, and the roughness Ra of the second surface can be 3.5-8μm.

[0032] The nonwoven fabric 100 of the embodiment of the present application may include only one fiber layer 11 or multiple fiber layers 11. The fiber layer 11 includes main fibers and molten fibers, and the melting point of the main fibers is greater than the melting point of the molten fibers. When heating and melting, the heating temperature is controlled so that the heating temperature is between the melting point of the main fibers and the melting point of the molten fibers. As the heating proceeds, the molten fibers melt and soften, and flow into the gap formed by the main fibers to achieve bonding to the main fibers. The main fibers have a high melting point and maintain a relatively complete shape when heated. There are still gaps on the surface of the fiber layer 11 formed after heating, so that the fiber layer 11 has good air permeability. By treating the two sides of the nonwoven fabric 100 at different temperatures, the melting degrees of the first surface 101 and the second surface 102 are different, and the two-sided anisotropy of the nonwoven fabric 100 is achieved. Preferably, the difference between the melting point of the main fiber and the melting point of the molten fiber is greater than or equal to 50°C. When the difference between the melting point of the main fiber and the melting point of the molten fiber is greater than or equal to 50°C, it is easier to regulate the melting degree of the main fiber and the molten fiber. The melting degrees of the two sides of the fiber layer 11 in the embodiment of the present application are different, resulting in different roughness and obvious two-sided anisotropy, thereby making the nonwoven fabric 100 composed of the fiber layer 11 also have two-sided anisotropy.

[0033] As an optional embodiment, the area of ​​the molten area in the first surface 101 accounts for 85%-95% of the total area of ​​the first surface 101. The molten area of ​​the first surface 101 accounts for 85%-95%, which can improve the smoothness of the first surface 101 and make the smoothness of each area in the first surface 101 more consistent with the second surface 102. The area of ​​the molten area in the second surface 102 accounts for 45%-70% of the total area of ​​the second surface 102. The molten area of ​​the second surface 102 accounts for less than or equal to 70%, which can make the performance of the second surface 102 different from that of the first surface 101 and rougher; the molten area of ​​the second surface 102 is greater than or equal to 45%, which can make the mechanical strength of the nonwoven fabric 100 higher and the thickness uniformity better. When the area of ​​the molten area in the second surface 102 accounts for 45%-70%, the two-sided anisotropy of the nonwoven fabric 100 is more obvious, and the air permeability uniformity and thickness uniformity of the nonwoven fabric 100 are better.

[0034] As an optional implementation, Figure 4 As shown, the two surfaces of the fiber layer 11 are respectively a first fiber surface 103 and a second fiber surface 104. The first fiber surface 103 (as shown in FIG. Figure 5 The melting area of ​​the second fiber surface 104 (as shown) is larger than that of the second fiber surface 104 (as shown Figure 6The roughness of the first fiber surface 103 is less than the roughness of the second fiber surface 104. The two sides of the fiber layer 11 can also be processed differentially. When the nonwoven fabric 100 includes only one fiber layer 11, the first fiber surface 103 of the fiber layer 11 is the first surface 101 of the nonwoven fabric 100, and the second fiber surface 104 of the fiber layer 11 is the second surface 102 of the nonwoven fabric 100. The different roughness of the first surface 101 and the second surface 102 can also make the fiber layer 11 easier to roll up, which is convenient for completing subsequent processing.

[0035] As an optional embodiment, the nonwoven fabric 100 may also include a plurality of fiber layers 11. After the plurality of fiber layers 11 are stacked, they need to be subjected to a heat pressing treatment so that the plurality of fiber layers 11 form a whole with stable structure and performance. The composite method of the plurality of fiber layers 11 can improve the tensile strength, toughness and other properties of the nonwoven fabric 100, and can reduce the difference between the nonwoven fabrics 100 produced in different batches. The stacking method of adjacent fiber layers 11 may include stacking the first fiber surface 103 of one fiber layer 11 close to the first fiber surface 103 of another fiber layer 11 (such as Figure 7 As shown in FIG. 1 ), the second fiber surface 104 of one fiber layer 11 is stacked close to the second fiber surface 104 of another fiber layer 11 (as shown in FIG. 1 ). Figure 8 ) or the first fiber surface 103 of a fiber layer 11 is stacked close to the second fiber surface 104 of another fiber layer 11 (as shown in Fig. 9 The fiber layers 11 in the same nonwoven fabric 100 can also be stacked in different stacking modes (such as Fig.10 shown). Figures 7 to 10 What is shown is a schematic diagram of the stacking method of multiple fiber layers 11 before lamination, rather than a schematic diagram of the structure of the nonwoven fabric 100 after lamination.

[0036] As an optional embodiment, the thickness of the nonwoven fabric 100 is 80-120 μm. When the thickness of the nonwoven fabric 100 is greater than or equal to 80 μm, the nonwoven fabric 100 has better mechanical properties such as tensile strength; when the thickness of the nonwoven fabric 100 is less than or equal to 120 μm, the nonwoven fabric 100 is relatively thin and has higher air permeability. The thickness of the nonwoven fabric 100 is 80-120 μm, which enables the nonwoven fabric 100 to have both higher mechanical properties and better air permeability.

[0037] As an optional embodiment, the fineness of the main fiber is 0.5-3D and the length is 2-15mm; the fineness of the molten fiber is 0.5-3D and the length is 2-15mm. Within the aforementioned length range, when the main fiber and the molten fiber are shorter, the smoothness of both sides of the nonwoven fabric 100 is higher; when the main fiber and the molten fiber are longer, the air permeability of the nonwoven fabric 100 is better. The lengths of the main fiber and the molten fiber can be the same or different. During production, the main fiber and the molten fiber of appropriate length can be selected according to demand.

[0038] As an optional embodiment, in the fiber slurry, the mass ratio of the main fiber to the molten fiber is (50-70): (30-50). Within the aforementioned ratio range, when the proportion of the main fiber is increased, the air permeability of the nonwoven fabric 100 can be improved. When the proportion of the molten fiber is increased, the tensile strength and surface smoothness of the nonwoven fabric 100 can be improved. The mass ratio of the main fiber to the molten fiber is (50-70): (30-50), which can make the air permeability, surface smoothness and tensile strength of the fiber layer 11 better.

[0039] As an optional embodiment, the main fiber includes at least one of polyester fiber, polyolefin fiber, polyamide fiber, aramid fiber or polyimide fiber. Preferably, the main fiber is polyester fiber. The melting fiber includes at least one of polyester fiber, polyolefin fiber, polyamide fiber, aramid fiber or polyimide fiber. Preferably, the melting fiber is polyester fiber.

[0040] The nonwoven fabric 100 in the present application has good air permeability; and the roughness of the two sides of the nonwoven fabric is different, which has obvious differences.

[0041] The embodiment of the present application also provides a preparation method, which includes pulping, dilution, cloth making, drying and hot pressing. Specifically, pulping: mixing the main fiber with the molten fiber to prepare a fiber pulp. Dilution: diluting the fiber pulp to obtain a diluted pulp. From the perspective of fiber distribution uniformity, preferably, the fiber pulp is diluted no less than three times. In the diluted pulp, the mass fraction of the pulp is 0.01% to 0.05%. Cloth making: the diluted pulp is put on the net for papermaking, and a paper sheet with a moisture content of 15%-25% is obtained after papermaking. Drying: drying the paper sheet to obtain a fiber layer 11; wherein the temperature of the drying treatment must be greater than or equal to the melting softening temperature of the molten fiber. Hot pressing: hot pressing the fiber layer 11 or the laminated body after laminating the fiber layers 11 at 150 to 240°C using at least one of hard pressing or soft pressing to obtain a non-woven fabric 100.

[0042] As an optional implementation, during the drying process, the two sides of the sheet can be dried at different temperatures, and the difference in hot pressing temperature between the two sides of the sheet can be 30-60°C, so that the fiber layer 11 with different properties on both sides can be obtained. For example, in a specific embodiment, the melting and softening temperature range of the molten short fiber is 130-180°C, the upper temperature of the drying tunnel can be set to 130°C, and the lower temperature of the drying tunnel can be set to 180°C. After the sheet is dried in the drying tunnel, the surface near the lower side of the drying tunnel forms the first fiber surface 103, and the surface near the upper side of the drying tunnel forms the second fiber surface 104, so as to obtain a fiber layer 11 with two-sided anisotropy.

[0043] As an optional embodiment, during the hot pressing treatment, the hot pressing temperatures on both sides of the fiber layer 11 or the laminate are different, and the difference in hot pressing temperature between the two sides of the fiber layer 11 or the laminate is 30 to 60° C., so that a nonwoven fabric 100 with different properties on both sides can be obtained.

[0044] As an optional embodiment, the hot pressing treatment includes hard pressing and soft pressing. Hard pressing: the two sides of the fiber layer 11 or the laminate are subjected to hard pressing treatment at different hard pressing temperatures, and the difference in hard pressing temperature between the two sides of the fiber layer 11 or the laminate is 30 to 60°C; Soft pressing: the fiber layer 11 is subjected to soft pressing treatment to obtain the nonwoven fabric 100. Before the soft pressing treatment, the temperature of the fiber layer 11 is maintained at 70 to 180°C. The interval between hard pressing and soft pressing is short, so that the fiber layer 11 or the laminate is maintained at a high temperature for soft pressing after hard pressing, and no preheating treatment is required, which saves energy.

[0045] As an optional embodiment, the diluted slurry also includes an additive. The mass fraction of the additive in the diluted slurry is 0.1‰ to 0.5‰. The additive may include a defoamer, a dispersant, etc. The additive is helpful to reduce bubbles in the diluted slurry, make the fiber dispersion more uniform, and improve the quality of the obtained fiber layer 11.

[0046] The embodiment of the present application also provides a membrane material, which includes any of the above nonwoven fabrics 100 or a nonwoven fabric prepared by any of the above preparation methods. The above nonwoven fabric 100 has two-sided anisotropy, and the prepared membrane material also has significant two-sided anisotropy. The second surface of the nonwoven fabric 100 has a greater roughness, better wetting performance and adsorption performance, and the second surface 102 can be used as a coating surface, and the casting liquid is coated on the second surface to obtain a semipermeable membrane; while the first surface 101 can be used as a non-coating surface due to its lower roughness, lower porosity and higher surface density, so that it has higher strength and better support. For example, when used as photovoltaic table paper, the first surface 101 of the nonwoven fabric 100 is relatively smooth and can better carry the battery cell, and the second surface 102 of the nonwoven fabric 100 is relatively rough, and the friction between the nonwoven fabric 100 and the table is relatively large, and it is not easy to slide and shift. Of course, it is understandable that although only two specific applications are mentioned here, ordinary technicians in this field can make further applications based on the two-sided anisotropy of non-woven fabrics and membrane materials, such as using the membrane material in the present application in the field of chemical batteries, as a diaphragm or a component of a diaphragm for lithium-ion batteries, etc.

[0047] The present application is further described below in conjunction with embodiments, but the protection scope of the present application is not limited to the embodiments.

[0048] 1. Preparation of fiber layer

[0049] Fiber layers P1 to P9 were prepared according to the raw materials and process parameters in Table 1 below.

[0050] Table 1: Raw materials and process parameters of fiber layers P1 to P9

[0051]

[0052]

[0053] 2. Preparation of nonwoven fabrics

[0054] The nonwoven fabrics in the examples and comparative examples were prepared according to the raw materials and process parameters in Table 2.

[0055] Table 2: Raw materials and process parameters of nonwoven fabrics in Examples 1-15 and Comparative Examples 1-4

[0056]

[0057] Note:

[0058] 1. The hot pressing process in the above embodiments and comparative examples adopts hard pressing treatment;

[0059] 2. In the stacking method, "rough / rough" specifically refers to Figure 7The first surface and the second surface of the laminated nonwoven fabric shown in the figure are both rough surfaces (or referred to as the second fiber surface with greater roughness in the fiber layer, the same below), and "light / light" specifically refers to Figure 8 The first surface and the second surface of the laminated nonwoven fabric shown in the figure are both smooth surfaces (or referred to as the first fiber surface with less roughness in the fiber layer, the same below), and "rough / smooth" specifically refers to Fig. 9 The laminated nonwoven fabric shown has a rough first surface and a glossy second surface.

[0060] 3. Performance test:

[0061] The above embodiments and comparative examples were subjected to performance tests.

[0062] 1. Air permeability: GB / T 5453-1997 “Determination of air permeability of textile fabrics”, test pressure difference 200Pa.

[0063] 2. Surface roughness: The surface roughness of the nonwoven fabric was tested by a KOSAKA LAB SE800C surface roughness tester, where the probe test force was 0.75 mN and the measuring length was 5 mm.

[0064] 3. Tensile strength: refer to GB / T 12914-2018 "Determination of tensile strength of paper and paperboard - Constant rate tensile method (20 mm / min)".

[0065] 4. Melting degree: The proportion of melted fibers in nonwoven fabrics is calculated by the area method. Ten samples are taken in parallel, with a minimum interval of 10 cm. The sample size is 2 cm*2 cm. Then, a random location of the independent sample is photographed under an electron microscope. Finally, the area of ​​melted fibers S in the electron microscope images of samples 1-10 is calculated using graphics processing software. 熔融 and electron microscope field of view area S 视野 Make measurements, calculate their geometric means and derive the corresponding proportions;

[0066] S 熔融程度 =[(S 熔融-1 / S 视野-1 )+(S 熔融-2 / S 视野-2 )+....+(S 熔融-10 / S 视野-10 )] / 10*100%;

[0067] Where S 熔融-1 Refers to the area of ​​the molten part in the electron microscope image of sample 1, S 视野-1 It refers to the field of view area of ​​the electron microscope image in sample 1, and the others refer to the corresponding melting part area and field of view area of ​​different samples.

[0068] 4. Performance test results:

[0069] The performance test results of the encapsulation films in the above embodiments and comparative examples are shown in Table 3.

[0070] Table 3: Test results of embodiments and comparative examples

[0071]

[0072]

[0073] As can be seen from Tables 1 to 3, the nonwoven fabrics in Examples 1 to 15 of the present application have good performance in terms of air permeability and tensile strength, and at the same time, the first surface and the second surface show significant differences in surface roughness, and can be well applied to fields that require nonwoven fabrics to have two-sided differences. The nonwoven fabrics in Comparative Examples 1 to 4 of the present application have a certain degree of decline or degradation in performance compared to the nonwoven fabrics in Examples 1 to 15, especially there is a problem that the two surfaces have similar roughness and are difficult to match different contact interfaces.

[0074] Comparing Comparative Examples 1 to 2 with Example 1, it can be seen that although all of them adopt the "rough / glossy" lamination method, the temperature difference on both sides during hot pressing is small, resulting in small differences between the two sides of the final nonwoven fabric. Even in Comparative Example 2, since the same temperature on both sides is used during hot pressing, the performance of the two surfaces of the final nonwoven fabric is basically the same and there is no difference.

[0075] Comparing Example 3 with Example 1, it can be seen that in Example 3, the temperature difference on both sides during hot pressing is large, and the melting degree on both sides of the nonwoven fabric is greatly different, which makes the first surface roughness of the nonwoven fabric too small and prone to slippage.

[0076] The difference in melting points between the main fiber and the molten fiber used in Comparative Example 4 is less than 50 degrees Celsius, which increases the difficulty of setting the temperature on both sides when preparing the fiber layer for drying and hot pressing. At the same time, it also significantly reduces the differences between the two sides of the fiber layer and the two sides of the final non-woven fabric and makes them tend to be the same, and basically no differences can be shown.

[0077] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the claims attached to this application.

Claims

1. A nonwoven fabric, It is characterized in that include: at least one fiber layer, the fiber layer comprising main fibers and molten fibers, the difference between the melting points of the main fibers and the molten fibers being greater than or equal to 50° C.; The two surfaces of the nonwoven fabric are respectively a first surface and a second surface, there are melting areas on the first surface and the second surface, and the difference between the ratio of the area of ​​the melting area in the first surface to the total area of ​​the first surface and the ratio of the area of ​​the melting area in the second surface to the total area of ​​the second surface is 20%-50%.

2. The nonwoven fabric according to claim 1, Features: The ratio of the area of ​​the molten region in the first surface to the total area of ​​the first surface is 85%-95%; the ratio of the area of ​​the molten region in the second surface to the total area of ​​the second surface is 45%-70%.

3. The nonwoven fabric according to claim 1, Features: The two surfaces of the fiber layer are respectively a first fiber surface and a second fiber surface, and the area of ​​the melting region in the first fiber surface is greater than the area of ​​the melting region in the second fiber surface.

4. The nonwoven fabric according to claim 3, Features: The nonwoven fabric comprises at least two fiber layers; Adjacent fiber layers are stacked in one of the following stacking modes: the first fiber surface of one fiber layer is close to the first fiber surface of another fiber layer, the second fiber surface of one fiber layer is close to the second fiber surface of another fiber layer, or the first fiber surface of one fiber layer is close to the second fiber surface of another fiber layer.

5. The nonwoven fabric according to claim 1, Features: The main fiber has a fineness of 0.5-3D and a length of 2-15mm; The molten fiber has a fineness of 0.5-3D and a length of 2-15 mm.

6. The nonwoven fabric according to claim 1, Features: The mass ratio of the main fiber to the molten fiber is (50-70):(30-50); Preferably, the main fiber includes at least one of polyester fiber, polyolefin fiber, polyamide fiber, aramid fiber or polyimide fiber, and the melting fiber includes at least one of polyester fiber, polyolefin fiber, polyamide fiber, aramid fiber or polyimide fiber.

7. A method for preparing the nonwoven fabric according to any one of claims 1 to 6, Features: The preparation method comprises: Pulping: mixing the main fiber and the molten fiber to prepare fiber slurry; Dilution: diluting the fiber slurry to obtain a diluted slurry; Cloth making: putting the diluted slurry on a net to make a paper sheet; Drying: drying the sheet to obtain the fiber layer; The temperature of the drying treatment is greater than or equal to the melting softening temperature of the molten fiber; Hot pressing: treating the fiber layer or the laminated body of the fiber layers at 150-240° C. by at least one of hard pressing and soft pressing to obtain the nonwoven fabric; During the heat pressing treatment, the difference in heat pressing temperature between the two surfaces of the fiber layer or the laminate is 30 to 70°C.

8. The nonwoven fabric according to claim 7, Features: During the drying, the difference in drying temperature between the two sides of the sheet is 30-60°C.

9. The nonwoven fabric according to claim 7, Features: In the hot pressing, The hard pressing includes performing a hard pressing treatment on the fiber layer or the laminate, and the difference in hard pressing temperature between the two sides of the fiber layer or the laminate is 30 to 70° C.; Soft pressing includes soft pressing the fiber layer or the laminate to obtain the nonwoven fabric; Before the soft pressing treatment, the temperature of the fiber layer is 70-180°C.

10. A membrane material, Features: The membrane material comprises the nonwoven fabric according to any one of claims 1 to 6 or the nonwoven fabric prepared by the preparation method according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Non-woven fabric for photovoltaic table paper and production method of non-woven fabric

    CN115305744A

  • Non-woven fabric for photovoltaic table paper and production method of non-woven fabric

    CN117166283A

  • Nonwoven fabric and its production

    JP1995026462A

  • Structure of mounting wiring for vehicle using a pillar bracket

    KR1020220055691A