Oxide semiconductor gas sensor array, preparation method, electronic nose and application
By growing precious metal-modified metal-organic frame nanosheets in situ on a ceramic substrate, combining ultrasonic treatment and insulating medium coverage, a high-stability oxide semiconductor gas sensor array was prepared, and a gas detection model was constructed through linear discriminant analysis and machine learning algorithms. , solves the problem of insufficient recognition and detection capabilities of traditional sensors in complex atmospheres, and realizes accurate identification and quantitative detection.
Patent Information
- Application Number
- CN202411285645.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-13
AI Technical Summary
Traditional semiconductor gas sensors have high working temperature and high power consumption, and the pattern recognition algorithm lacks the ability to analyze signal characteristics, so they cannot achieve accurate identification and quantitative detection of target gas in complex atmospheres.
Using the preparation method of oxide semiconductor gas sensor array, a high-stability sensor array is prepared by growing precious metal-modified metal-organic frame nanosheets on a ceramic substrate in situ, combined with ultrasonic treatment and insulating medium covering, and analyzed through linear discriminant analysis. and machine learning algorithms to build gas detection models.
It realizes accurate identification and quantitative detection of target gas in complex atmospheres, improves recognition accuracy and detection accuracy, reduces power consumption, and maintains the microstructure and device consistency of nanomaterials.
Smart Images

Figure CN119086658A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of smart sensor technology, and more specifically, to oxide semiconductor gas sensor arrays, preparation methods, electronic noses, and applications. Background Art
[0002] With the increasing demand for various harmful gas monitoring and air pollutant control, it is urgent to develop more efficient gas sensors to detect gases quickly and accurately. The electronic nose is an artificial olfactory system that simulates the biological olfactory system, based on a gas sensor array and combined with pattern recognition technology to achieve gas or odor recognition. It has a wide range of application needs in public safety, food industry, environmental monitoring and medical testing. However, traditional semiconductor gas sensors have high operating temperatures and high power consumption, and traditional pattern recognition algorithms are insufficient in their ability to analyze sensor signal characteristics, which restricts the accuracy of qualitative identification. Quantitative detection is still imperfect and cannot achieve accurate detection of target gases in complex atmospheres. Summary of the invention
[0003] In view of the defects of the prior art, the purpose of this application is to provide an oxide semiconductor gas sensor array, a preparation method, an electronic nose and applications to solve the problem of how to accurately identify and quantitatively detect the target gas in a complex atmosphere.
[0004] To achieve the above-mentioned purpose, the present application provides a method for preparing an oxide semiconductor gas sensor array, the preparation method comprising the following steps:
[0005] S1 preparing a mixed solution, wherein the mixed solution comprises 2-methylimidazole, a metal compound and deionized water;
[0006] S2: adding a noble metal source to the mixed solution so that the molar ratio of metal atoms to noble metal atoms in the mixed solution is a preset ratio; and then performing ultrasonic treatment to obtain a dispersed mixed solution;
[0007] S3 inserting a ceramic substrate into the dispersed mixed liquid and soaking and growing it at a preset ambient temperature, wherein the portion of the ceramic substrate where no material is grown is covered with an insulating medium; after soaking, taking out the ceramic substrate and removing the sediment on its surface to obtain a precursor of a metal organic framework nanosheet doped with a noble metal grown on the surface of the interdigitated test electrode;
[0008] S4: placing the precursor in an air atmosphere, heating it to a preset temperature at a preset heating rate, and calcining it, so that the precursor is converted into a metal oxide nanosheet modified with a noble metal;
[0009] S5 repeats steps S1-S4, and only the amount of the noble metal source added is adjusted during each repetition, while other conditions remain unchanged, thereby preparing metal oxide nanosheet sensor arrays modified with different amounts of noble metals.
[0010] Furthermore, the mixed solution contains 2-methylimidazole with a concentration of 2 mol / L to 10 mol / L and a metal compound aqueous solution with a concentration of 2 mol / L to 10 mol / L.
[0011] Furthermore, in step S2, the molar ratio of metal atoms to noble metal atoms in the mixed solution is 0-3.5%.
[0012] Further, the metal compound includes cobalt nitrate hexahydrate, nickel chloride hexahydrate, ferric chloride hexahydrate and vanadium chloride; preferably, the noble metal source includes potassium tetrachloropalladate, chloroauric acid hydrate, silver nitrate or ruthenium chloride.
[0013] Furthermore, in step S3, the ambient temperature is preset to be 25° C. to 30° C., and the immersion growth time is 3 hours to 5 hours.
[0014] Furthermore, in step S4, the preset heating rate is 5°C / min-10°C / min, the preset temperature is 350°C, and the calcination time is 2 hours-4 hours.
[0015] According to another aspect of the present invention, an oxide semiconductor gas sensor array is further disclosed. The oxide semiconductor gas sensor array is prepared by any of the above methods for preparing an oxide semiconductor gas sensor array.
[0016] According to another aspect of the present invention, an electronic nose is also disclosed, which includes multiple groups of oxide semiconductor gas sensor arrays as described above, and different amounts of precious metal sources are added during the preparation process of each group of oxide semiconductor gas sensor arrays to make the molar ratio of metal atoms and precious metal atoms in the corresponding mixed liquid different.
[0017] According to another aspect of the present invention, an application of the electronic nose as described above in gas detection is also disclosed, and the application method comprises the following steps:
[0018] S1 obtains resistance signal data of each oxide semiconductor gas sensor array in a target gas of preset concentration under preset humidity, and outputs a resistance curve;
[0019] S2 extracts the dynamic response characteristics of all resistance curves, and constructs a multidimensional feature matrix based on the dynamic response characteristics;
[0020] S3 performs dimensionality reduction processing and concentration quantification on the multidimensional feature matrix by a linear discriminant analysis method;
[0021] S4 performs power function fitting on the dimension reduction data in step S3 and the quantitative concentration to obtain a concentration detection model of the target gas by the gas sensor array;
[0022] S5 detects the gas concentration in the test environment using the concentration detection model, and then detects the type and concentration of the gas to be tested.
[0023] Further, in step S1, the preset humidity is 30%-70% relative humidity (RH); the preset concentration is 0.1ppm-20ppm; preferably, the preset humidity and the preset concentration respectively include multiple groups of different values; more preferably, the target gas includes at least two types.
[0024] The above technical solution conceived by this application has the following advantages compared with the prior art:
[0025] 1. The method for preparing an oxide semiconductor gas sensor array provided in the present application can maintain the microstructure of the nanomaterial well after calcination in an air atmosphere by in-situ growing sensitive materials on interdigitated electrodes, thereby ensuring a large number of adsorption sites and avoiding the problem of poor consistency of device surface materials caused by traditional film-forming methods such as drop coating and spin coating. At the same time, the gas-sensitive activity of cobalt oxide is regulated by changing the content of precious metals and a sensor array is constructed, and the recognition accuracy of the target gas is improved by combining the coordinated optimization of the feature extraction algorithm.
[0026] 2. In the process of preparing the oxide semiconductor gas sensor array, the mixed solution is ultrasonically treated to efficiently disperse the mixed liquid material; the part of the ceramic substrate where no material is grown is covered with an insulating medium, that is, the part of the interdigitated electrode is exposed, and the mixed solution is inserted to grow at 25°C-30°C for 3-5 hours, and the obtained device has stronger stability; after cleaning the deposits on the surface of the device, a metal organic framework nanosheet modified with precious metals grown on the surface of the device's interdigitated electrodes can be obtained.
[0027] 3. The electronic nose prepared in the present application comprises a plurality of groups of gas sensor arrays. The amount of precious metal doped in the preparation process of each group of gas sensor arrays is different, so that the surface activity of the gas sensors varies, which is conducive to constructing a sensor array that can respond to the unique gas sensitivity of gases through different sensors.
[0028] 4. The electronic nose disclosed in the present application is composed of multiple groups of different sensor arrays. At a specific working temperature, the resistance data of the sensor array at different humidity and different concentrations of target gas (formaldehyde, ethanol) are collected, the kinetic response characteristics are extracted, and a multi-dimensional feature matrix is constructed. The gas detection model is obtained by combining the machine learning algorithm. The gas detection model makes up for the gaps of poor selectivity and difficulty in quantification, and realizes accurate identification and quantitative detection of target gas in a wider humidity range. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the process of preparing a gas sensor array provided in the present application;
[0030] Figure 2 This is a schematic diagram of formaldehyde and ethanol concentration monitoring classification provided in Example 3 of the present application;
[0031] Figure 3 is a function fitting diagram of formaldehyde concentration and one-dimensional signal projection provided in Example 3 of the present application;
[0032] Figure 4 This is a schematic diagram of formaldehyde and ethanol concentration monitoring classification provided in Example 6 of the present application;
[0033] Figure 5 This is a function fitting diagram of formaldehyde concentration and one-dimensional signal projection provided in Example 6 of the present application. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0035] The present application provides a method for preparing an oxide semiconductor gas sensor array, such as Figure 1 As shown, the preparation method comprises the following steps:
[0036] S1: preparing a mixed solution comprising 2-methylimidazole, a metal compound (including but not limited to cobalt nitrate hexahydrate, nickel chloride hexahydrate, ferric chloride hexahydrate, vanadium chloride) and deionized water;
[0037] S2: adding a certain amount of noble metal source (including but not limited to potassium tetrachloropalladate, chloroauric acid hydrate, silver nitrate, and ruthenium chloride) into the mixed solution so that the molar ratio of noble metal atoms to metal atoms in the mixed solution is a preset ratio, and ultrasonically treating the mixed solution to which the noble metal source is added to obtain a dispersed mixed solution;
[0038] S3: Covering the part of the ceramic substrate where no material is grown, that is, exposing the interdigital electrode part, with an insulating medium, and then inserting the ceramic substrate into the dispersed mixed liquid, and soaking and growing it for a certain period of time at a preset ambient temperature, taking out the soaked ceramic substrate and removing the sediment on its surface, to obtain a precursor of a metal-organic framework nanosheet (MOF) modified with a noble metal grown on the surface of the interdigital test electrode;
[0039] S4: placing the precursor in an air atmosphere, and heating it to a preset calcination temperature at a certain heating rate for a period of time to convert the precursor into a metal oxide nanosheet modified with a noble metal;
[0040] S5 repeats steps S1-S4, and in the repetitive process, by adjusting the amount of the noble metal source added in step S2, a sensor array of metal oxide nanosheets modified with different amounts of noble metals is prepared.
[0041] In a preferred embodiment, the mixed solution contains 2mol / L to 10mol / L 2-methylimidazole and 2mol / L to 10mol / L aqueous solution of a metal compound, such as 2mol / L, 3mol / L, 4mol / L, 5mol / L, 6mol / L, 7mol / L, 8mol / L, 9mol / L, and 10mol / L 2-methylimidazole and 2mol / L, 3mol / L, 4mol / L, 5mol / L, 6mol / L, 7mol / L, 8mol / L, 9mol / L, and 10mol / L aqueous solution of a metal compound. The specific ratio will be selected and combined arbitrarily within the above range according to actual needs. However, if the concentration exceeds 2mol / L to 10mol / L, the sensitivity and accuracy of the sensor array of metal oxide nanosheets modified with different amounts of precious metals will be reduced.
[0042] In a preferred embodiment, in step S2, the molar ratio of noble metal atoms to metal atoms in the mixed solution is preferably 0%-3.5%, such as 0.5%, 1.5%, 2%, 3.5%, etc.
[0043] In a preferred embodiment, in step S2, the ultrasonic treatment time is 5-15 minutes, such as 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, etc.
[0044] In a preferred embodiment, in step S3, the preset ambient temperature is 25°C to 30°C, such as 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, etc.; the immersion growth time is preferably 3 hours to 5 hours, such as 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, etc.
[0045] In a preferred embodiment, in step S4, the high-temperature calcination temperature is preferably 350°C; the heating rate during high-temperature calcination is preferably 5°C / min-10°C / min, such as 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min. The temperature is gradually increased uniformly; the high-temperature calcination time is preferably 2 hours to 4 hours, such as 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, etc.
[0046] In all the above embodiments, when steps S1-S4 are repeated to prepare metal oxide nanosheet sensor arrays modified with different amounts of noble metals, other conditions remain unchanged except for adjusting the amount of the noble metal source.
[0047] According to another aspect of the present application, an oxide semiconductor gas sensor array is also provided, and the gas sensor array is prepared by any of the previous oxide semiconductor gas sensor preparation methods.
[0048] According to another aspect of the present application, an electronic nose is also provided, which includes multiple groups of gas sensor arrays as described above, and different amounts of precious metal sources are added during the preparation process of each group of gas sensor arrays to make the molar ratio of metal atoms and precious metal atoms in the mixed solution different, while other conditions remain unchanged.
[0049] According to another aspect of the present application, there is also provided an application of an electronic nose as described in any one of the above items in gas detection, wherein the gas detection method comprises the following steps:
[0050] S1 obtains resistance signal data of each oxide semiconductor gas sensor array in a target gas of a specific concentration under specific humidity conditions, and outputs a resistance curve;
[0051] S2 extracts the dynamic response characteristics of all resistance curves and constructs a multi-dimensional feature matrix based on the dynamic response characteristics;
[0052] S3 uses linear discriminant analysis to reduce the dimension of the multidimensional feature matrix and quantify the concentration;
[0053] S4 performs power function fitting on the dimension reduction data in step S3 and the quantitative concentration to obtain a concentration detection model of the target gas by the gas sensor array;
[0054] S5 detects the gas concentration in the test environment using a concentration detection model, and then detects the type and concentration of the gas to be tested.
[0055] In a preferred embodiment, the specific humidity is 30%-70% RH (Relative Humidity), such as 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc.; the specific concentration is preferably 0.1ppm-20ppm, such as 0.1ppm, 0.2ppm, 0.4ppm, 0.7ppm, 0.9ppm, 1ppm, 2ppm, 3ppm, 4ppm, 5ppm, 6ppm, 7ppm, 8ppm, 9ppm, 10ppm, 11ppm, 12ppm, 13ppm, 14ppm, 15ppm, 16ppm, 17ppm, 18ppm, 19ppm, 20ppm, etc.; more preferably, the specific humidity and the specific concentration are divided into multiple groups of different values, that is, the same specific humidity corresponds to different specific concentrations, and the same specific concentration corresponds to different specific humidity; more preferably, the target gas in step S1 includes at least two types, and in other embodiments, it may also include three, four, five, etc.
[0056] In order to illustrate the present application, the aforementioned method provided by the present application is described in detail below in combination with examples, but the following examples cannot be understood as limiting the scope of protection of the present application.
[0057] Example 1
[0058] like Figure 1 FIG. 1 is a flow chart of a method for preparing an oxide semiconductor gas sensor array provided in this embodiment. The method for preparing an oxide semiconductor gas sensor array includes the following steps:
[0059] S1. Prepare a mixed solution comprising 2-methylimidazole, cobalt nitrate hexahydrate and deionized water; the mixed solution comprises 50 ml of deionized water, 50 mL of 2-methylimidazole with a molar concentration of 4 mol / L and 50 mL of cobalt nitrate hexahydrate with a molar concentration of 4 mol / L, that is, a mixed solution of 16.42 g of 2-methylimidazole and 72.76 g of cobalt nitrate hexahydrate and 50 mL of deionized water.
[0060] S2. According to the preset atomic molar ratio of palladium and cobalt in the mixed solution, a corresponding amount of potassium tetrachloropalladate is added to the mixed solution, and ultrasonic treatment is performed for 10 minutes to fully disperse the mixed solution; the preset atomic molar ratio of palladium and cobalt in the mixed solution is 0%-3.5%, and the atomic molar ratio of palladium and cobalt is preferably any value of 0%, 0.5%, 1.5%, 2.5% or 3.5%.
[0061] S3, covering the part of the ceramic substrate where no material is grown, that is, exposing the interdigital electrode part of the ceramic substrate, with an insulating medium, and then inserting the ceramic substrate into the dispersed mixed liquid, and soaking and growing for 3 hours to 5 hours at an ambient temperature of 25°C to 30°C; after the soaking, taking out the ceramic substrate and removing the sediment on its surface, to obtain a precursor of Co-MOF nanosheets modified with blue Pd grown on the surface of the interdigital test electrode;
[0062] S4, placing the precursor in an air atmosphere, heating it to 350°C at a heating rate of 5°C / min-10°C / min and calcining it for 2-4 hours, so that the precursor is converted into PdO-modified Co3O4 nanosheets. The Co3O4 gas sensor prepared in this way can better maintain the microstructure of the nanomaterial, and has higher recognition accuracy and device stability.
[0063] Example 2
[0064] Five gas sensor arrays were prepared using the method disclosed in Example 1. The specific preparation method is as follows:
[0065] Take five mixed solutions, each of which contains an equal amount of a mixed solution of 16.42g (4mol / L, 50mL) 2-methylimidazole, 72.76g (4mol / L, 50mL) cobalt nitrate hexahydrate and 50mL deionized water, and at the same time, according to the atomic molar ratio of palladium to cobalt in the mixed solution being 0%, 0.5%, 1.5%, 2.5% and 3.5%, potassium tetrachloropalladate is added to the five mixed solutions in a corresponding amount; then all the five mixed solutions are subjected to ultrasonic treatment for 10 minutes to fully disperse the materials in each mixed solution, so as to obtain five mixed solutions in which the atomic molar ratio of palladium to cobalt is 0%, 0.5%, 1.5%, 2.5% and 3.5%, respectively.
[0066] A gas-sensitive material is grown in situ on a ceramic chip device. The ceramic chip device is 26 mm long and 2 mm wide. The front of the device is a gold-based interdigital and test electrode, and the back is a platinum-based heating electrode. The portion of the ceramic substrate (i.e., the ceramic chip device) where no material is grown is covered with tape, that is, the interdigital electrode portion is exposed. Then, 5 ceramic chip devices treated in the same manner are respectively inserted into the five solutions after the aforementioned ultrasonic treatment, and grown at a room temperature of 25°C to 30°C for 3 to 5 hours. In this embodiment, it is preferred that the growth be 4 hours to achieve the best growth effect. Too low a temperature or too short a growth time is not conducive to obtaining a precursor with the best performance.
[0067] After the immersion was completed, all the devices were taken out, and the ceramic wafer devices were rinsed with deionized water to remove surface deposits, obtaining 5 blue Pd-modified Co-MOF nanosheet precursors grown on the surface of the interdigitated electrode part of the ceramic wafer device.
[0068] The obtained Pd-modified Co-MOF nanosheet precursor was placed in an air atmosphere and heated to 350°C at a heating rate of 5°C / min-10°C / min for calcination for 2-4 hours to convert the precursor into PdO-modified Co3O4 nanosheets, thereby obtaining 5 Co3O4 nanosheets with different properties.
[0069] In other embodiments, the content of potassium tetrachloropalladate may be adjusted to make the molar ratio of palladium atoms to cobalt atoms in the prepared mixed solution different from the molar ratio of palladium atoms to cobalt atoms in the above five mixed solutions, thereby preparing other gas sensor arrays with different performances.
[0070] Example 3
[0071] The electronic nose is formed by using the five Co3O4 nanosheets with different characteristics prepared in Example 2 to detect gas. Specifically, the five Co3O4 nanosheets with different characteristics form a gas sensor array. The electronic nose in this embodiment includes five groups of oxide semiconductor gas sensor arrays. The steps of using the electronic nose for detection include:
[0072] S1. Provide 25 groups of formaldehyde and 25 groups of ethanol as gases to be detected, respectively. The formaldehyde to be detected and the ethanol to be detected respectively include 5 groups of gases with different humidity conditions, and the humidity of each group of gases is 30% RH, 40% RH, 50% RH, 60% RH and 70% RH, respectively. Each group of gases with the same humidity has 5 groups of different gas concentrations, and the gas concentrations are set to 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm respectively; specifically, the gas under 30% RH includes 5 groups, and the concentration of each group of gases is 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm, respectively; the gas under 40% RH includes 5 groups , the concentration of each gas group is 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm respectively; the gas under 50%RH contains 5 groups, and the concentration of each gas group is 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm respectively; the gas under 60%RH contains 5 groups, and the concentration of each gas group is 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm respectively; the gas under 70%RH contains 5 groups, and the concentration of each gas group is 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm respectively. The above humidity conditions and gas concentrations are cross-combined to form a total of 25 test environments;
[0073] The Co3O4 gas sensor arrays prepared above were placed in 25 formaldehyde environments and 25 ethanol environments respectively. The resistance signal data of each Co3O4 gas sensor array in the 25 environments corresponding to formaldehyde and ethanol were obtained through the acquisition circuit and the host computer system, and the corresponding resistance curve was output. The specific process of how to perform acquisition through the acquisition circuit and the host computer system is well known to those skilled in the art and will not be repeated here.
[0074] S2. Using programming software Python to extract the kinetic response characteristics of the 50 groups of resistance curves collected in step S1, each Co3O4 gas sensor takes three characteristics of sensitivity, integrated area, and response time, and constructs a multidimensional feature matrix based on these kinetic response characteristics;
[0075] S3, using linear discriminant analysis method to reduce the dimension of multidimensional feature matrix and quantify the concentration;
[0076] S4, performing power function fitting on the dimension reduction data in step S3 and the quantitative concentration to obtain a concentration detection model of the Co3O4 gas sensor array for the target gas;
[0077] S5. Use the concentration detection model to detect the gas concentration in the test environment, and then provide the type and concentration of the gas to be tested.
[0078] The specific steps of constructing a multidimensional feature matrix and obtaining a concentration detection model in steps S2-S4 are:
[0079] (1) A total of 15 features of the five gas sensor arrays are spliced in the horizontal direction to form a 1*15 row vector, and then the row vectors of the five concentrations of the two gas samples measured at five humidity levels are spliced in the vertical direction to construct a multidimensional feature matrix of size 50*15.
[0080] (2) The multidimensional feature matrix is reduced in dimension by linear discriminant analysis. The specific dimension reduction process is as follows: At this time, the five concentration values of the two gases are used as the dimension reduction target, so the target classification number C = 10. After extracting the three dynamic characteristics of each gas sensor array, each gas detection sample has a 15-dimensional feature vector. Therefore, it is necessary to select a basis vector of the same size of 15 dimensions (K = 15) for projection. The basic form of the basis vector is:
[0081] W=[w1|w2|…|w15] (1)
[0082] Among them, W is the basis vector set, w1 is the first basis vector;
[0083] By projection:
[0084] y=W Tx (2)
[0085] Among them, x is the feature matrix set of all samples;
[0086] The result of projecting the sample point on the K-dimensional vector is expressed as:
[0087] [y1,y2,...,y15] (3)
[0088] The degree of hashing of sample points in each class relative to the center point in the class is expressed as:
[0089]
[0090]
[0091] Among them, S w is the sum of the hashing degrees of all sample points in each class relative to the center point in the class, μ i is the mean size of the i-th category sample, and c is the total number of sample categories.
[0092] The degree of hashing of the sample mean point of each class relative to the center point of all samples is expressed as:
[0093]
[0094] Among them, S B is the sum of the hashing degrees of the mean points of various samples relative to the center points of all samples, N i is the number of samples in the i-th category, ω i represents the i-th class sample;
[0095] After projection, the mean value of the sample point of the i-th category after projection on a certain basis vector is:
[0096]
[0097] Comprehensive projection vector and And update:
[0098]
[0099] Where W is the basis vector matrix, is the sum (variance) of the hash matrices within each class after projection, It is the sum (mean) of the hash matrices of the projections of the centers of each class relative to the center of the entire sample. The central idea of linear discriminant analysis is to maximize the distance between classes and minimize the distance within a class. The distance after the projection of the class mean is used as a way to measure the degree of separation between classes.
[0100] Therefore, in order to minimize the sum of the hash matrices within a class and maximize the sum of the hash matrices between classes, define:
[0101]
[0102] Among them, J(w) is the ratio of the defined between-class hash matrix sum and the within-class hash matrix sum.
[0103] Since the numerator and denominator of the above formula are both hash matrices, we take their determinant to convert the matrix into a real number. And because the value of the determinant is actually the product of the matrix eigenvalues, and an eigenvalue can represent the degree of divergence on the eigenvector, we use the determinant to calculate.
[0104] Taking the derivative of J(w), we get:
[0105] S B w i =λS w w i (11)
[0106] This formula is equivalent to:
[0107]
[0108] Among them, λ is a matrix Finally, it comes down to finding the matrix The eigenvalues of the first two largest eigenvalues are taken, and the eigenvectors w1 and w2 corresponding to the first two largest eigenvalues are taken, and the projection formula y = W T The x obtained is the projection direction 1 and the projection direction 2. There is a certain change relationship between the projection direction 1 or the projection direction 2 and the concentration of the gas. These change relationships become the basis for fitting the dimensionality reduction signal and the concentration. The projection vector with the same change trend as the concentration of each type of gas is extracted and defined as the one-dimensional output signal of the electronic nose. The one-dimensional output signal and the concentration are fitted with a power function using the Origin software. The fitted power function form is:
[0109] y=a*x b (13)
[0110] x is the gas concentration, y is the one-dimensional signal after dimensionality reduction, and a and b are function coefficients.
[0111] Thus, a concentration detection model that can be used for target gas concentration detection in actual environments is obtained. The concentration detection model can first identify the gas type through a linear discriminant analysis algorithm, that is, the one-dimensional data after dimensionality reduction is brought into the fitted power function, and the concentration of the corresponding gas can be detected.
[0112] In other embodiments, more types of gas sensor arrays may be used in combination with machine learning algorithms for gas detection, so as to obtain a more accurate gas detection model through a larger amount of sample data.
[0113] Figure 2 : is a schematic diagram of formaldehyde and ethanol concentration monitoring classification provided in this embodiment. After constructing a differentiated sensor array, formaldehyde and ethanol of different concentrations are detected, and feature extraction is performed on the detected data. The extracted features are normalized and displayed in the form of a heat map. The constructed multi-dimensional feature matrix is reduced to projection direction 1 and projection direction 2 by a linear discriminant analysis method, such as Figure 2 As shown in the figure, when the number of target categories is 2, linear discriminant analysis can only reduce the target matrix to one-dimensional space. The numbers in the figure represent the specific values after reducing to one-dimensional space. When the number of target categories is greater than 2, it can be reduced to two-dimensional space. The numbers in the figure represent the specific values of projection direction 1 and projection direction 2 after reducing to two-dimensional space.
[0114] Figure 3 is a function fitting diagram of formaldehyde concentration and one-dimensional signal projection provided in this embodiment, wherein the projection direction showing a certain relationship with the concentration is defined as a one-dimensional output signal, which can be used for quantitative analysis of gas concentration. Since there is a certain relationship between the projection direction 1 after dimensionality reduction and the gas concentration, the projection direction 1 is selected as the one-dimensional output signal in this embodiment, and R is obtained. 2 Around 0.9 (respectively 0.902, 0.928, 0.940, 0.924, 0.895), close to 1, the function fitting relationship with an error accuracy within 5% can be obtained by (true value - fitting value) / range, where R 2 Refers to the degree of fit of the regression line to the observed value. The gray triangles in the figure represent the different depths of the fitted lines. 2 Therefore, some of the output images overlap with each other.
[0115] Example 4
[0116] A schematic diagram of a process for preparing an oxide semiconductor gas sensor array provided in this embodiment, the preparation method comprises the following steps:
[0117] S1. Prepare a mixed solution comprising 2-methylimidazole, nickel chloride hexahydrate and deionized water; the mixed solution comprises 50 ml of deionized water, 50 mL of 2-methylimidazole with a molar concentration of 4 mol / L and 50 mL of nickel chloride hexahydrate with a molar concentration of 4 mol / L, i.e., a mixed solution of 16.42 g of 2-methylimidazole and 47.6 g of nickel chloride hexahydrate and 50 mL of deionized water.
[0118] S2. According to the preset atomic molar ratio of ruthenium to nickel in the mixed solution, a corresponding amount of ruthenium chloride is added to the mixed solution, and ultrasonic treatment is performed for 10 minutes to fully disperse the mixed solution; the preset atomic molar ratio of ruthenium to nickel in the mixed solution is 0%-3.5%, and the atomic molar ratio of ruthenium to nickel is preferably any value of 0%, 0.5%, 1.5%, 2.5% or 3.5%.
[0119] S3, covering the part of the ceramic substrate where no material is grown, that is, exposing the interdigital electrode part, with an insulating medium, and then inserting it into the dispersed mixed liquid, and soaking and growing for 3 hours to 5 hours at an ambient temperature of 25°C to 30°C; after the soaking, taking out the ceramic substrate and removing the sediment on its surface, to obtain a precursor of Ru-doped Ni-MOF nanosheets grown on the surface of the interdigital test electrode;
[0120] S4, placing the precursor in an air atmosphere, heating it to 350°C at a heating rate of 5°C / min-10°C / min for 2-4 hours, so that the precursor is converted into Ru-doped NiO nanosheets. The NiO gas sensor prepared in this way can better maintain the microstructure of the nanomaterial, and has higher recognition accuracy and device stability.
[0121] Example 5
[0122] Five gas sensor arrays were prepared using the method disclosed in Example 4. The specific preparation method is as follows:
[0123] Take five equal mixed solutions containing 16.42g (4mol / L, 50mL) of 2-methylimidazole, 47.6g (4mol / L, 50mL) of nickel chloride hexahydrate and 50mL of deionized water, and add corresponding amounts of ruthenium chloride to the five mixed solutions according to the atomic molar ratios of ruthenium and nickel of the mixed solutions being 0%, 0.5%, 1.5%, 2.5% and 3.5%, respectively. All of them are ultrasonically treated for 10 minutes to fully disperse the materials in each mixed solution, thereby obtaining five mixed solutions with atomic molar ratios of ruthenium and nickel being 0%, 0.5%, 1.5%, 2.5% and 3.5%, respectively.
[0124] The gas-sensitive material is grown in situ on a ceramic wafer device. The device is 26 mm long and 2 mm wide. The front of the device is a fork finger and a test electrode based on a gold material, and the back is a heating electrode based on a platinum material. The part of the ceramic substrate where the material is not grown is covered with tape, that is, the fork finger electrode part is exposed, and it is inserted into the five solutions after the aforementioned ultrasonic treatment, and grown for 3 to 5 hours at room temperature of 25°C to 30°C. In this embodiment, it is preferred to grow for 4 hours to achieve the best growth effect. Too low a temperature or too short a growth time is not conducive to obtaining the best performance precursor. After that, all the devices after immersion are taken out, and the device is rinsed with deionized water to remove surface deposits, and five Ni-MOF nanosheets doped with different concentrations of Ru are grown on the surface of the fork finger electrode part of the device. The precursor of the Ru-doped Ni-MOF nanosheet obtained is placed in an air atmosphere, and the temperature is raised to 350°C at a heating rate of 5°C / min-10°C / min and calcined for 2-4 hours to convert the precursor into Ru-doped NiO nanosheets, thereby obtaining five NiO nanosheets with different characteristics. The content of ruthenium chloride can also be adjusted to prepare a mixed solution with a ruthenium and nickel atomic molar ratio different from the above five ratios, thereby preparing other gas sensor arrays with different performances.
[0125] In other preferred embodiments, the above preparation method is the same, the only difference is that the metal compound is any one of cobalt nitrate hexahydrate, nickel chloride hexahydrate, ferric chloride hexahydrate or vanadium chloride, and the precious metal source is any one of potassium tetrachloropalladate, chloroauric acid hydrate, silver nitrate and ruthenium chloride. In more preferred embodiments, other applicable metal compounds and precious metal sources other than the metal compounds and precious metal sources listed above can also be selected.
[0126] Example 6
[0127] Using the preparation method of Example 5, a gas sensor array comprising five different characteristics is prepared to form an electronic nose for gas detection. The detection steps include:
[0128] S1 is carried out according to the combination method in step S1 of Example 3, with humidity conditions of 30% RH, 40% RH, 50% RH, 60% RH and 70% RH, and gas concentrations of 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm, to provide 25 different combinations of formaldehyde and ethanol with different humidity and concentrations. Then, each NiO gas sensor array is placed in 25 groups of formaldehyde to be tested and 25 groups of ethanol to be tested, and then the resistance signal data of each NiO gas sensor array in 25 environments is obtained through the acquisition circuit and the host computer system, and the corresponding resistance curve is output; each NiO gas sensor array is placed in humidity conditions of 30% RH, 40% RH, 50% RH, 60% RH and 70% RH, and each humidity condition corresponds to 5 groups of ethanol with gas concentrations of 0.1ppm, 1ppm, 5ppm, 10ppm and 20ppm, respectively, and the resistance signal data of each NiO gas sensor array in 25 formaldehyde environments and 25 ethanol environments is obtained through the acquisition circuit and the host computer system, and the corresponding resistance curve is output;
[0129] S2 uses programming software Python or other software that can achieve the same function to extract the kinetic response characteristics of all resistance curves collected in step S1, and each NiO gas sensor array takes three characteristics of sensitivity, integrated area, and response time, and constructs a multidimensional feature matrix based on these kinetic response characteristics;
[0130] S3 uses linear discriminant analysis to reduce the dimension of the multidimensional feature matrix and quantify the concentration;
[0131] S4 performs power function fitting on the dimension reduction data in step S8 and the quantitative concentration to obtain a concentration detection model of the NiO gas sensor array for the target gas;
[0132] S5 detects the gas concentration in the test environment using a concentration detection model, and then gives the type and concentration of the gas to be tested.
[0133] The specific steps of constructing a multidimensional feature matrix and obtaining a concentration detection model in steps S2-S4 of this embodiment are the same as the method of constructing a multidimensional feature matrix and obtaining a concentration detection model in Example 3, and will not be repeated here.
[0134] Figure 4 This is a schematic diagram of formaldehyde and ethanol concentration monitoring classification provided in this embodiment. After constructing a differentiated sensor array, formaldehyde and ethanol of different concentrations are detected, and feature extraction is performed on the detected data. The extracted features are normalized and displayed in the form of a heat map. The constructed multi-dimensional feature matrix is reduced to projection direction 1 and projection direction 2 by a linear discriminant analysis method. Figure 4As shown in the figure, when the number of target categories is 2, linear discriminant analysis can only reduce the target matrix to one-dimensional space. The numbers after the two projection directions 1 in the figure represent the specific values after being reduced to one-dimensional space. When the number of target categories is greater than 2, it can be reduced to two-dimensional space. The numbers after projection direction 1 and projection direction 2 in the figure represent the specific values of projection direction 1 and projection direction 2 after being reduced to two-dimensional space.
[0135] Figure 5 is a function fitting diagram of formaldehyde concentration and one-dimensional signal projection provided in this embodiment, wherein the projection direction showing a certain relationship with the concentration is defined as a one-dimensional output signal, which can be used for quantitative analysis of gas concentration. Since there is a certain relationship between the projection direction 1 after dimensionality reduction and the gas concentration, the projection direction 1 is selected as the one-dimensional output signal in this embodiment, and R is obtained. 2 All of them are around 0.9 (respectively 0.90, 0.91, 0.90, 0.89, and 0.90), all close to 1. By (true value - fitting value) / range, the function fitting relationship with an error accuracy within 5% can be obtained, where R 2 Refers to the degree of fit of the regression line to the observed value. The gray marks in the figure represent different depths of different fitting lines due to R 2 Therefore, the labels in the output graphics partially overlap with each other.
[0136] This application prepares an oxide semiconductor gas sensor array by changing the content of precious metals to regulate the gas-sensitive activity of metal oxides. The in-situ growth of sensitive materials on the interdigitated electrodes well maintains the microstructure of the nanomaterials, ensuring a large number of adsorption sites and the consistency of subsequent film-forming devices. In terms of application, by constructing an electronic nose composed of differentiated sensors, extracting feature sets from the output response curve data of the sensor array for different gases and performing dimensionality reduction processing, combined with machine learning algorithms to improve gas recognition accuracy and detection precision.
[0137] This application improves accurate gas identification and concentration detection by preparing sensor arrays, regulating signal feature engineering, and combining machine learning algorithms, and has the characteristics of high sensitivity, high specificity, and excellent long-term stability.
[0138] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing an oxide semiconductor gas sensor array, characterized in that: The preparation method comprises the following steps: S1 preparing a mixed solution, wherein the mixed solution comprises 2-methylimidazole, a metal compound and deionized water; S2: adding a noble metal source to the mixed solution so that the molar ratio of metal atoms to noble metal atoms in the mixed solution is a preset ratio; and then performing ultrasonic treatment to obtain a dispersed mixed solution; S3 inserting a ceramic substrate into the dispersed mixed liquid and soaking and growing it at a preset ambient temperature, wherein the portion of the ceramic substrate where no material is grown is covered with an insulating medium; after soaking, taking out the ceramic substrate and removing the sediment on its surface to obtain a precursor of a metal organic framework nanosheet doped with a noble metal grown on the surface of the interdigitated test electrode; S4: placing the precursor in an air atmosphere, heating it to a preset temperature at a preset heating rate, and calcining it, so that the precursor is converted into a metal oxide nanosheet modified with a noble metal; S5 repeats steps S1-S4, and only the amount of the noble metal source added is adjusted during each repetition, while other conditions remain unchanged, thereby preparing metal oxide nanosheet sensor arrays modified with different amounts of noble metals.
2. The method for preparing an oxide semiconductor gas sensor array according to claim 1, characterized in that: The mixed solution contains 2-methylimidazole with a concentration of 2 mol / L to 10 mol / L and a metal compound aqueous solution with a concentration of 2 mol / L to 10 mol / L.
3. The method for preparing an oxide semiconductor gas sensor array according to claim 1, characterized in that: In step S2, the molar ratio of metal atoms to noble metal atoms in the mixed solution is 0-3.5%.
4. The method for preparing an oxide semiconductor gas sensor array according to claim 1, wherein the metal compound comprises cobalt nitrate hexahydrate, nickel chloride hexahydrate, ferric chloride hexahydrate and vanadium chloride; preferably, the noble metal source comprises potassium tetrachloropalladate, chloroauric acid hydrate, silver nitrate and ruthenium chloride.
5. The method for preparing an oxide semiconductor gas sensor array according to claim 1, characterized in that: In step S3, the preset ambient temperature is 25° C. to 30° C., and the immersion growth time is 3 hours to 5 hours.
6. The method for preparing an oxide semiconductor gas sensor array according to claim 1, characterized in that: In step S4, the preset heating rate is 5°C / min-10°C / min, the preset temperature is 350°C, and the calcination time is 2 hours-4 hours.
7. An oxide semiconductor gas sensor array, characterized in that: The oxide semiconductor gas sensor array is prepared by the method for preparing an oxide semiconductor gas sensor array according to any one of claims 1 to 6.
8. An electronic nose, characterized in that: The electronic nose comprises a plurality of groups of oxide semiconductor gas sensor arrays as described in claim 7, and different amounts of precious metal sources are added during the preparation of each group of the oxide semiconductor gas sensor arrays, so that the molar ratio of metal atoms to precious metal atoms in the corresponding mixed solution is different.
9. An application of the electronic nose as claimed in claim 8 in gas detection, characterized in that: The application method includes the following steps: S1 obtains resistance signal data of each oxide semiconductor gas sensor array in a target gas of preset concentration under preset humidity, and outputs a resistance curve; S2 extracts the dynamic response characteristics of all resistance curves, and constructs a multidimensional feature matrix based on the dynamic response characteristics; S3 performs dimensionality reduction processing and concentration quantification on the multidimensional feature matrix by a linear discriminant analysis method; S4 performs power function fitting on the dimension reduction data in step S3 and the quantitative concentration to obtain a concentration detection model of the target gas by the gas sensor array; S5 detects the gas concentration in the test environment using the concentration detection model, and then detects the type and concentration of the gas to be tested.
10. The use of the electronic nose in gas detection as claimed in claim 9, characterized in that: In step S1, the preset humidity is 30%-70% relative humidity (RH); the preset concentration is 0.1ppm-20ppm; preferably, the preset humidity and the preset concentration respectively include multiple groups of different values; more preferably, the target gas includes at least two types.
Citation Information
Patent Citations
Transition metal oxide surface heteroepitaxial metal organic framework shell layer and preparation method and application thereof
CN105588860A
Gas-sensitive material for detecting low-concentration formaldehyde at room temperature and preparation method of gas-sensitive material and gas sensor
CN107290389A
High-sensitivity ammonia gas sensor and preparation method thereof
CN110849955A
High-activity noble metal modified cobalt oxide nano array electrocatalyst and preparation method thereof
CN118186485A
Sensor devices comprising a metal-organic framework material and methods of making and using the same
US20180011010A1
Cited By
Gas sensor electronic nose based on ferroelectric semiconductor, preparation method and application
CN122238436A