Evaluation method of pore diameter preservation effect of nano-pore membrane and pore diameter preservation method of nano-pore membrane

Through the current-voltage curve test and pore size preservation method, the problem of the difficulty in maintaining the stability of the pore size of the solid-state nanopore membrane is solved, and simple and accurate pore size preservation effect evaluation is achieved and storage stability is improved, reducing costs.

CN119086690AActive Publication Date: 2024-12-06GUANGZHOU INSIGHT TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411280526.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-06
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

In actual applications, the pore size of solid-state nanopore membranes is difficult to maintain a long-term stability, and the existing pore size measurement methods are costly and cumbersome, which limits their application and promotion.

Method used

The current-voltage curve test method is used to calculate the pore size storage effect by comparing the current and voltage after initial and storage, and the pore size storage effect is calculated using dimensionless number ΔD, and the pore size storage is carried out in combination with the method of contacting the nanopore membrane with neutral liquid, organic solvent or inert gas.

Benefits of technology

A simple and accurate method for evaluating pore size storage effect is provided, which improves the storage stability of the nanopore membrane, is simple to operate and low cost, and can effectively maintain the pore size of the nanopore membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086690A_ABST
    Figure CN119086690A_ABST
Patent Text Reader

Abstract

The invention relates to an evaluation method for the pore diameter preservation effect of a nanopore membrane and a pore diameter preservation method of the nanopore membrane, and the evaluation method comprises the following steps: (1) carrying out a current-voltage curve test on the nanopore membrane without pore diameter preservation, and obtaining the initial current and initial voltage of the nanopore membrane; (2) carrying out aperture preservation on the nano-pore film, and then carrying out current-voltage curve test on the nano-pore film subjected to aperture preservation, so as to obtain the stored current and the stored voltage of the nano-pore film; and (3) the preservation effect is calculated through an evaluation formula, and the smaller the delta D is, the smaller the aperture change is, and the better the preservation effect is. The evaluation method is convenient to operate, high in accuracy and suitable for verification of the preservation effect of the nanopore membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano material preparation, and in particular to a method for evaluating the pore size preservation effect of a nanoporous membrane and a method for preserving the pore size of a nanoporous membrane. Background Art

[0002] Nanoporous membrane is a thin film material with nanoscale pores, which is widely used in medical diagnosis, biological research, drug development and other fields. In recent years, it has also shown great application prospects in agriculture and environmental monitoring. Currently, nanopores are divided into two categories: protein pores embedded in biological membranes and solid pores made on insulating films.

[0003] With the rise of the third-generation sequencing technology, sequencing equipment based on protein pores has been successfully commercialized by a foreign company. The research on this technology has a far-reaching impact on the development of biomolecular sensors and detection. However, compared with protein pores, solid-state pores have the advantages of low cost, high stability, and easy integration, so they have become the recognized next-generation technology in the field of nanopore gene sequencing. The current solid-state nanopore gene sequencing technology is to make nanoscale pores by punching holes on solid-state thin films such as silicon nitride membrane chips, and pass the DNA chain through the solid-state nanopore under the action of voltage to obtain the DNA base sequence.

[0004] In the actual solid-state pore preparation process, due to the extremely small scale of the nanopore, extremely high manufacturing precision is often required. Then, during the preparation process, active functional groups are usually introduced on the surface of the nanopore, affecting the stability of the pore size. The above factors make it difficult for the pore size of solid-state nanopores to remain stable for a long time in practical applications, limiting their further application and promotion. In addition, the commonly used nanopore pore size measurement methods are mainly transmission electron microscopy (TEM) measurement and atomic force microscopy (AFM) measurement. These two pore size measurement methods are not only expensive, but also cumbersome steps, and it takes a long time to obtain an accurate pore size. Therefore, there is an urgent need to develop a method that can effectively preserve nanopore membranes and simply evaluate the preservation effect, so as to optimize the nanopore membrane preservation process and improve the preservation stability of the nanopore membrane. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a simple, convenient and highly accurate method for evaluating the pore size preservation effect of a nanoporous membrane and a method for preserving the pore size of a nanoporous membrane.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for evaluating the pore size preservation effect of a nanoporous membrane comprises the following steps:

[0008] (1) performing a current-voltage curve test on a nanoporous membrane without pore size preservation to obtain an initial current and an initial voltage of the nanoporous membrane;

[0009] (2) preserving the pore size of the nanoporous membrane, and then performing a current-voltage curve test on the nanoporous membrane after the pore size preservation to obtain the post-preservation current and post-preservation voltage of the nanoporous membrane;

[0010] (3) Calculate the preservation effect using an evaluation formula, which is:

[0011]

[0012] Wherein, ΔD is the absolute value of the dimensionless number describing the pore size preservation effect, I0 is the initial current of the nanopore membrane, V0 is the initial voltage of the nanopore membrane, I1 is the current of the nanopore membrane after preservation, V1 is the voltage of the nanopore membrane after preservation, t is the preservation time,

[0013] The smaller the ΔD is, the smaller the pore size change is, and the better the preservation effect is.

[0014] Preferably, the nanoporous membrane includes any one of a silicon nitride membrane, a silicon dioxide membrane, a silicon membrane, and a silicon carbide membrane, or a composite membrane of two or more thereof.

[0015] Preferably, the thickness of the nanoporous membrane is 5 to 20 nm, more preferably 5 to 15 nm.

[0016] Preferably, the pore size of the nanoporous membrane is 1 to 30 nm.

[0017] Preferably, the current-voltage curve test comprises immersing the nanoporous membrane in a salt solution and then applying a voltage of -200 to 200 mV to the nanoporous membrane to obtain a current-voltage curve. Applying a voltage of -200 to 200 mV will not affect the pore size of the nanoporous membrane.

[0018] Further preferably, the salt solution is a potassium chloride solution.

[0019] Preferably, the concentration of the salt solution is 0.1-2 mol / L.

[0020] Preferably, the evaluation method further comprises the steps of washing the nanoporous membrane with deionized water and then drying the nanoporous membrane after the current-voltage curve test is completed and / or after the pore size preservation is completed.

[0021] In some embodiments, the drying includes air-drying the nanoporous membrane.

[0022] Preferably, the pore size preservation comprises using a neutral liquid, an organic solvent or an inert gas to contact the inner surface of the nanoporous membrane to isolate the nanopores of the nanoporous membrane from the external environment.

[0023] In some embodiments, the neutral liquid includes a mixed solution of one or more of lithium chloride, potassium chloride, sodium chloride and water.

[0024] Preferably, the concentration of the neutral solution is 0.5 to 4.0 mol / L, more preferably 0.5 to 2.0 mol / L, and even more preferably 0.8 to 1.8 mol / L.

[0025] In some embodiments, the organic solvent includes one or more of dimethyl sulfoxide, N-methylpyrrolidone, and isopropanol.

[0026] In some embodiments, the inert gas includes one or more of helium, nitrogen, and argon.

[0027] Preferably, the contacting method includes one or more of immersion, spraying and shower coating.

[0028] The present invention also provides a method for preserving the pore size of a nanoporous membrane, the method comprising using a neutral liquid, an organic solvent or an inert gas to contact the inner surface of the nanoporous membrane to isolate the nanopores of the nanoporous membrane from the external environment, wherein the neutral liquid comprises a mixed solution of one or more of lithium chloride, potassium chloride, and sodium chloride and water, the organic solvent comprises one or more of dimethyl sulfoxide, N-methylpyrrolidone, and isopropanol, and the inert gas comprises one or more of helium, nitrogen, and argon.

[0029] Preferably, the concentration of the neutral solution is 0.5 to 4.0 mol / L, more preferably 0.5 to 2.0 mol / L, and even more preferably 0.8 to 1.8 mol / L.

[0030] Preferably, the contacting method includes one or more of immersion, spraying and shower coating.

[0031] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0032] The evaluation method of the invention is simple, convenient and highly accurate, and is suitable for verifying the preservation effect of nanoporous membranes.

[0033] The storage method of the invention can improve the storage stability of the nanoporous membrane, maintain the pore size of the nanoporous membrane, and has simple operation and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1is a graph showing the change in the current-voltage (IV) curve of the first membrane in Example 1;

[0035] Figure 2 is a graph showing the change in the current-voltage (IV) curve of the second membrane in Example 1;

[0036] Figure 3 This is a graph showing the change in the current-voltage (IV) curve of the third diaphragm in Example 1. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the examples. However, the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0038] Unless otherwise specified, the raw materials or instruments involved in the following can be commercially available products or can be prepared by referring to the preparation methods of the prior art. In order to test the pore size preservation effect of the nanoporous membrane, the inventor punched holes in the self-made membrane to obtain nanopores, and verified the accuracy of the evaluation method and the preservation effect by comparing the pore size before and after the nanopores were preserved. The punching process can refer to the existing process, such as the dielectric breakdown process.

[0039] The preparation method of the nanoporous membrane is as follows: using a silicon wafer as a substrate, using low-pressure chemical vapor deposition technology (the pressure of vapor deposition is 0.01 torr and the temperature is 500 to 1200°C) to deposit the required nanofilm on the silicon substrate; then, using photolithography and etching technology to pattern the film; finally, etching the silicon wafer from the back to produce a cavity under the membrane window, thereby forming an independent and unsupported nanofilm. The nanoporous membrane can also be directly purchased from the market with reference to the existing technology, and this application does not make specific restrictions.

[0040] If not otherwise specified, the current-voltage curve test in the present invention can refer to the prior art, including placing the diaphragm on a test device, connecting one end to the positive electrode and the other end to the negative electrode, and performing a voltage scan at -200 to 200 mV at room temperature (25±5°C) to obtain the current-voltage curve change of the diaphragm.

[0041] If not otherwise specified, the units of I0 and I1 in the formula for evaluating the pore size preservation effect of the present invention are nA, the units of V0 and V1 are V, and the unit of t is day.

[0042] Example 1

[0043] Three 12 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film, the second film and the third film were measured by TEM and were found to be 8.5 nm, 8.6 nm and 8.7 nm respectively.

[0044] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0045] Then, the first membrane and the second membrane were immersed in a 1 mol / L potassium chloride solution and dimethyl sulfoxide, respectively, and stored at room temperature (25±5°C) for 1 day. The third membrane was exposed to air as a control and stored at room temperature for 1 day. After storage, the membrane was cleaned with deionized water and dried for later use.

[0046] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0047] The pore size preservation effects ΔD of the first, second and third membranes were 0.20, 0.03 and 0.43 respectively, among which the pore size preservation effect ΔD of the second membrane was the smallest, followed by the first membrane. That is to say, for a silicon nitride membrane with a thickness of 12 nm and a pore size of about 8.5 nm, compared with not using any preservation means, using 1 mol / L potassium chloride solution or dimethyl sulfoxide has a certain pore size preservation effect, and using dimethyl sulfoxide has a better pore size preservation effect.

[0048] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM method to be 13 nm, 8 nm and 2 nm respectively, and the actual preservation effects were consistent with the evaluation results of the above-mentioned pore size preservation effect formula.

[0049] Example 2

[0050] Three 11.5 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film, the second film and the third film were measured by TEM and were found to be 3.3 nm, 3.2 nm and 3.4 nm respectively.

[0051] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0052] Then, the first membrane and the second membrane were immersed in a 1 mol / L potassium chloride solution and isopropanol respectively and stored at room temperature for 1 day. The third membrane was exposed to air as a control and stored at room temperature for 1 day. After storage, the membrane was cleaned with deionized water and dried for later use.

[0053] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0054] The pore preservation effects ΔD of the first, second and third membranes are 0.13, 0.20 and 0.75 respectively, among which the pore preservation effect ΔD of the first membrane is the smallest, followed by the second membrane. That is to say, for the silicon nitride membrane with a thickness of 11.5nm and a pore size of about 3.3nm, the potassium chloride solution has a better pore preservation effect.

[0055] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM method to be 4.2 nm, 4.7 nm and 10.5 nm respectively, and the actual preservation effects were consistent with the evaluation results of the above-mentioned pore size preservation effect formula.

[0056] Example 3

[0057] Three 11.5 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film, the second film and the third film were measured by TEM and were found to be 5 nm, 4.9 nm and 4.8 nm respectively.

[0058] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0059] Then, the first membrane and the second membrane were immersed in a 1.56 mol / L potassium chloride solution and N-methylpyrrolidone, respectively, and stored at room temperature for 2 days. The third membrane was exposed to air as a control and stored at room temperature for 2 days. After storage, the membrane was cleaned with deionized water and dried for later use.

[0060] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0061] The pore preservation effects ΔD of the first, second and third membranes are 0.09, 0.06 and 0.24 respectively, among which the pore preservation effect ΔD of the second membrane is the smallest. That is to say, for the silicon nitride membrane with a thickness of 11.5nm and a pore size of about 5nm, N-methylpyrrolidone has a better pore preservation effect.

[0062] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM method to be 6.1 nm, 5.6 nm and 7.8 nm respectively. The actual preservation effect was consistent with the evaluation result of the above-mentioned pore size preservation effect formula.

[0063] Example 4

[0064] Three 11.5 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film, the second film and the third film were measured by TEM and were found to be 2.8 nm, 2.7 nm and 2.9 nm respectively.

[0065] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0066] Then, the first membrane and the second membrane were immersed in a 1 mol / L lithium chloride solution and dimethyl sulfoxide solution, respectively, and stored at room temperature for 4 days. The third membrane was exposed to air as a control and stored at room temperature for 4 days. After storage, the membrane was cleaned with deionized water, dried and set aside.

[0067] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0068] The pore preservation effects ΔD of the first, second and third membranes are 0.04, 0.03 and 0.86 respectively, among which the pore preservation effect ΔD of the second membrane is the smallest. That is to say, for the silicon nitride membrane with a thickness of 11.5nm and a pore size of about 2.8nm, dimethyl sulfoxide has a better pore preservation effect.

[0069] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM method to be 3 nm, 2.6 nm and 13.3 nm respectively. The actual preservation effect was consistent with the evaluation result of the above-mentioned pore size preservation effect formula.

[0070] Example 5

[0071] Three 7.5 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film and the second film were measured by TEM measurement method, and the initial pore size of the third film was 3 nm.

[0072] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0073] Then, the first membrane and the second membrane were immersed in a 1 mol / L lithium chloride solution and dimethyl sulfoxide solution, respectively, and stored at room temperature for 5 days. The third membrane was exposed to air as a control and stored at room temperature for 5 days. After storage, the membrane was cleaned with deionized water, dried and set aside.

[0074] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0075] The pore preservation effects ΔD of the first, second and third membranes are 0.06, 0.03 and 0.60 respectively, among which the pore preservation effect ΔD of the second membrane is the smallest. That is to say, for the silicon nitride membrane with a thickness of 7.5nm and a pore size of about 3nm, dimethyl sulfoxide has a better pore preservation effect.

[0076] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM method to be 3.5 nm, 3.2 nm and 10.1 nm respectively, and the actual preservation effect was consistent with the evaluation result of the above-mentioned pore size preservation effect formula.

[0077] Example 6

[0078] Three 11.5 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film and the second film were measured by TEM measurement method to be 3.6 nm, and the initial pore size of the third film was 3.5 nm.

[0079] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0080] Then, the first membrane and the second membrane were immersed in a 1wt% sodium hypochlorite solution and dimethyl sulfoxide solution respectively and stored at room temperature for 3 days, and the third membrane was exposed to air as a control and stored at room temperature for 3 days. After storage, the membrane was cleaned with deionized water and dried for later use.

[0081] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0082] The pore preservation effects ΔD of the first, second and third membranes are 2.33, 0.03 and 0.33 respectively, among which the pore preservation effect ΔD of the second membrane is the smallest. That is to say, for the silicon nitride membrane with a thickness of 11.5nm and a pore size of about 3.6nm, dimethyl sulfoxide has a better pore preservation effect.

[0083] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM measurement method to be 43.8nm, 3.4nm and 1.8nm respectively, and the actual preservation effect was consistent with the evaluation result of the pore size preservation effect formula mentioned above. Sodium hypochlorite will cause the pore size to increase sharply and is not suitable for the pore size preservation of nanoporous membranes.

[0084] Example 7

[0085] Three 11.5 nm thick silicon nitride films were taken and named as the first film, the second film and the third film. The initial pore sizes of the first film and the second film were measured by TEM and were found to be 5.8 nm, and the initial pore size of the third film was 5.9 nm.

[0086] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the three membranes. After the test, the three membranes were cleaned with deionized water, dried and set aside.

[0087] Then, the first membrane and the second membrane were immersed in deionized water and dimethyl sulfoxide respectively and stored at room temperature for 10 days, and the third membrane was exposed to air as a control and stored at room temperature for 10 days. After the storage, the first membrane was dried and used for later use, and the membrane was cleaned with deionized water and dried for later use.

[0088] Finally, the first membrane, the second membrane and the third membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the nanopores of the three membranes. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0089] The pore preservation effects ΔD of the first, second and third membranes are 1.01, 0 and 0.68 respectively, among which the pore preservation effect ΔD of the second membrane is the smallest. That is to say, for the silicon nitride membrane with a thickness of 11.5nm and a pore size of about 5.8nm, dimethyl sulfoxide has a better pore preservation effect.

[0090] The actual pore sizes of the first, second and third membranes after preservation were measured by TEM method to be 33.3 nm, 5.8 nm and 22.1 nm respectively. The actual preservation effect was consistent with the evaluation result of the above-mentioned pore size preservation effect formula. Deionized water will cause the pore size to increase sharply and is not suitable for pore size preservation of nanoporous membranes.

[0091] Example 8

[0092] Two 11.5 nm thick silicon nitride films were taken and named as the first film and the second film. The initial pore sizes of the first film and the second film were measured by TEM and were found to be 5.7 nm and 5.8 nm respectively.

[0093] The first membrane, the second membrane and the third membrane were immersed in 1 mol / L potassium chloride solution respectively, and the current-voltage (IV) curve test was carried out to obtain the initial current I0 and initial voltage V0 of the nanopores of the two membranes. After the test, the two membranes were cleaned with deionized water and dried for use.

[0094] Then, the first membrane was exposed to air and stored at room temperature for 2 days, and the second membrane was immersed in dimethyl sulfoxide and stored at room temperature for 2 days. After the storage, the stored membrane was cleaned with deionized water and dried for later use.

[0095] Finally, the first membrane and the second membrane are tested for current-voltage (IV) curves to obtain the final current I1 and final voltage V1 of the membrane nanopore. Substitute all parameters into the formula for evaluating the pore size preservation effect:

[0096] The pore preservation effects ΔD of the first, second and third membranes are 0.50 and 0.01 respectively, among which the pore preservation effect ΔD of the second membrane is the smallest. That is to say, for the silicon nitride membrane with a thickness of 11.5nm and a pore size of about 5.8nm, dimethyl sulfoxide has a better pore preservation effect.

[0097] The actual pore sizes of the first and second membranes after preservation were measured by TEM method to be 1.6 nm and 5.7 nm respectively. The actual preservation effect was consistent with the evaluation result of the above-mentioned pore size preservation effect formula.

[0098] The above detailed description of the present invention is intended to enable persons familiar with the art to understand the contents of the present invention and implement them. It does not limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for evaluating the pore size preservation effect of a nanoporous membrane, characterized in that: The evaluation method comprises the following steps: (1) performing a current-voltage curve test on a nanoporous membrane without pore size preservation to obtain an initial current and an initial voltage of the nanoporous membrane; (2) preserving the pore size of the nanoporous membrane, and then performing a current-voltage curve test on the nanoporous membrane after the pore size preservation to obtain the post-preservation current and post-preservation voltage of the nanoporous membrane; (3) Calculate the preservation effect using an evaluation formula, which is: Wherein, ΔD is the absolute value of the dimensionless number describing the pore size preservation effect, I0 is the initial current of the nanopore membrane, V0 is the initial voltage of the nanopore membrane, I1 is the current of the nanopore membrane after preservation, V1 is the voltage of the nanopore membrane after preservation, t is the preservation time, The smaller the ΔD is, the smaller the pore size change is, and the better the preservation effect is.

2. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 1, characterized in that: The nanoporous membrane includes any one of a silicon nitride membrane, a silicon dioxide membrane, a silicon membrane, and a silicon carbide membrane, or a composite membrane of two or more thereof.

3. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 1, characterized in that: The thickness of the nanoporous membrane is 5 to 20 nm; and / or, The pore size of the nanoporous membrane is 1 to 30 nm.

4. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 1, characterized in that: The current-voltage curve test includes immersing the nanoporous membrane in a salt solution, and then applying a voltage of -200 to 200 mV to the nanoporous membrane to obtain a current-voltage curve.

5. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 4, characterized in that: The salt solution is a potassium chloride solution; and / or, The concentration of the salt solution is 0.1-2 mol / L.

6. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 1, characterized in that: The evaluation method further comprises the steps of washing the nanoporous membrane with deionized water and then drying the nanoporous membrane after the current-voltage curve test is completed and / or after the pore size preservation is completed.

7. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 1, characterized in that: The pore size preservation includes using a neutral liquid, an organic solvent or an inert gas to contact the inner surface of the nanoporous membrane to isolate the nanopores of the nanoporous membrane from the external environment.

8. The method for evaluating the pore size preservation effect of a nanoporous membrane according to claim 7, characterized in that: The neutral liquid includes a mixed solution of one or more of lithium chloride, potassium chloride, sodium chloride and water; and / or, The organic solvent includes one or more of dimethyl sulfoxide, N-methylpyrrolidone, and isopropanol; and / or, The inert gas includes one or more of helium, nitrogen and argon; and / or, The contacting method includes one or more of immersion, spraying, and shower coating.

9. A method for preserving the pore size of a nanoporous membrane, characterized in that: The pore size preservation method includes using a neutral liquid, an organic solvent or an inert gas to contact the inner surface of the nanoporous membrane to isolate the nanopores of the nanoporous membrane from the external environment, wherein the neutral liquid includes a mixed solution of one or more of lithium chloride, potassium chloride, sodium chloride and water, The organic solvent includes one or more of dimethyl sulfoxide, N-methylpyrrolidone, and isopropanol. The inert gas includes one or more of helium, nitrogen and argon.

10. The method for preserving the pore size of a nanoporous membrane according to claim 9, characterized in that: The contacting method includes one or more of immersion, spraying, and shower coating.

Citation Information

Patent Citations

  • Method for precisely preparing nanopores in silicon nitride thin film on basis of electric breakdown

    CN105368938A

  • Method for expanding pore diameter of nano-pore membrane

    CN118594272A

  • Package, method for storing or transporting sub-nano membrane structure, and sub-nano membrane structure

    US20170203254A1

  • Nanopore-forming method, nanopore-forming device and biomolecule measurement device

    US20190369080A1