Optical fiber for high-temperature non-fading and non-migration optical cable and preparation method of optical fiber
A melt-drawn optical fiber with a modified acrylic inner and self-repairing polyimide outer coating addresses high-temperature degradation issues by enhancing adhesion and self-repair, ensuring stability and reliability in high-temperature environments.
Patent Information
- Application Number
- CN202411242191.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Conventional optical fibers fail to maintain optical performance, mechanical strength, and reliability at high temperatures, experiencing aging, delamination, and failure due to coating degradation in high-temperature environments.
A melt-drawn optical fiber with a modified acrylic inner coating layer and a self-repairing polyimide outer coating layer, utilizing a diamine monomer with a maleimide group and a bisimide unit, is prepared through specific coating processes to enhance temperature resistance and self-repair capabilities.
The solution provides high-temperature stability by preventing migration and delamination, maintaining optical performance and mechanical integrity, with improved adhesion and self-repair mechanisms for long-term use.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical fibers, in particular to an optical fiber for a high-temperature non-fading and non-migrating optical cable and a preparation method thereof. Background Art
[0002] With the rapid development of optical communication, optical fiber has been widely used in many fields as a basic material. Different application scenarios have different requirements for the performance of optical fiber. For example, high-temperature sensing, oil and gas fields and other high-temperature fields have special requirements for the temperature resistance of optical fiber. At present, conventional optical fiber cannot meet the reliability of use at higher temperatures. In order to meet the needs of use in high-temperature environments, optical fiber must maintain the same or similar optical performance, mechanical strength and reliability as that at room temperature and normal use environment.
[0003] Conventional UV-curable polyacrylate coated optical fibers will experience severe aging and failure when the temperature exceeds 85°C. Specifically, the coating will turn yellow and black, the mechanical properties will weaken, and the protective effect on the optical fiber will be lost, resulting in natural breakage of the optical fiber, which cannot meet the reliability of optical fiber transmission. After long-term use, high-temperature resistant optical fibers will have a large area of delamination between the inner coating and the outer coating. In view of the above problems, the present invention provides an optical fiber for high-temperature non-fading and non-migrating optical cables and a preparation method thereof to solve the problems existing in the prior art. Summary of the invention
[0004] The object of the present invention is to provide an optical fiber for a high temperature non-fading and non-migrating optical cable and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: an optical fiber for high temperature non-fading and non-migrating optical cable, wherein the optical fiber for the optical cable is made of a melt-drawn optical fiber with a modified acrylic inner coating layer and a self-repairing polyimide outer coating layer.
[0006] Furthermore, the self-healing polyimide is prepared using a diamine monomer containing a bisimide unit and having a maleimide group as a raw material.
[0007] A method for preparing an optical fiber for a high-temperature non-fading and non-migrating optical cable comprises the following preparation steps:
[0008] (1) The optical fiber preform is fed into a furnace at a temperature of 2000-2200℃ by a feeding system and heated. After the preform is softened, it is pulled out from the lower outlet of the furnace at a speed of more than 800-1600m / min in the form of a filament. A certain error in the diameter of the optical fiber preform is allowed.
[0009] (2) After melt drawing, the optical fiber is directly put into the inner coating mold after annealing and cooling at room temperature. The maximum outer diameter of the cladding of the inner coating optical fiber is 125 μm, the maximum outer diameter of the inner coating layer of the single coating optical fiber is 230 μm, and the coating pressure of the inner coating is 2.5 bar;
[0010] (3) After the inner layer is coated, the optical fiber quickly enters the outer layer coating mold. The maximum outer diameter of the cladding of the inner coating optical fiber is 125 μm, the maximum outer diameter of the inner coating of the single coating optical fiber is 230 μm, and the coating pressure of the outer coating is 5 bar;
[0011] (4) The optical fiber after double-layer coating is cured under 6 high-power UV lamps; after the curing is completed, it is taken up by an automatic take-up device to prepare an optical fiber for high-temperature non-fading and non-migration optical cable.
[0012] Furthermore, in the steps (2) and (3), the coating temperature is maintained at 40°C.
[0013] Furthermore, the inner coating layer material in step (2) is a homemade modified acrylic resin.
[0014] Furthermore, the preparation process of the homemade modified acrylic resin is as follows: according to weight parts, 1-3 parts of 2-hydroxy-4-(3-methacrylate-2-hydroxypropoxy)benzophenone, 15-25 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, 20 parts of butanone, and 0.15-0.55 parts of 3-aminopropylmethyldimethoxysilane are weighed, and the mixture is stirred at 150 rpm for 20 minutes to mix evenly, and then added into a light-shielded reactor, and stirred and reacted at 150 rpm in a water bath at 80°C for 60 minutes to obtain a modified acrylic resin.
[0015] Furthermore, in step (3), the outer coating layer material is self-healing polyimide.
[0016] Furthermore, the preparation process of the self-healing polyimide is as follows: first weigh a certain amount of diamine monomer containing a diimide unit into a three-day bottle, then add p-phenylenediamine and stir at high speed to completely dissolve it, the mass ratio of the diamine monomer containing a diimide unit to p-phenylenediamine is 1:0.5-2; then add 0.9 times of pyromellitic anhydride when the molar amount of the diamine monomer containing a diimide unit is equal in 4 times, the addition method of pyromellitic anhydride is dichotomy, and it is added in 4 times, and the time interval between each addition of pyromellitic anhydride is 20 minutes; after the reaction is complete, a self-healing polyimide liquid is obtained.
[0017] Furthermore, the preparation process of the diamine monomer containing the bisimide unit is as follows: in a dry three-necked flask equipped with an electromagnetic stirrer, under nitrogen protection, 0.01 mmol of 4,4'-diaminodiphenyl ether and 20 mL of acetone are added; 20 mL of acetone dissolved with 0.01 mmol of maleic anhydride is slowly dripped in, and the maleic anhydride is dripped in 30 minutes, and stirring is continued at 150 rpm for 2 hours to complete the reaction; after the reaction is completed, filtering, washing with acetone, and recrystallizing with ethanol to obtain the diamine monomer containing the bisimide unit.
[0018] Furthermore, it is characterized in that the UV lamp in step (4) is a 3W high-power lamp.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The present invention uses a melt-drawn optical fiber to modify an acrylic inner coating layer and a self-repairing polyimide outer coating layer to achieve a high-temperature stable effect.
[0021] First, curing monomers and 3-aminopropylmethyldimethoxysilane are added to the acrylic resin of the inner coating layer. The additives do not contain small molecular active substances, thereby avoiding the migration of small molecular active substances during storage. Applying them to the acrylic resin can make the acrylic resin have excellent high temperature resistance. Aminosiloxane can enhance the adhesion between the high temperature resistant acrylate layer and the polyimide layer, and at the same time improve the viscosity of the acrylic film after the curing monomer is added, so that the inner coating layer does not migrate, fall off or fade under high temperature conditions.
[0022] Secondly, a diamine monomer containing a maleimide group and a bisimide unit was synthesized using maleic anhydride and 4,4'-diaminodiphenyl ether as diamine monomers as reaction raw materials. The diamine monomer was reacted with p-phenylenediamine and pyromellitic dianhydride to prepare a thermosetting polyimide film with a dynamic imide bond in the molecular main chain. This film was used as an outer coating and cured quickly. This film not only has excellent heat resistance, but also utilizes the primary amine group in the aminosilane coupling agent added to the inner coating layer to promote the reversible imide bond exchange reaction, thereby achieving self-repair of the thermosetting polyimide film under mild conditions. After long-term use, a large area of delamination between the modified acrylic layer and the polyimide layer of the optical fiber can be repaired, thereby improving the high temperature resistance of the optical fiber. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of an optical fiber for a high temperature non-fading and non-migrating optical cable prepared in the following examples are as follows:
[0025] High temperature stability: The delamination ratio between the inner and outer coating layers of the double-coated optical fiber is tested at 250°C for 30 days. The typical value of additional attenuation at 150°C is tested based on part 40 of GB-T15972.40-2008 for long-term operation.
[0026] Example 1
[0027] (1) The optical fiber preform is fed into a 2000℃ high temperature furnace by a feeding system for heating. After the preform softens, it is pulled out from the lower outlet of the furnace at a speed of more than 800m / min in a filamentary form. A certain error in the diameter of the optical fiber preform is allowed.
[0028] (2) According to the weight ratio, 1 part of 2-hydroxy-4-(3-methacrylate-2-hydroxypropoxy)benzophenone, 15 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, 20 parts of butanone, and 0.15 parts of 3-aminopropylmethyldimethoxysilane were weighed, stirred at 150 rpm for 20 minutes, and then added to a light-shielded reactor. The mixture was stirred at 150 rpm in a water bath at 80° C. for 60 minutes to obtain a modified acrylic resin; the optical fiber after melt drawing was directly put into the mold for inner coating after annealing and cooling at room temperature, and the coating temperature was maintained at 40° C. The inner coating material was a homemade modified acrylic resin, the maximum outer diameter of the cladding of the inner coating optical fiber was 10 μm, the maximum outer diameter of the inner coating of the double-coated optical fiber was 200 μm, and the coating pressure of the inner coating was 2.5 bar;
[0029] (3) In a dry three-necked flask equipped with an electromagnetic stirrer, under nitrogen protection, add 0.01 mmol of 4,4'-diaminodiphenyl ether and 20 mL of acetone; slowly drop 20 mL of acetone dissolved with 0.01 mmol of maleic anhydride, and complete the dropwise addition of maleic anhydride within 30 min, and continue stirring at 150 rpm for 2 h to allow the reaction to proceed completely; after the reaction is completed, filter, rinse with acetone, and recrystallize with ethanol to obtain a diamine monomer containing a diimide unit; first weigh a certain amount of the diamine monomer containing a diimide unit into a three-necked flask, then add p-phenylenediamine and stir at high speed to completely dissolve it, and the diamine monomer containing a diimide unit and p-phenylenediamine are mixed and stirred at high speed to obtain a diamine monomer containing a diimide unit. The mass ratio of dimethylamine is 1:0.5; then, 0.9 times of the molar amount of diamine monomer containing diimide unit is added in 4 times, and the addition method of pyromellitic anhydride is dichotomy, and it is added in 4 times, and the time interval between each addition of pyromellitic anhydride is 20 minutes; after the reaction is complete, a self-repairing polyimide liquid is obtained; after the inner layer is coated, the optical fiber quickly enters the outer layer coating mold, and the coating temperature is maintained at 40°C. The outer coating material is a self-repairing polyimide liquid, the maximum outer diameter of the cladding of the outer coating optical fiber is 150μm, the maximum outer diameter of the outer coating of the double-coated optical fiber is 250μm, and the coating pressure of the outer coating is 5bar;
[0030] (4) The optical fiber after double-layer coating is cured under high power of 6 3W high-power UV lamps; after the curing is completed, it is taken up by an automatic take-up device to prepare an optical fiber for high-temperature non-fading and non-migration optical cable.
[0031] Example 2
[0032] (1) The optical fiber preform is fed into a 2100℃ high temperature furnace by a feeding system for heating. After the preform softens, it is pulled out from the lower outlet of the furnace at a speed of more than 1200m / min. A certain error in the diameter of the optical fiber preform is allowed.
[0033] (2) According to the weight ratio, 2 parts of 2-hydroxy-4-(3-methacrylate-2-hydroxypropoxy)benzophenone, 20 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, 20 parts of butanone, and 0.30 parts of 3-aminopropylmethyldimethoxysilane were weighed, stirred at 150 rpm for 20 minutes, and then added to a light-shielded reactor, and stirred at 150 rpm in an 80°C water bath for 60 minutes to prepare a modified acrylic resin; the optical fiber after melt drawing was directly put into the inner coating mold after annealing and cooling at room temperature, and the coating temperature was maintained at 40°C. The inner coating material was a homemade modified acrylic resin, the maximum outer diameter of the cladding of the inner coating optical fiber was 10 μm, the maximum outer diameter of the inner coating of the double-coated optical fiber was 200 μm, and the coating pressure of the inner coating was 2.5 bar;
[0034] (3) In a dry three-necked flask equipped with an electromagnetic stirrer, under nitrogen protection, add 0.01 mmol of 4,4'-diaminodiphenyl ether and 20 mL of acetone; slowly drop 20 mL of acetone dissolved with 0.01 mmol of maleic anhydride, and complete the dropwise addition of maleic anhydride within 30 min, and continue stirring at 150 rpm for 2 h to allow the reaction to proceed completely; after the reaction is completed, filter, rinse with acetone, and recrystallize with ethanol to obtain a diamine monomer containing a diimide unit; first weigh a certain amount of the diamine monomer containing a diimide unit into a three-necked flask, then add p-phenylenediamine and stir at high speed to completely dissolve it, and the diamine monomer containing a diimide unit and p-phenylenediamine are mixed and stirred at high speed to obtain a diamine monomer containing a diimide unit. The mass ratio of dimethylamine is 1:1.5; then, 0.9 times of the molar amount of diamine monomer containing diimide unit is added in 4 times, and the addition method of pyromellitic anhydride is dichotomy, and it is added in 4 times, and the time interval between each addition of pyromellitic anhydride is 20 minutes; after the reaction is complete, a self-repairing polyimide liquid is obtained; after the inner layer is coated, the optical fiber quickly enters the outer layer coating mold, and the coating temperature is maintained at 40°C. The outer coating material is a self-repairing polyimide liquid, the maximum outer diameter of the cladding of the outer coating optical fiber is 150μm, the maximum outer diameter of the outer coating of the double-coated optical fiber is 250μm, and the coating pressure of the outer coating is 5bar;
[0035] (4) The optical fiber after double-layer coating is cured under high power of 6 3W high-power UV lamps; after the curing is completed, it is taken up by an automatic take-up device to prepare an optical fiber for high-temperature non-fading and non-migration optical cable.
[0036] Example 3
[0037] (1) The optical fiber preform is fed into a 2200℃ high temperature furnace by a feeding system for heating. After the preform softens, it is pulled out from the lower outlet of the furnace at a speed of more than 1600m / min. A certain error in the diameter of the optical fiber preform is allowed.
[0038] (2) According to the weight ratio, 3 parts of 2-hydroxy-4-(3-methacrylate-2-hydroxypropoxy)benzophenone, 25 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, 20 parts of butanone, and 0.55 parts of 3-aminopropylmethyldimethoxysilane were weighed, stirred at 150 rpm for 20 minutes to mix evenly, and then added to a light-shielded reactor, stirred at 150 rpm in an 80°C water bath for 60 minutes to prepare a modified acrylic resin; the optical fiber after melt drawing was directly put into the inner coating mold after annealing and cooling at room temperature, and the coating temperature was maintained at 40°C. The inner coating material was a homemade modified acrylic resin, the maximum outer diameter of the cladding of the inner coating optical fiber was 10 μm, the maximum outer diameter of the inner coating of the double-coated optical fiber was 200 μm, and the coating pressure of the inner coating was 2.5 bar;
[0039] (3) In a dry three-necked flask equipped with an electromagnetic stirrer, under nitrogen protection, add 0.01 mmol of 4,4'-diaminodiphenyl ether and 20 mL of acetone; slowly drop 20 mL of acetone dissolved with 0.01 mmol of maleic anhydride, and complete the dropwise addition of maleic anhydride within 30 min, and continue stirring at 150 rpm for 2 h to allow the reaction to proceed completely; after the reaction is completed, filter, rinse with acetone, and recrystallize with ethanol to obtain a diamine monomer containing a diimide unit; first weigh a certain amount of diamine monomer containing a diimide unit into a three-necked flask, then add p-phenylenediamine and stir at high speed to completely dissolve it, and the diamine monomer containing a diimide unit and p-phenylenediamine are mixed. The mass ratio of benzyl diamine is 1:2; then, 0.9 times of the molar amount of diamine monomer containing diimide unit is added in 4 times, and the addition method of benzyl dicarboxylic anhydride is dichotomy, and it is added in 4 times, and the time interval of each addition of benzyl dicarboxylic anhydride is 20 minutes; after the reaction is complete, a self-repairing polyimide liquid is obtained; after the inner layer is coated, the optical fiber quickly enters the outer layer coating mold, and the coating temperature is maintained at 40°C. The outer coating material is a self-repairing polyimide liquid, the maximum outer diameter of the cladding of the outer coating optical fiber is 150μm, the maximum outer diameter of the outer coating of the double-coated optical fiber is 250μm, and the coating pressure of the outer coating is 5bar;
[0040] (4) The optical fiber after double-layer coating is cured under high power of 6 3W high-power UV lamps; after the curing is completed, it is taken up by an automatic take-up device to prepare an optical fiber for high-temperature non-fading and non-migration optical cable.
[0041] Comparative Example 1
[0042] The difference between Comparative Example 1 and Example 2 lies in step (3). Step (3) is changed as follows: after the inner layer is coated, the optical fiber quickly enters the outer layer coating mold, the coating temperature is maintained at 40°C, the outer coating material is isophthalic polyimide, the maximum outer diameter of the cladding of the outer coating optical fiber is 150 μm, the maximum outer diameter of the outer coating of the double-coated optical fiber is 250 μm, and the coating pressure of the outer coating is 5 bar; the remaining steps are the same as Example 2.
[0043] Comparative Example 2
[0044] The difference between Comparative Example 2 and Example 2 is that step (2) is different, and step (2) is changed to: according to weight parts, weigh 2 parts of 2-hydroxy-4-(3-methacrylate-2-hydroxypropoxy) benzophenone, 20 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, and 20 parts of butanone, stir at 150 rpm for 20 min to mix evenly, then add to a light-shielded reactor, stir and react at 150 rpm in an 80° C. water bath for 60 min to obtain a modified acrylic resin; the optical fiber after melt drawing is directly annealed and cooled at room temperature and then enters the inner coating mold, the coating temperature is maintained at 40° C., the inner coating material is a homemade modified acrylic resin, the maximum outer diameter of the cladding of the inner coating optical fiber is 10 μm, the maximum outer diameter of the inner coating of the double-coated optical fiber is 200 μm, and the coating pressure of the inner coating is 2.5 bar; the remaining steps are the same as in Example 2.
[0045] Comparative Example 3
[0046] The difference between Comparative Example 3 and Example 2 is that step (2) is different. Step (2) is changed to: according to weight parts, 20 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, 20 parts of butanone, and 0.30 parts of 3-aminopropylmethyldimethoxysilane are weighed, stirred at 150 rpm for 20 min to mix evenly, and then added to a light-shielded reactor, stirred at 150 rpm in an 80°C water bath for 60 min to obtain a modified acrylic resin; the optical fiber after melt drawing is directly put into the inner coating mold after annealing and cooling at room temperature, the coating temperature is maintained at 40°C, the inner coating material is a homemade modified acrylic resin, the maximum outer diameter of the cladding of the inner coating optical fiber is 10 μm, the maximum outer diameter of the inner coating of the double-coated optical fiber is 200 μm, and the coating pressure of the inner coating is 2.5 bar; the remaining steps are the same as those in Example 2.
[0047] Effect example
[0048] Table 1 below shows the performance analysis results of an optical fiber for a high temperature non-fading and non-migrating optical cable using Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0049] Table 1
[0050] Percentage of divested parts (%) Attenuation value (dB / km) Example 1 8.9 0.03 Example 2 8.6 0.01 Example 3 9.0 0.02 Comparative Example 1 16.7 0.28 Comparative Example 2 11.2 0.24 Comparative Example 3 14.3 0.11
[0051] From the comparison of the experimental data of high temperature resistance of the embodiment and the comparative example, it can be found that the present invention adds a curing monomer and 3-aminopropylmethyldimethoxysilane to the acrylic resin of the inner coating layer, and the additive does not contain small molecule active substances, thereby avoiding the migration phenomenon of small molecule active substances during storage. Applying it to the acrylic resin can make the acrylic resin have excellent high temperature resistance; aminosilicone can enhance the adhesion between the high temperature resistant acrylate layer and the polyimide layer, and at the same time can improve the viscosity of the acrylic film after the curing monomer is added, so that the inner coating layer still does not migrate, fall off or fade under high temperature conditions. The invention uses maleic anhydride and 4,4'-diaminodiphenyl ether as diamine monomers as reaction raw materials, synthesizes a diamine monomer containing a maleimide group in the molecular structure, and prepares a thermosetting polyimide film with a dynamic imide bond in the molecular main chain through an amine-aldehyde condensation reaction with p-phenylenediamine and pyromellitic dianhydride. The film is used as an outer coating layer, which not only has excellent heat resistance, but also promotes the reversible imide bond exchange reaction by utilizing the primary amine group in the aminosilane coupling agent added to the inner coating layer, thereby realizing the self-repair of the thermosetting polyimide film under mild conditions, and repairs the delamination and peeling of a large area between the modified acrylic layer and the polyimide layer of the optical fiber after long-term use, thereby improving the high temperature resistance of the optical fiber.
[0052] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. An optical fiber for a high temperature non-fading and non-migration optical cable, characterized in that: The optical fiber for the optical cable is prepared by subjecting the melt-drawn optical fiber to a modified acrylic inner coating layer and a self-repairing polyimide outer coating layer.
2. The optical fiber for high temperature non-fading and non-migration optical cable according to claim 1, characterized in that: The self-repairing polyimide is prepared using a diamine monomer containing a maleimide group and a bisimide unit as a raw material.
3. A method for preparing an optical fiber for a high temperature non-fading and non-migration optical cable, characterized in that: The method comprises the following preparation steps: (1) The optical fiber preform is fed into a furnace at a temperature of 2000-2200℃ by a feeding system and heated. After the preform is softened, it is pulled out from the lower outlet of the furnace at a speed of more than 800-1600m / min in the form of a filament. A certain error in the diameter of the optical fiber preform is allowed. (2) After melt drawing, the optical fiber is directly put into the inner coating mold after annealing and cooling at room temperature. The maximum outer diameter of the cladding of the inner coating optical fiber is 125 μm, the maximum outer diameter of the inner coating layer of the single coating optical fiber is 230 μm, and the coating pressure of the inner coating is 2.5 bar; (3) After the inner layer is coated, the optical fiber quickly enters the outer layer coating mold. The maximum outer diameter of the cladding of the inner coating optical fiber is 125 μm, the maximum outer diameter of the inner coating of the single coating optical fiber is 230 μm, and the coating pressure of the outer coating is 5 bar; (4) The optical fiber after double-layer coating is cured under 6 high-power UV lamps; after the curing is completed, it is taken up by an automatic take-up device to prepare an optical fiber for high-temperature non-fading and non-migration optical cable.
4. The method for preparing a high-temperature non-fading and non-migrating optical fiber for optical cable according to claim 3, characterized in that: In the steps (2) and (3), the coating temperature is maintained at 40°C.
5. The method for preparing an optical fiber for a high temperature non-fading and non-migrating optical cable according to claim 3, characterized in that: The inner coating layer material in step (2) is a homemade modified acrylic resin.
6. The method for preparing an optical fiber for a high temperature non-fading and non-migrating optical cable according to claim 5, characterized in that: The preparation process of the homemade modified acrylic resin is as follows: according to weight parts, 1-3 parts of 2-hydroxy-4-(3-methacrylate-2-hydroxypropoxy)benzophenone, 15-25 parts of butyl acrylate, 2 parts of methyl methacrylate, 0.5 parts of methacrylic acid, 0.03 parts of benzoyl peroxide, 20 parts of butanone, and 0.15-0.55 parts of 3-aminopropylmethyldimethoxysilane are weighed, and the mixture is stirred at a speed of 150 rpm for 20 minutes to be evenly mixed, and then added into a light-shielded reaction kettle, and stirred and reacted for 60 minutes in a water bath at 80°C and 150 rpm to obtain the modified acrylic resin.
7. The method for preparing an optical fiber for a high temperature non-fading and non-migrating optical cable according to claim 3, characterized in that: In the step (3), the outer coating layer material is self-healing polyimide.
8. The method for preparing an optical fiber for a high temperature non-fading and non-migrating optical cable according to claim 7, characterized in that: The preparation process of the self-healing polyimide is as follows: first weigh a certain amount of diamine monomer containing a diimide moiety into a three-day bottle, then add p-phenylenediamine and stir at high speed to completely dissolve it, the mass ratio of the diamine monomer containing a diimide moiety to p-phenylenediamine is 1:0.5-2; then add 0.9 times of pyromellitic anhydride when the molar amount of the diamine monomer containing a diimide moiety is equal in four times, the addition method of pyromellitic anhydride is a dichotomy method, and it is added in four times, and the time interval between each addition of pyromellitic anhydride is 20 minutes; after the reaction is complete, a self-healing polyimide liquid is obtained.
9. The method for preparing an optical fiber for a high temperature non-fading and non-migrating optical cable according to claim 8, characterized in that: The preparation process of the diamine monomer containing the bisimide moiety is as follows: in a dry three-necked flask equipped with an electromagnetic stirrer, under nitrogen protection, 0.01 mmol of 4,4'-diaminodiphenyl ether and 20 mL of acetone are added; 20 mL of acetone dissolved with 0.01 mmol of maleic anhydride is slowly dripped in, the maleic anhydride is dripped in 30 minutes, and stirring is continued at a speed of 150 rpm for 2 hours to complete the reaction; after the reaction is completed, filtering is performed, washing with acetone, and recrystallization is performed with ethanol to obtain the diamine monomer containing the bisimide moiety.
10. The method for preparing an optical fiber for a high temperature non-fading and non-migrating optical cable according to claim 3, characterized in that: The UV lamp in step (4) is a 3W high power lamp.
Citation Information
Patent Citations
Optical fiber comprising polyimide-silicone block copolymer coating, and method and apparatus therefor
CN1040187A
High temperature resistant optical fiber and preparation method thereof
CN109180023A
Low-temperature preparation method of polyimide coated optical fiber
CN110007391A
High-temperature-resistant optical fiber and preparation method thereof
CN113655578A
Strength-adjustable high-temperature-resistant optical fiber and preparation method thereof